High-temperature-resistant low-heat-conductivity aerogel composite material as well as preparation method and application thereof
By mixing mullite aerogel powder with surfactant and potassium hexattitanate whiskers and combining with high-temperature annealing treatment, a high-temperature resistant and low-thermal conductivity aerogel composite material was prepared, which solved the problem of mullite gas in the prior art. The problem of gel performance degradation at high temperatures achieves low thermal conductivity and stability above 1600°C, simplifying the process and improving production efficiency.
Patent Information
- Application Number
- CN202411067146.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing mullite aerogels are sintered at high temperatures, resulting in collapse of nanopore structures and degradation of performance, making them difficult to apply to high-temperature fields above 1600°C, and the preparation process is complex and the production efficiency is low.
Mullite aerogel powder is mixed with surfactant and water, potassium hexattitanate whiskers and mullite synthetic raw materials are added, and high-temperature and low-thermal conductivity aerogel is prepared after dehydration, molding and high-temperature annealing. Composite material.
By regulating the pore structure and inserting fill raw materials, the stability and thermal insulation and temperature resistance of the aerogel composite material are improved, so that it maintains low thermal conductivity and nanopore structure at 1600°C, and has excellent thermal insulation and temperature resistance.
Smart Images

Figure CN118955086A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of mullite aerogel, and in particular to a high temperature resistant and low thermal conductivity aerogel composite material and a preparation method and application thereof. Background Art
[0002] Aerogel is a new material with a three-dimensional nanoporous structure and low density (0.003-0.8 g·cm -3 ), high porosity (80-99.8%), high specific surface area (200-1000m 2 ·g -1 ), low thermal conductivity (~0.02W·m -1 K -1 ) and other properties, and has a very broad prospect in the fields of aerospace, chemical industry, energy-saving construction, military, communication, electronics, metallurgy, etc. However, traditional silica aerogels sinter at high temperatures exceeding 650°C, resulting in the collapse of the nanopore structure and the decline of performance, making it difficult to be used in high-temperature fields.
[0003] Patent CN110078425B discloses a method for preparing a lightweight and heat-insulating mullite nanofiber aerogel with ultra-low solid content. The method directly uses nano-mullite fiber membrane as raw material, disperses it to obtain single mullite fibers; mixes silica sol and acrylamide system gel injection molding premix with the dispersed single mullite fibers to form a gel; freeze-dries the gel to obtain an aerogel blank, and finally calcines it at high temperature to obtain a mullite nanofiber aerogel product. The mullite nanofiber aerogel has high porosity and low thermal conductivity, providing a thermal conductivity of 0.0375W / (m·K) at 1300°C.
[0004] However, existing research has not involved the application of mullite aerogel in scenarios with high temperature and low thermal conductivity up to 1600°C. Therefore, an aerogel material with simple process, high efficiency and high temperature resistance and low thermal conductivity is needed. Summary of the invention
[0005] In order to solve the above-mentioned technical problems existing in the prior art, the present application provides a high-temperature resistant and low-thermal conductivity aerogel composite material and its preparation method and application, so as to overcome the technical problems in the prior art such as complex preparation process, low production efficiency and high temperature resistance.
[0006] In order to achieve the above purpose, the technical solution of the embodiment of the present application is:
[0007] The first aspect of the present application provides a method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, comprising:
[0008] The mullite aerogel powder, a surfactant and water are stirred and mixed to obtain a mullite aerogel aqueous paste;
[0009] The mullite aerogel aqueous paste, potassium hexatitanate whiskers and mullite synthetic raw materials are uniformly mixed and then dehydrated to obtain a reaction precursor powder;
[0010] The reaction precursor powder is molded and then subjected to high temperature annealing to obtain a high temperature resistant and low thermal conductivity aerogel composite material;
[0011] The mullite synthesis raw material is composed of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3-4.
[0012] In combination with the first aspect, preferably, the mass ratio of the mullite aerogel aqueous paste, the potassium hexatitanate whiskers and the mullite synthetic raw material is 1:1-3:0.05-0.2.
[0013] In combination with the first aspect, preferably, the mass ratio of the mullite aerogel aqueous paste, the potassium hexatitanate whiskers and the mullite synthetic raw material is 1:2:0.125.
[0014] In combination with the first aspect, preferably, the water contact angle of the mullite aerogel powder is greater than 150°, the particle size is 50-200 μm, and the tap density is 0.05-0.1 g / cm 3 , thermal conductivity is 0.012~0.018W / (m·K).
[0015] In combination with the first aspect, preferably, the surfactant is one or more of an ammonium salt type surfactant, a quaternary ammonium salt type surfactant, a heterocyclic surfactant, a carboxylate, a sulfonate, a sulfate ester salt and a phosphate ester salt.
[0016] In combination with the first aspect, preferably, the content of the surfactant accounts for 0.1 to 1 wt% of the total mass of the mullite aerogel powder and water;
[0017] And / or, the content of the mullite aerogel powder accounts for 20-30wt% of the total mass of the mullite aerogel powder and water.
[0018] In combination with the first aspect, preferably, when the reaction precursor powder is compression molded, the compression molding pressure is 0.2-0.5 MPa.
[0019] In combination with the first aspect, preferably, when the high temperature annealing treatment is performed, the annealing temperature is 1000-1200° C. and the annealing time is 2 hours.
[0020] The second aspect of the present application provides a high temperature resistant and low thermal conductivity aerogel composite material as described in the first aspect.
[0021] The third aspect of the present application provides a use of the high temperature resistant and low thermal conductivity aerogel composite material prepared by the method described in the first aspect or the high temperature resistant and low thermal conductivity aerogel composite material described in the second aspect for preparing nanoporous thermal insulation materials.
[0022] Compared with the prior art, the advantages or beneficial effects of the embodiments of the present application include at least:
[0023] The preparation method provided in the present application comprises adding a surfactant to a water-dispersible slurry of mullite aerogel powder, mixing it with potassium hexatitanate whiskers and mullite synthetic raw materials, and then dehydrating it, and subjecting the dehydrated reaction precursor powder to compression molding and high-temperature annealing in sequence. On the one hand, the pore structure of the mullite aerogel matrix phase can be effectively regulated based on the foaming effect of the surfactant, so that the pore structure of the mullite aerogel matrix phase can be controllably increased and the uniformity of the pore structure is improved, which is beneficial to the formation of small molecular weight potassium hexatitanate whiskers and mullite synthetic raw materials into mullite aerogel. The filling is inserted into the matrix phase, so that based on the negative temperature coefficient characteristics and infrared reflection ability of potassium hexatitanate whiskers, the prepared mullite aerogel composite material has low thermal conductivity. On the other hand, the mullite synthetic raw materials inserted into the mullite aerogel matrix phase can interact with each other during high-temperature annealing and generate a mullite binding phase. Since the generated mullite binding phase is inserted and bonded to the mullite aerogel matrix phase, the stability of the prepared mullite aerogel composite material can be greatly improved, and the prepared mullite aerogel composite material has excellent thermal insulation and temperature resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope image of the high temperature resistant and low thermal conductivity aerogel composite material prepared in Example 1;
[0025] Figure 2 This is a scanning electron microscope image of the high temperature resistant and low thermal conductivity aerogel composite material prepared in Example 5. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings. The described embodiments should not be regarded as limiting the present application. All other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of this application.
[0027] In the following description, reference is made to "some embodiments", which describe a subset of all possible embodiments, but it is understood that "some embodiments" may be the same subset or different subsets of all possible embodiments, and may be combined with each other without conflict. Unless otherwise defined, all technical and scientific terms used in the embodiments of the present application have the same meaning as those commonly understood by those skilled in the art of the technical field of the embodiments of the present application. The terms used in the embodiments of the present application are only for the purpose of describing the embodiments of the present application and are not intended to limit the present application.
[0028] In the following description of this embodiment, the terms "include", "comprising", "having" and "containing" are all open terms, meaning including but not limited to.
[0029] It should be noted that all raw materials / reagents in the examples of the present application can be purchased on the market or prepared according to conventional methods well known to those skilled in the art; the term "and / or" in the examples of the present application is only used to describe the association relationship between associated objects, indicating that three relationships may exist, for example, A and / or B means the existence of A alone, B alone, and A and B at the same time, wherein A and B may be singular or plural, and the character " / " generally indicates that the associated objects before and after are in an "or" relationship.
[0030] In the following description of this embodiment, the term "at least one" refers to one or more, and "plurality" refers to two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b or c", or "at least one of a, b and c", can all represent: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0031] Those skilled in the art should understand that in the following description of the embodiments of the present application, the order of serial numbers does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0032] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0033] Those skilled in the art will appreciate that the numerical ranges in the examples of the present application are to be understood as also specifically disclosing each intermediate value between the upper and lower limits of the range. Each smaller range between the intermediate values in any stated value and stated range and any other stated value or intermediate value in the range is also included in the present application. The upper and lower limits of these smaller ranges may be independently included or excluded in the scope.
[0034] Unless otherwise stated, the technical / scientific terms used herein have the same meanings as those generally understood by those skilled in the art in the field described in the present application. Although the present application only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the embodiments or test cases of the present application. All documents mentioned in this specification are generally incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of the present application shall prevail.
[0035] It should be noted that all raw materials and / or reagents in the examples of the present application are purchased on the market or prepared according to conventional methods well known to those skilled in the art.
[0036] In a first aspect, an embodiment of the present application provides a method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, the preparation method comprising:
[0037] S10: stirring and mixing mullite aerogel powder, surfactant and water to obtain a mullite aerogel aqueous paste;
[0038] S20: uniformly mixing the mullite aerogel aqueous paste, potassium hexatitanate whiskers and mullite synthetic raw materials and then dehydrating the mixture to obtain a reaction precursor powder;
[0039] S30: After the reaction precursor powder is molded, it is subjected to high temperature annealing treatment to obtain a high temperature resistant and low thermal conductivity aerogel composite material;
[0040] The mullite synthesis raw material is composed of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3-4.
[0041] Wherein, the molecular formula of the mullite is 3Al2O3-2SiO2.
[0042] The preparation method provided in the present application comprises adding a surfactant to a water-dispersible slurry of mullite aerogel powder, mixing it with potassium hexatitanate whiskers and mullite synthetic raw materials, and then dehydrating it, and subjecting the dehydrated reaction precursor powder to compression molding and high-temperature annealing in sequence. On the one hand, the pore structure of the mullite aerogel matrix phase can be effectively regulated based on the foaming effect of the surfactant, so that the pore structure of the mullite aerogel matrix phase can be controllably increased and the uniformity of the pore structure is improved, which is beneficial to the formation of small molecular weight potassium hexatitanate whiskers and mullite synthetic raw materials into mullite aerogel. The filling is inserted into the matrix phase, so that based on the negative temperature coefficient characteristics and infrared reflection ability of potassium hexatitanate whiskers, the prepared mullite aerogel composite material has low thermal conductivity. On the other hand, the mullite synthetic raw materials inserted into the mullite aerogel matrix phase can interact with each other during high-temperature annealing and generate a mullite binding phase. Since the generated mullite binding phase is inserted and bonded to the mullite aerogel matrix phase, the stability of the prepared mullite aerogel composite material can be greatly improved, and the prepared mullite aerogel composite material has excellent thermal insulation and temperature resistance.
[0043] In step S10 of the preparation method provided in the present application, there is no limitation on the specific implementation method of dissolving. For example, stirring can be performed under heating conditions or dissolving can be performed under room temperature conditions, as long as the mullite aerogel powder and the surfactant are evenly dispersed in water. In the present invention, the stirring speed can be 1000-5000 rpm, and the stirring time can be 10-180 min.
[0044] In the present application, mullite aerogel powder, surfactant and water are subjected to high-speed stirring reaction to obtain an aqueous paste with an aerogel content of 20-30%. The aqueous paste is characterized in that the properties of the mullite aerogel powder can be restored after drying.
[0045] Here, mullite aerogel has the characteristics of high temperature resistance and can still maintain a nanoporous structure at 1600°C, which can give the composite material a low thermal conductivity in the medium and low temperature stages, while reducing the density of the composite material.
[0046] In step S20 of the preparation method provided in the present application, the gas phase SiO2 and the gas phase Al2O3 can be mixed uniformly first, and then potassium hexatitanate whiskers are added to the mixture and mixed uniformly at high speed, and then the water is dried to obtain a reaction precursor powder. It should be noted that the reaction precursor powder collected in the embodiment of the present application is white powder.
[0047] The potassium hexatitanate whiskers in the present application have the characteristic of negative temperature coefficient, that is, the higher the temperature, the lower the thermal conductivity; at the same time, they also have the function of infrared reflection, so under the appropriate ratio, they can not only maintain low thermal conductivity at medium and low temperatures, but also maintain low thermal conductivity at high temperatures.
[0048] In step S30 of the preparation method provided in the present application, the white powder obtained in the above step S20 is molded at a molding pressure of 0.2 to 0.5 MPa, and the mixed white powder is compacted to obtain a block, but this molding process does not destroy the nanoporous structure of the aerogel. After the white powder is molded, the obtained block is placed in a high-temperature furnace and heated at 1000 to 1200°C for 2 hours, and the gas phase SiO2 and gas phase Al2O3 in the block react to form mullite.
[0049] In a specific embodiment, the mass ratio of the mullite aerogel aqueous paste, potassium hexatitanate whiskers and mullite synthetic raw materials in the embodiment of the present application is preferably 1:1-3:0.05-0.2.
[0050] In a specific embodiment, the mass ratio of the mullite aerogel aqueous paste, potassium hexatitanate whiskers and mullite synthetic raw material in the embodiment of the present application is more preferably 1:2:0.125.
[0051] In a specific embodiment, the water contact angle of the mullite aerogel powder in the embodiment of the present application is greater than 150°, the particle size is preferably 50 to 200 μm, and the tap density is preferably 0.05 to 0.1 g / cm 3 , the thermal conductivity is preferably 0.012 to 0.018 W / (m·K).
[0052] In a specific embodiment, the surfactant in the embodiment of the present application is preferably one of an ammonium salt surfactant, a quaternary ammonium salt surfactant, a heterocyclic surfactant, a carboxylate, a sulfonate, a sulfate ester salt and a phosphate ester salt.
[0053] In a specific embodiment, the content of the surfactant in the embodiment of the present application accounts for 0.1-1 wt % of the total mass of the mullite aerogel powder and water.
[0054] Among them, when the amount of surfactant added is too little, it may not be able to fully cover the surface of the aerogel nanoparticles, resulting in easy agglomeration between particles. The agglomerated nano-ions will block the pores, reduce the porosity and specific surface area of the aerogel, and thus affect its high temperature resistance and low thermal conductivity. When the amount of surfactant added is too much, although it can better prevent the agglomeration of nanoparticles, too much surfactant may form a thick coating layer, hindering the interaction between aerogel nanoparticles. This may cause the network structure of the aerogel to become loose, and may also affect the viscosity, fluidity, etc. of the water-based paste, thereby affecting its high temperature resistance and low thermal conductivity.
[0055] In the examples of the present application, the content of the surfactant is 0.1-1 wt %.
[0056] In a specific embodiment, the content of the mullite aerogel powder in the embodiment of the present application accounts for 20 to 30 wt % of the total mass of the mullite aerogel powder and water.
[0057] In the embodiment of the present application, the content of the mullite aerogel powder accounts for 20-30wt% of the total mass of the mullite aerogel powder and water.
[0058] In a specific embodiment, when compression molding is performed in the embodiment of the present application, the compression molding pressure is preferably 0.2 to 0.5 MPa.
[0059] It should be noted that in the embodiment of the present application, the mixed white powder obtained in the above steps can be compacted to obtain a block under a molding pressure of 0.2 to 0.5 MPa, but the nanoporous structure of the aerogel is not destroyed.
[0060] In a specific embodiment, when high temperature annealing is performed in the embodiment of the present application, the annealing temperature is preferably 1000-1200° C., and the annealing time is preferably 2 hours.
[0061] It should be noted that the compacted block is subjected to annealing treatment at 1000-1200° C. in a high-temperature furnace, and the gas phase SiO 2 and gas phase Al 2 O 3 in the block can react to form mullite.
[0062] In the present application, during the preparation process of the aerogel composite material, gas phase SiO2 and gas phase Al2O3 are introduced, and the two react at high temperature to form a high temperature resistant mullite phase, thereby improving the mechanical strength and temperature resistance of the aerogel material.
[0063] In a second aspect, an embodiment of the present application provides a high temperature resistant and low thermal conductivity aerogel composite material prepared by the method described in the first aspect.
[0064] In a third aspect, an embodiment of the present application provides an application of a high temperature resistant and low thermal conductivity aerogel composite material prepared by the method described in the first aspect or a high temperature resistant and low thermal conductivity aerogel composite material described in the second aspect for preparing a nanoporous thermal insulation material.
[0065] The technical method of the present application will be further described below in conjunction with specific embodiments.
[0066] Example 1
[0067] This embodiment provides a method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, and the specific steps are as follows:
[0068] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water are stirred at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0069] Step 2: Add 0.125 parts by mass of mullite synthesis raw material and 2 parts by mass of potassium hexatitanate whisker to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder. The mullite synthesis raw material is a mixture of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3;
[0070] Step 3: After the reaction precursor powder is compression molded at 0.35 MPa, it is subjected to high temperature annealing treatment at 1100° C. to obtain a high temperature resistant and low thermal conductivity aerogel composite material.
[0071] Example 2
[0072] This embodiment provides a method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, and the specific steps are as follows:
[0073] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water are stirred at 1000 rpm for 20 minutes to obtain a mullite aerogel aqueous paste;
[0074] Step 2: Add 0.125 parts by mass of mullite synthesis raw material and 2 parts by mass of potassium hexatitanate whisker to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder. The mullite synthesis raw material is a mixture of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3;
[0075] Step 3: After the reaction precursor powder is compression molded at 0.2 MPa, it is subjected to high temperature annealing treatment at 1000° C. to obtain a high temperature resistant and low thermal conductivity aerogel composite material.
[0076] Example 3
[0077] This embodiment provides a method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, and the specific steps are as follows:
[0078] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water are stirred at 3000 rpm for 5 minutes to obtain a mullite aerogel aqueous paste;
[0079] Step 2: Add 0.125 parts by mass of mullite synthesis raw material and 2 parts by mass of potassium hexatitanate whisker to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder. The mullite synthesis raw material is a mixture of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3;
[0080] Step 3: After the reaction precursor powder is compression molded at 0.5 MPa, it is subjected to high temperature annealing treatment at 1100° C. to obtain a high temperature resistant and low thermal conductivity aerogel composite material.
[0081] Example 4
[0082] This embodiment provides a method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, and the specific steps are as follows:
[0083] Step 1: 20 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 80 parts by mass of water are stirred and reacted at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0084] Step 2: Add 0.05 parts by mass of mullite synthesis raw material and 1 part by mass of potassium hexatitanate whisker to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder. The mullite synthesis raw material is a mixture of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3;
[0085] Step 3: After the reaction precursor powder is compression molded at 0.35 MPa, it is subjected to high temperature annealing treatment at 1100° C. to obtain a high temperature resistant and low thermal conductivity aerogel composite material.
[0086] Example 5
[0087] This embodiment provides a method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, and the specific steps are as follows:
[0088] Step 1: 30 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 70 parts by mass of water are stirred at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0089] Step 2: Add 0.2 parts by mass of mullite synthesis raw material and 3 parts by mass of potassium hexatitanate whiskers to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder. The mullite synthesis raw material is a mixture of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3;
[0090] Step 3: After the reaction precursor powder is compression molded at 0.35 MPa, it is subjected to high temperature annealing treatment at 1100° C. to obtain a high temperature resistant and low thermal conductivity aerogel composite material.
[0091] In order to illustrate the practical effects of the embodiments, the present application also provides comparative examples 1-4.
[0092] Comparative Example 1
[0093] This comparative example 1 provides a method for preparing an aerogel composite material, and the specific steps are as follows:
[0094] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water are stirred at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0095] Step 2: Add 0.125 parts by mass of mullite synthesis raw material and 0.5 parts by mass of potassium hexatitanate whisker to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder. The mullite synthesis raw material is a mixture of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3;
[0096] Step 3: After the reaction precursor powder is molded at 0.35 MPa, it is subjected to high temperature annealing treatment at 1100° C. to obtain an aerogel composite material.
[0097] Comparative Example 2
[0098] This comparative example 2 provides a method for preparing an aerogel composite material, and the specific steps are as follows:
[0099] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water are stirred at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0100] Step 2: Add 0.125 parts by mass of a mullite synthesis raw material to 1 part by mass of a mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder. The mullite synthesis raw material is a mixture of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3;
[0101] Step 3: After the reaction precursor powder is molded at 0.35 MPa, it is subjected to high temperature annealing treatment at 1100° C. to obtain an aerogel composite material.
[0102] Comparative Example 3
[0103] This comparative example 3 provides a method for preparing an aerogel composite material, and the specific steps are as follows:
[0104] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water were stirred at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0105] Step 2: Add 0.125 parts by mass of commercially available mullite powder and 2 parts by mass of potassium hexatitanate whiskers to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder;
[0106] (3) The reaction precursor powder is compression molded at 0.35 MPa and then subjected to high temperature annealing treatment at 1100° C. to obtain an aerogel composite material.
[0107] Comparative Example 4
[0108] This comparative example 4 provides a method for preparing an aerogel composite material, and the specific steps are as follows:
[0109] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water were stirred at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0110] Step 2: Add 2 parts by mass of gas-phase SiO2 and 2 parts by mass of potassium hexatitanate whiskers to the mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder;
[0111] Step 3: After the reaction precursor powder is molded at 0.35 MPa, it is subjected to high temperature annealing treatment at 1100° C. to obtain an aerogel composite material.
[0112] Comparative Example 5
[0113] This comparative example 5 provides a method for preparing an aerogel composite material, and the specific steps are as follows:
[0114] Step 1: 25 parts by mass of mullite aerogel powder, 0.1 parts by mass of dodecyltrimethylammonium chloride and 75 parts by mass of water were stirred at 2000 rpm for 10 minutes to obtain a mullite aerogel aqueous paste;
[0115] Step 2: Add 3 parts by mass of gas-phase Al2O3 and 2 parts by mass of potassium hexatitanate whiskers to 1 part by mass of mullite aerogel aqueous paste, mix well, dry the water, and collect the reaction precursor powder;
[0116] Step 3: The reaction precursor powder is compression molded at 0.35 MPa, and then subjected to high temperature annealing treatment at 1100° C. to obtain an aerogel composite material.
[0117] The performance of the aerogel composite materials prepared in the examples and comparative examples was tested, and the results are shown in Table 1.
[0118]
[0119] According to Table 1, Examples 1-3 have strong heat resistance, with the highest instantaneous heat resistance temperature reaching 1600°C and the longest heat resistance temperature reaching 1300°C. Moreover, they not only have a low thermal conductivity at room temperature, with the lowest reaching 0.022W / (m·K), but also when the temperature rises to 1600°C, the thermal conductivity does not exceed 0.053W / (m·K). The prepared mullite aerogel composite material has excellent heat insulation and temperature resistance.
[0120] Comparative Example 1 and Example 4-5 show that when the content of mullite (3Al2O3-2SiO2) aerogel and potassium hexatitanate whisker decreases, the instantaneous thermal conductivity and long-term thermal conductivity at high temperature will both increase. This is because mullite aerogel can still maintain a nanoporous structure at 1600°C and has the characteristics of efficient heat insulation. When its total content decreases, the heat insulation effect will also decrease, resulting in a higher thermal conductivity at high temperature. Potassium hexatitanate whiskers have the characteristics of a negative temperature coefficient, that is, the higher the temperature, the lower the thermal conductivity; at the same time, they also have the function of infrared reflection. Under a suitable ratio, they can not only maintain low thermal conductivity at medium and low temperatures, but also maintain low thermal conductivity at high temperatures. Therefore, when its content is reduced, the thermal conductivity at room temperature and high temperature increases. When the content of mullite aerogel and potassium hexatitanate whisker increases, the mixed paste formed is mixed with the whisker. Since the concentration of the paste and the content of the whisker increase, the uniformity of the mixing decreases, thereby reducing the thermal insulation performance of the composite material.
[0121] Comparison of Example 1 and Comparative Examples 1-2 shows that when the content of potassium hexatitanate whiskers is too low or not added, the temperature resistance and thermal insulation performance are greatly reduced. This is because potassium hexatitanate whiskers have the characteristics of negative temperature coefficient, that is, the higher the temperature, the lower the thermal conductivity; at the same time, they also have the function of infrared reflection. Under the appropriate ratio, they can not only maintain low thermal conductivity at medium and low temperatures, but also maintain low thermal conductivity at high temperatures. When its content is reduced, the temperature resistance and thermal insulation performance are greatly reduced.
[0122] Comparative Example 1 and Comparative Examples 3-5 show that the mullite powder available on the market added to the aerogel composite material prepared in Comparative Example 3 absorbs water into the nanoporous structure, and the capillary pressure generated during the drying process causes the aerogel pore structure to collapse, and eventually loses the nanoporous thermal insulation performance. The heat resistance and strength of the aerogel composite material prepared by adding only gas-phase SiO2 in Comparative Example 4 decrease. The heat resistance and strength of the aerogel composite material prepared by adding only gas-phase Al2O3 in Comparative Example 5 decrease.
[0123] Figure 1 This is a scanning electron microscope image of the high temperature resistant and low thermal conductivity aerogel composite material prepared in Example 1. Figure 2 This is a scanning electron microscope image of the high temperature resistant and low thermal conductivity aerogel composite material prepared in Example 5.
[0124] according to Figure 1 and Figure 2 It can be seen that Figure 1 The particle distribution in the mixture is relatively uniform. This is because when the content of mullite aerogel and potassium hexatitanate whiskers increases, the uniformity of mixing decreases.
[0125] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any person skilled in the art who is familiar with the present technical field can easily think of changes or substitutions within the technical scope disclosed in the present application, which should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing a high temperature resistant and low thermal conductivity aerogel composite material, characterized in that: include: The mullite aerogel powder, surfactant and water are stirred and mixed to obtain a mullite aerogel aqueous paste; The mullite aerogel aqueous paste, potassium hexatitanate whiskers and mullite synthetic raw materials are uniformly mixed and then dehydrated to obtain a reaction precursor powder; The reaction precursor powder is molded and then subjected to high temperature annealing to obtain a high temperature resistant and low thermal conductivity aerogel composite material; The mullite synthesis raw material is composed of gas phase SiO2 and gas phase Al2O3 in a molar ratio of 2:3-4.
2. The method for preparing a high temperature resistant and low thermal conductivity aerogel composite material according to claim 1, characterized in that: The mass ratio of the mullite aerogel aqueous paste, the potassium hexatitanate whisker and the mullite synthetic raw material is 1:1-3:0.05-0.
2.
3. The method for preparing a high temperature resistant and low thermal conductivity aerogel composite material according to claim 2, characterized in that: The mass ratio of the mullite aerogel aqueous paste, the potassium hexatitanate whisker and the mullite synthetic raw material is 1:2:0.
125.
4. The method for preparing a high temperature resistant and low thermal conductivity aerogel composite material according to claim 1, characterized in that: The water contact angle of the mullite aerogel powder is greater than 150°, the particle size is 50-200 μm, and the tap density is 0.05-0.1 g / cm 3 , thermal conductivity is 0.012~0.018W / (m·K).
5. The method for preparing a high temperature resistant and low thermal conductivity aerogel composite material according to claim 1, characterized in that: The surfactant is one or more of an ammonium salt surfactant, a quaternary ammonium salt surfactant, a heterocyclic surfactant, a carboxylate, a sulfonate, a sulfate ester salt and a phosphate ester salt.
6. The method for preparing a high temperature resistant and low thermal conductivity aerogel composite material according to claim 1, characterized in that: The content of the surfactant accounts for 0.1-1wt% of the total mass of the mullite aerogel powder and water; And / or, the content of the mullite aerogel powder accounts for 20-30wt% of the total mass of the mullite aerogel powder and water.
7. The method for preparing a high temperature resistant and low thermal conductivity aerogel composite material according to claim 1, characterized in that: When the reaction precursor powder is compression molded, the compression molding pressure is 0.2-0.5 MPa.
8. The method for preparing a high temperature resistant and low thermal conductivity aerogel composite material according to claim 1, characterized in that: When the high temperature annealing treatment is performed, the annealing temperature is 1000-1200° C. and the annealing time is 2 hours.
9. A high temperature resistant and low thermal conductivity aerogel composite material prepared by the method according to any one of claims 1 to 8.
10. Use of the high temperature resistant and low thermal conductivity aerogel composite material prepared by the method according to any one of claims 1 to 8 or the high temperature resistant and low thermal conductivity aerogel composite material according to claim 9 in preparing nanoporous thermal insulation materials.
Citation Information
Patent Citations
A method for preparing lightweight, heat-insulating mullite nanofiber aerogel
CN110078425B