Preparation method of alumina ceramic sintered at ultralow temperature

Through the combination of B2O3-Li2O-Cr2O3-TiO2-SiO2 sintering assist system and nanomodified silicon carbide, the problems of high sintering temperature of alumina ceramics and monomer acrylamide toxicity are solved, ultra-low temperature sintering and performance improvement are achieved, and oxidation is significantly improved Mechanical properties of aluminum ceramics.

CN118955104AActive Publication Date: 2024-11-15YANTAI HEJING CERAMIC NEW MATERIALS

Patent Information

Application Number
CN202411026669.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing alumina ceramics have high sintering temperature, which leads to high energy consumption, and the monomer acrylamide is neurotoxic, which limits its application. It is urgently needed to prepare an ultra-low-temperature sintered alumina ceramic to improve flexural strength, compressive strength, and fracture. Toughness and Young's modulus performance.

Method used

Using the combination of B2O3-Li2O-Cr2O3-TiO2-SiO2 sintering aid system and nanomodified silicon carbide, low-melting point glass and solid-phase sintered bodies are formed through ball milling and surface modification, which activates the sintering activity of alumina and passes through nano The good combination of modified silicon carbide and alumina matrix improves the mechanical properties of the material.

Benefits of technology

The densification process is achieved at a lower temperature, the mechanical strength and wear resistance of alumina ceramics are improved, the bending strength, compressive strength, fracture toughness and Young's modulus performance are significantly improved, and the sintering temperature and energy consumption are reduced. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968744430000101
    Figure BDA0004968744430000101
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of aluminum oxide ceramics, in particular to a preparation method of ultralow-temperature sintered aluminum oxide ceramics, which comprises the following steps: S1.1, putting aluminum oxide powder and water into a ball mill filled with ballstones according to a ratio of (3-4): 1, and carrying out ball milling for 20-30 hours to obtain aluminum oxide grinding slurry with the specific gravity of 1.60-1.70; s1.2, B2O3-Li2O-Cr2O3-TiO2-SiO2 is selected as a sintering assisting system, and the B2O3-Li2O-Cr2O3-TiO2-SiO2 and the S1.3, heating 2-3wt% of Cardlan gum to dissolve the Cardlan gum, adding the Cardlan gum into the prepared aluminum oxide slurry, uniformly stirring, and injecting into an aluminum oxide ceramic mold; and S1.4, putting the baked aluminum oxide primary blank into a sintering kiln to form the aluminum oxide ceramic. Nano-modified silicon carbide is introduced into a mixed sintering assisting system, and a firm interface structure is formed between the nano-modified silicon carbide and an aluminum oxide matrix, so that cracks can be effectively prevented from being generated and expanded on an interface of nano-modified silicon carbide particles and the aluminum oxide matrix, and the bending strength of the composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alumina ceramic preparation, and in particular to a method for preparing ultra-low temperature sintered alumina ceramic. Background Art

[0002] Alumina ceramics are the most common advanced precision ceramic materials and are also relatively traditional materials. High-purity alumina ceramics have been widely used in many industries as an excellent ceramic material. This material has excellent performance in electrical insulation, high thermal conductivity, high chemical resistance, good wear resistance and low thermal expansion. However, due to the high sintering temperature of alumina ceramics, it consumes a lot of energy and has high requirements for thermal equipment, which limits the scope of use of alumina ceramics to a certain extent; the gel molding process of type ceramics can reduce the manufacturing cost of ceramics and improve the reliability of ceramic parts, so it has received widespread attention. Gel injection molding has the advantages of high strength, near net size, and the ability to mold complex and large-sized green bodies. It is considered to be an advanced industrial molding method. However, due to the neurotoxicity of monomer acrylamide, its promotion and application are limited. The selection of a new non-toxic gel system to achieve non-toxic gel injection molding of ceramics has important practical significance.

[0003] In order to solve the shortcomings of the existing technology, there is an urgent need for a method for preparing ultra-low temperature sintered alumina ceramics to prepare alumina ceramic green bodies with complex shapes and improve the flexural strength, compressive strength, fracture toughness and Young's modulus properties of alumina ceramics. In view of this, we propose a method for preparing ultra-low temperature sintered alumina ceramics. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing ultra-low temperature sintered alumina ceramics to solve the problems raised in the above background technology to solve the deficiencies of the prior art and improve the bending strength, compressive strength, fracture toughness and Young's modulus properties of alumina ceramics.

[0005] To achieve the above object, the present invention provides a method for preparing ultra-low temperature sintered alumina ceramics, comprising the following steps:

[0006] S1.1. Put alumina powder and water in a ratio of 3 to 4:1 into a ball mill equipped with ball stones for ball milling for 20 to 30 hours to obtain alumina grinding slurry. The specific gravity of the alumina grinding slurry is 1.60 to 1.70, indicating that an appropriate solid-liquid ratio and particle refinement degree have been achieved;

[0007] The alumina grinding slurry, alumina powder, dispersant and adhesive are mixed evenly in a ratio of 200:100-180:30-50:2-5, and the specific gravity after mixing is 1.80-1.90;

[0008] S1.2, select B2O3-Li2O-Cr2O3-TiO2-SiO2 as the sintering aid system, and mix B2O3, Li2O, Cr2O3, TiO2 and SiO2 in a weight ratio of 3-4: 0.5-1: 0.5-1: 1-2: 0.5-1 by a mixer;

[0009] Introducing nano-modified silicon carbide into the mixed sintering aid system, wherein the mixing mass ratio of the nano-modified silicon carbide to the sintering aid system is 1 to 3:100;

[0010] B2O3 is a strong flux material. When heated and fired, it will form low-melting glass with SiO2, which helps the sintering process go smoothly. B2O3 is easy to form low-melting compounds with SiO2, further dissolving Al2O3, thus forming a more complex boron-containing silicate melt, activating the sintering of corundum, and at the same time improving the mechanical strength and wear resistance. 3+ With Al 3+ The two ionic radii are not much different and have the same crystal form, so they are easy to form a solid solution with Al2O3; TiO2 reacts with Al2O3 to form Al2Ti7O 15 Solid-phase sintering can more easily promote the growth and densification of alumina ceramic grains; Li2O can form a liquid phase with Al2O3 during high temperature, increasing the fluidity of the system;

[0011] S1.3, heat 2-3wt% of Curdlan gum to dissolve it and then add it to the prepared alumina slurry, stir it evenly and inject it into the mold of alumina ceramics, place it in a curing room at 20-30°C, wait for the slurry to cool, and start demoulding; Curdlan gum is used to increase the viscosity of the alumina slurry, which helps to improve the stability of the molded body, reduce cracking, and maintain the integrity of the shape during the subsequent drying and sintering process;

[0012] The alumina embryos after demoulding are cured in the curing room for 12-24 hours, and then moved into a drying room at 80-85℃ for 10-16 hours;

[0013] S1.4. Place the baked alumina embryo in a sintering kiln at 1350°C-1400°C for 24-28 hours to form alumina ceramics.

[0014] Preferably, in S1.1, the alumina powder is a mixed powder of 100-200:300-400 mesh with a mass ratio of 2:1.

[0015] Preferably, in S1.1, the dispersant is a mixture of one or more of ammonium citrate, polycarboxylate, and polyacrylate.

[0016] Preferably, in S1.1, the adhesive is a mixture of one or more of polyvinyl alcohol, polyacrylamide and polyethylene glycol.

[0017] Preferably, in said S1.1, the pH of the prepared alumina slurry is 9-10.

[0018] Preferably, in S1.2, the nano-modified silicon carbide is obtained by surface-modifying nano-silicon carbide with γ-mercaptopropyltriethoxysilane;

[0019] Among them, γ-mercaptopropyltriethoxysilane is an organic compound containing a silane coupling agent, one end of γ-mercaptopropyltriethoxysilane contains a silane group that can react with the surface of an inorganic material (such as SiC), and the other end contains an organic functional group (thiol) that can react or be compatible with an organic matrix (such as a polymer); the silane group can react with the hydroxyl group on the surface of SiC to form a stable silicon-oxygen bond, so that the silane is firmly attached to the surface of SiC; the thiol group can react with the functional group in some polymer matrices, or at least be compatible with them, thereby improving the interface bonding strength between SiC and the matrix;

[0020] Furthermore, nano-modified silicon carbide has extremely high strength and hardness. When it is evenly distributed in the alumina matrix, it can effectively hinder the expansion of cracks and improve the bending strength and compressive strength of the material. This "bridging effect" and "pinning effect" can significantly improve the overall mechanical properties of the material.

[0021] At the same time, the interface bonding force between nano-modified silicon carbide and alumina matrix is ​​strong, which can form a strong interface structure, further improving the overall performance of the composite material. By controlling the sintering conditions, the good bonding between nano-modified silicon carbide and alumina is promoted, and the interface compatibility is enhanced;

[0022] The specific modification steps are:

[0023] S2.1, dispersing nano silicon carbide powder in ethanol solvent to obtain a 20wt% nano silicon carbide solution, and adding γ-mercaptopropyltriethoxysilane to the nano silicon carbide solution;

[0024] S2.2, at room temperature, stirring with a stirrer, and promoting the chemical reaction between γ-mercaptopropyltriethoxysilane and the hydroxyl groups on the surface of the nano-silicon carbide to form a stable chemical bond;

[0025] The mercapto group (-SH) and / or silanol group (-Si(OC2H5)3) in γ-mercaptopropyltriethoxysilane undergoes condensation or substitution reaction with the hydroxyl group (-OH) on the surface of SiC to form a stable silicon-oxygen bond (-Si iOS i-) or thiol bond, thereby achieving surface coating and modification of nano-silicon carbide;

[0026] S2.3, after the reaction is completed, remove the unreacted γ-mercaptopropyltriethoxysilane and other by-products by filtering;

[0027] S2.4. Dry the modified nano-silicon carbide powder at a suitable temperature to obtain the final product.

[0028] Preferably, in S2.1, the mass ratio of γ-mercaptopropyltriethoxysilane to nano-silicon carbide powder is 1:10.

[0029] Preferably, in S2.2, the stirrer continues stirring at a speed of 680-800 rpm for 6-8 hours.

[0030] Preferably, in S1.4, the sintering kiln is a shuttle kiln.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. In the preparation method of ultra-low temperature sintered alumina ceramics, a B2O3-Li2O-Cr2O3-TiO2-SiO2 sintering aid system is used, wherein B2O3 is used as a strong flux raw material to enable alumina to complete the densification process at a relatively low temperature, i.e., the so-called ultra-low temperature sintering, which helps to accelerate material migration and particle rearrangement, and promote the densification of the sintered body; and the complex borosilicate melt formed by B2O3 and SiO2 can further dissolve Al 2O3 particles, activate the sintering activity of alumina, and is conducive to forming a more compact microstructure, thereby improving the mechanical strength and wear resistance of the ceramics; the sintering aid system effectively reduces the sintering temperature and improves the sintering efficiency through the synergistic effect of multiple mechanisms, while optimizing the microstructure and mechanical properties of alumina ceramics, and solving the problems of insufficient strength and toughness that may exist in traditional sintering methods.

[0033] 2. In the preparation method of ultra-low temperature sintered alumina ceramics, nano-modified silicon carbide is introduced into the mixed sintering aid system. The interface bonding force between the nano-modified silicon carbide and the alumina matrix is ​​strong, and a strong interface structure can be formed, further improving the overall performance of the composite material. By controlling the sintering conditions, the good bonding between the nano-modified silicon carbide and alumina is promoted, and the interface compatibility is enhanced. The enhancement of the interface bonding force can effectively prevent the initiation and expansion of cracks at the interface between the nano-modified silicon carbide particles and the alumina matrix. Under the action of bending load, the stronger interface can more effectively transfer stress and avoid stress concentration, thereby improving the bending strength of the composite material. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The present invention relates to a method for preparing ultra-low temperature sintered alumina ceramics, wherein the dispersant is a mixture of one or more of ammonium citrate, polycarboxylate, and polyacrylate; the adhesive is a mixture of one or more of polyvinyl alcohol, polyacrylamide, and polyethylene glycol;

[0036] In this embodiment, the dispersant is preferably ammonium citrate, and the adhesive is preferably polyvinyl alcohol.

[0037] B2O3 is a strong flux material. When heated and fired, it will form low-melting glass with SiO2, which helps the sintering process go smoothly. B2O3 is easy to form low-melting compounds with SiO2, further dissolving Al2O3, thus forming a more complex boron-containing silicate melt, activating the sintering of corundum, and at the same time improving the mechanical strength and wear resistance. 3+ With Al 3+ The two ionic radii are not much different and have the same crystal form, so they are easy to form a solid solution with Al2O3; TiO2 reacts with Al2O3 to form Al2Ti7O 15 Solid-phase sintering can more easily promote the growth and densification of alumina ceramic grains; Li2O can form a liquid phase with Al2O3 during high temperature, increasing the fluidity of the system;

[0038] Among them, γ-mercaptopropyltriethoxysilane is an organic compound containing a silane coupling agent, one end of γ-mercaptopropyltriethoxysilane contains a silane group that can react with the surface of an inorganic material (such as SiC), and the other end contains an organic functional group (thiol) that can react or be compatible with an organic matrix (such as a polymer); the silane group can react with the hydroxyl group on the surface of SiC to form a stable silicon-oxygen bond, so that the silane is firmly attached to the surface of SiC; the thiol group can react with the functional group in some polymer matrices, or at least be compatible with them, thereby improving the interface bonding strength between SiC and the matrix;

[0039] Furthermore, nano-modified silicon carbide has extremely high strength and hardness. When it is evenly distributed in the alumina matrix, it can effectively hinder the expansion of cracks and improve the bending strength and compressive strength of the material. This "bridging effect" and "pinning effect" can significantly improve the overall mechanical properties of the material.

[0040] At the same time, the interface bonding force between nano-modified silicon carbide and alumina matrix is ​​strong, which can form a strong interface structure, further improving the overall performance of the composite material. By controlling the sintering conditions, the good bonding between nano-modified silicon carbide and alumina is promoted, and the interface compatibility is enhanced;

[0041] The modification steps of nano-modified silicon carbide are:

[0042] S2.1, dispersing nano silicon carbide powder in ethanol solvent to obtain a 20wt% nano silicon carbide solution, adding γ-mercaptopropyltriethoxysilane to the nano silicon carbide solution, the mass ratio of γ-mercaptopropyltriethoxysilane to nano silicon carbide powder being 1:10;

[0043] S2.2, at room temperature, stirring at a speed of 680-800 rpm for 6-8 hours, and promoting the chemical reaction between γ-mercaptopropyltriethoxysilane and the hydroxyl groups on the surface of the nano-silicon carbide to form a stable chemical bond;

[0044] The mercapto group (-SH) and / or silanol group (-Si(OC2H5)3) in γ-mercaptopropyltriethoxysilane undergoes condensation or substitution reaction with the hydroxyl group (-OH) on the surface of SiC to form a stable silicon-oxygen bond (-Si iOS i-) or thiol bond, thereby achieving surface coating and modification of nano-silicon carbide;

[0045] S2.3, after the reaction is completed, remove the unreacted γ-mercaptopropyltriethoxysilane and other by-products by filtering;

[0046] S2.4. Dry the modified nano-silicon carbide powder at a suitable temperature to obtain the final product.

[0047] Example 1

[0048] A method for preparing ultra-low temperature sintered alumina ceramics is as follows:

[0049] S1.1, putting alumina powder and water in a ratio of 3:1 into a ball mill equipped with ball stones for ball milling for 20 hours to obtain alumina grinding slurry, the specific gravity of the alumina grinding slurry is 1.63, and the pH of the prepared alumina slurry is 9.4;

[0050] Alumina grinding slurry, alumina powder, polycarboxylate dispersant and polyacrylamide adhesive are mixed in a ratio of 200:160:35:3, the specific gravity after mixing is 1.82, and the alumina powder is a mixed powder with a mass ratio of 100-200:300-400 meshes and a mass ratio of 2:1;

[0051] S1.2, select B2O3-Li2O-Cr2O3-TiO2-SiO2 as the sintering aid system, and mix B2O3, Li2O, Cr2O3, TiO2 and SiO2 in a weight ratio of 3:1:0.5:1:1 by a mixer;

[0052] Introducing nano-modified silicon carbide into the mixed sintering aid system, wherein the nano-modified silicon carbide is obtained by surface-modifying nano-silicon carbide with γ-mercaptopropyltriethoxysilane, wherein the mixing mass ratio of the nano-modified silicon carbide to the sintering aid system is 1:100;

[0053] S1.3, heat 3wt% of cardan gum to dissolve it and add it to the prepared alumina slurry, stir it evenly and inject it into the alumina ceramic mold, place it in a curing room at 30°C, wait for the slurry to cool, and start demoulding;

[0054] The alumina embryos after demoulding are cured in the curing room for 12 hours, and then moved into a drying room at 80℃ for 10 hours;

[0055] S1.4. The baked alumina embryos are placed in a shuttle kiln and sintered at 138°C for 24 hours to form alumina ceramics.

[0056] Example 2

[0057] A method for preparing ultra-low temperature sintered alumina ceramics is as follows:

[0058] S1.1, putting alumina powder and water in a ratio of 3:1 into a ball mill equipped with ball stones for ball milling for 20 hours to obtain alumina grinding slurry, the specific gravity of the alumina grinding slurry is 1.63, and the pH of the prepared alumina slurry is 9.4;

[0059] Alumina grinding slurry, alumina powder, polycarboxylate dispersant and polyacrylamide adhesive are mixed in a ratio of 200:160:35:3, the specific gravity after mixing is 1.82, and the alumina powder is a mixed powder with a mass ratio of 100-200:300-400 meshes and a mass ratio of 2:1;

[0060] S1.2, select B2O3-Li2O-Cr2O3-TiO2-SiO2 as the sintering aid system, and mix B2O3, Li2O, Cr2O3, TiO2 and SiO2 in a weight ratio of 3:1:0.5:1:1 by a mixer;

[0061] Introducing nano-modified silicon carbide into the mixed sintering aid system, wherein the nano-modified silicon carbide is obtained by surface-modifying nano-silicon carbide with γ-mercaptopropyltriethoxysilane, wherein the mixing mass ratio of the nano-modified silicon carbide to the sintering aid system is 3:100;

[0062] S1.3, heat 3wt% of cardan gum to dissolve it and add it to the prepared alumina slurry, stir it evenly and inject it into the alumina ceramic mold, place it in a curing room at 30°C, wait for the slurry to cool, and start demoulding;

[0063] The alumina embryos after demoulding are cured in the curing room for 12 hours, and then moved into a drying room at 80℃ for 10 hours;

[0064] S1.4. The baked alumina embryos are placed in a shuttle kiln and sintered at 138°C for 24 hours to form alumina ceramics.

[0065] Example 3

[0066] A method for preparing ultra-low temperature sintered alumina ceramics is as follows:

[0067] S1.1, put alumina powder and water in a ratio of 3:1 into a ball mill equipped with ball stones for ball milling for 20 to 30 hours to obtain alumina grinding slurry, the specific gravity of the alumina grinding slurry is 1.68, and the pH of the prepared alumina slurry is 9.6;

[0068] Alumina grinding slurry, alumina powder, ammonium citrate dispersant and polyvinyl alcohol adhesive are mixed in a ratio of 200:130:40:3, and the specific gravity after mixing is 1.87, and the alumina powder is a mixed powder with a mass ratio of 100-200:300-400 mesh and a mass ratio of 2:1;

[0069] S1.2, select B2O3-Li2O-Cr2O3-TiO2-SiO2 as the sintering aid system, and mix B2O3, Li2O, Cr2O3, TiO2 and SiO2 in a weight ratio of 4:0.5:1:2:0.5 by a mixer;

[0070] Introducing nano-modified silicon carbide into the mixed sintering aid system, wherein the nano-modified silicon carbide is obtained by surface-modifying nano-silicon carbide with γ-mercaptopropyltriethoxysilane, wherein the mixing mass ratio of the nano-modified silicon carbide to the sintering aid system is 3:100;

[0071] S1.3, heat 3wt% of Curdlan gum to dissolve it and add it to the prepared alumina slurry, stir it evenly and inject it into the alumina ceramic mold, place it in a curing room at 25°C, wait for the slurry to cool, and start demoulding;

[0072] The alumina embryos after demoulding are cured in the curing room for 24 hours, and then moved into a drying room at 85°C for 12 hours;

[0073] S1.4. Place the baked alumina embryos in a shuttle kiln and sinter at 1400°C for 24 hours to form alumina ceramics.

[0074] Comparative Example 1

[0075] The method of Example 2 is adopted without introducing nano-modified silicon carbide into the mixed sintering aid system.

[0076] Comparative Example 1

[0077] Using the method of Example 2, the nano-silicon carbide in the mixed sintering aid system is not modified by γ-mercaptopropyltriethoxysilane.

[0078] For the preparation method of the ultra-low temperature sintered alumina ceramics prepared in the above Examples 1-3 and Comparative Examples 1-2, the performance test method of the preparation method of the ultra-low temperature sintered alumina ceramics is as follows:

[0079] Refer to GB / T 6569-2006 "Test Method for Bending Strength of Fine Ceramics" to specify the corresponding test equipment, specimens, test steps, result calculation and data processing methods. The three-point bending or four-point bending method is used on a material mechanics testing machine to determine the bending strength by measuring the maximum load of the specimen at bending failure.

[0080] Refer to B / T 4740-1999 "Test Method for Compressive Strength of Ceramic Materials" to stipulate the test equipment, sample preparation, test steps, result calculation and other aspects. Use the unconfined compression test method. Apply pressure at a certain speed on the pressure testing machine until the sample is destroyed, and record the maximum pressure value at the time of destruction.

[0081] The corresponding test methods and requirements are specified in GB / T 23806-2009 "Test Method for Fracture Toughness of Fine Ceramics - Single-Sided Pre-cracked Beam Method". The surface crack bending method is used to evaluate the fracture toughness of the material by measuring the crack propagation behavior of the specimen under external load.

[0082] Refer to GB / T 10700-2006 "Fine Ceramics Elastic Modulus Test Method Bending Method" to specify the corresponding test methods and requirements, and use the resonance method to determine the Young's modulus by measuring the natural frequency of the material;

[0083] Refer to GB / T 3810.9-2016 national standard on thermal shock resistance test of ceramic tiles, and test the thermal shock resistance of alumina ceramics according to the standards related to the thermal shock resistance test of ceramic tiles;

[0084] In summary, the mechanical properties of alumina ceramics are shown in Table 1:

[0085] Table 1 Mechanical properties data of alumina ceramics of Examples 1-3 and Comparative Example 1

[0086]

[0087] The above data fully show that Examples 1-3 are better than Comparative Examples 1-2, as follows:

[0088] It can be seen from Examples 1-3 that as the proportion of nano-modified silicon carbide introduced into the sintering system increases, the mechanical properties of alumina ceramics are significantly improved, especially the flexural strength, compressive strength, fracture toughness and Young's modulus of the ceramics.

[0089] Nano-modified silicon carbide has extremely high strength and hardness. When it is evenly distributed in the alumina matrix, it can effectively hinder the expansion of cracks and improve the bending strength and compressive strength of the material. This "bridging effect" and "pinning effect" can significantly improve the overall mechanical properties of the material.

[0090] Taking all factors into consideration, Example 2 is taken as the best example. By comparing Example 2 with Comparative Example 1, it can be seen that:

[0091] Without introducing nano-modified silicon carbide into the mixed sintering system, the mechanical properties of alumina ceramics, especially the flexural strength, compressive strength, fracture toughness and Young's modulus of the ceramics, were significantly reduced. It can be seen that nano-modified silicon carbide has a significant effect on improving the flexural strength, compressive strength and fracture toughness of alumina ceramics.

[0092] γ-Mercaptopropyltriethoxysilane is an organic compound containing a silane coupling agent. One end of γ-mercaptopropyltriethoxysilane contains a silane group that can react with the surface of an inorganic material (such as SiC), and the other end contains an organic functional group (thiol) that can react or be compatible with an organic matrix (such as a polymer); the silane group can react with the hydroxyl group on the surface of SiC to form a stable silicon-oxygen bond, so that the silane is firmly attached to the surface of SiC; the thiol group can react with the functional groups in certain polymer matrices, or at least be compatible with them, thereby improving the interfacial bonding strength between SiC and the matrix, reducing interfacial voids, increasing effective load transfer, and further improving the mechanical properties of the composite material. The modification effect of γ-mercaptopropyltriethoxysilane helps to control the dispersion of nanoparticles and reduce agglomeration, thereby optimizing the microstructure of the material and enhancing the toughness and overall stability of the material.

[0093] Further, by combining Example 2 with Comparative Example 1, it can be seen that:

[0094] When the nano-silicon carbide in the mixed sintering aid system is not modified by γ-mercaptopropyltriethoxysilane, and the nano-silicon carbide is directly mixed with the sintering aid system, the various mechanical properties data of the alumina ceramic, especially the ceramic flexural strength, ceramic compressive strength, ceramic fracture toughness and Young's modulus are significantly reduced, but the various mechanical properties data of the alumina ceramic in Example 2 are improved relative to Example 1. It can be seen that nano-silicon carbide has a significant effect on improving the flexural strength, compressive strength, ceramic fracture toughness and Young's modulus of alumina ceramics, and γ-mercaptopropyltriethoxysilane can significantly improve the flexural strength, compressive strength and fracture toughness of alumina ceramics.

[0095] In summary, the interfacial bonding force between nano-modified silicon carbide and alumina matrix is ​​strong, which can form a strong interfacial structure and further improve the overall performance of the composite material. By controlling the sintering conditions, the good bonding between nano-modified silicon carbide and alumina is promoted, and the interfacial compatibility is enhanced. The enhancement of the interfacial bonding force can effectively prevent the initiation and expansion of cracks at the interface between nano-modified silicon carbide particles and alumina matrix. Under the action of bending load, the stronger interface can more effectively transfer stress and avoid stress concentration, thereby improving the bending strength of the composite material. As a reinforcing phase, nano-modified silicon carbide has high strength and hardness, which can significantly improve the ability of the composite material to resist compressive loads. Good interfacial bonding ensures that there is no detachment from the reinforcing phase when subjected to high pressure, maintaining the overall stability and strength of the material and improving the compressive strength.

[0096] At the same time, the addition of nano-modified silicon carbide and interface optimization help change the crack propagation path. When microcracks exist in the material, the strong interface can cause the cracks to deflect or bypass the reinforcing particles, increase the resistance to crack propagation, and absorb more energy, which directly leads to the improvement of the fracture toughness of the material. In addition, the bridging effect and crack pinning effect of nanoparticles are also important mechanisms for improving fracture toughness.

[0097] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing ultra-low temperature sintered alumina ceramics, characterized in that: The following steps are involved: S1.1, put alumina powder and water in a ratio of 3 to 4:1 into a ball mill equipped with ball stones for 20 to 30 hours to obtain alumina grinding slurry, the specific gravity of the alumina grinding slurry is 1.60 to 1.70; The alumina grinding slurry, alumina powder, dispersant and adhesive are mixed evenly in a ratio of 200:100-180:30-50:2-5, and the specific gravity after mixing is 1.80-1.90; S1.2, select B2O3-Li2O-Cr2O3-TiO2-SiO2 as the sintering aid system, and mix B2O3, Li2O, Cr2O3, TiO2 and SiO2 in a weight ratio of 3-4: 0.5-1: 0.5-1: 1-2: 0.5-1 by a mixer; Introducing nano-modified silicon carbide into the mixed sintering aid system, wherein the mixing mass ratio of the nano-modified silicon carbide to the sintering aid system is 1 to 3:100; S1.3, heat 2-3wt% of cardan gum to dissolve it and add it to the prepared alumina slurry, stir it evenly and inject it into the alumina ceramic mold, place it in a curing room at 20-30℃, wait for the slurry to cool, and start demoulding; The alumina embryos after demoulding are cured in the curing room for 12-24 hours, and then moved into a drying room at 80-85℃ for 10-16 hours; S1.

4. Place the baked alumina embryo in a sintering kiln at 1350°C-1400°C for 24-28 hours to form alumina ceramics.

2. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 1, characterized in that: In the S1.1, the alumina powder is a mixed powder of 100-200:300-400 meshes with a mass ratio of 2:

1.

3. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 1, characterized in that: In the above S1.1, the dispersant is one or a mixture of more than one of ammonium citrate, polycarboxylate and polyacrylate.

4. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 1, characterized in that: In S1.1, the adhesive is a mixture of one or more of polyvinyl alcohol, polyacrylamide and polyethylene glycol.

5. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 1, characterized in that: In the above S1.1, the pH of the prepared alumina slurry is 9-10.

6. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 1, characterized in that: In S1.2, the nano-modified silicon carbide is obtained by surface-modifying nano-silicon carbide with γ-mercaptopropyltriethoxysilane; The specific modification steps are: S2.1, dispersing nano silicon carbide powder in ethanol solvent to obtain a 20wt% nano silicon carbide solution, and adding γ-mercaptopropyltriethoxysilane to the nano silicon carbide solution; S2.2, at room temperature, stirring with a stirrer to promote a chemical reaction between γ-mercaptopropyltriethoxysilane and hydroxyl groups on the surface of nano-silicon carbide; S2.3, after the reaction is completed, remove the unreacted γ-mercaptopropyltriethoxysilane and other by-products by filtering; S2.

4. Dry the modified nano-silicon carbide powder at a suitable temperature to obtain the final product.

7. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 6, characterized in that: In the S2.1, the mass ratio of γ-mercaptopropyltriethoxysilane to nano-silicon carbide powder is 1:

10.

8. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 6, characterized in that: In S2.2, the stirrer continues stirring at a speed of 680-800 rpm for 6-8 hours.

9. The method for preparing ultra-low temperature sintered alumina ceramics according to claim 1, characterized in that: In S1.4, the sintering kiln is a shuttle kiln.

Citation Information

Patent Citations

  • Formula for reducing ceramic sintering temperature

    CN113582670A

  • Silicon carbide whisker reinforced alumina ceramic composites

    US5108963A

Cited By

  • Nanometer composite mineral cable insulation layer and preparation method thereof