Ceramic material for dielectric filter, preparation method of ceramic material, dielectric filter and communication antenna

By adjusting the comparison value and particle size of the crystal phase and glass in the ceramic material, combined with the addition of Nd2O3, the dielectric performance of the ceramic filter is optimized, and the problem of limited performance of traditional ceramic filters in the high frequency band is solved, achieving lower losses and Ceramic materials with higher dielectric constant meet the performance requirements of 5G and 6G.

CN118955119APending Publication Date: 2024-11-15DONGGUAN SUNLORD HONGDIAN ELECTRONICS CO LTD

Patent Information

Application Number
CN202411030621.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional ceramic filters are limited in high frequency bands (such as above 6GHz), increased insertion loss, decreased out-of-band suppression capability, and greater technical challenges in improving the Q value of ceramic filters, requiring lower loss ceramic materials to achieve better signal selectivity and lower noise levels.

Method used

By adjusting the ratio and particle size of the crystal phase and glass phase in the MgTiO3 and CaTiO3 ceramic systems, a ceramic material with a dielectric constant of 25.2-56.7 was prepared. Combined with the addition of Nd2O3 powder, the dielectric properties and mechanical strength of the ceramic are optimized. Fine preparation methods such as ball milling, prefixing, granulation, dry pressing and sintering steps ensure high purity and uniformity of ceramic materials.

Benefits of technology

It realizes stable dielectric filter performance over a wider frequency range, improves mechanical strength and chemical stability, extends service life, and meets the performance requirements of 5G and 6G filters for ceramic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955119A_ABST
    Figure CN118955119A_ABST
Patent Text Reader

Abstract

The invention discloses a ceramic material for a dielectric filter, a preparation method of the ceramic material, the dielectric filter and a communication antenna, the ceramic material is a ceramic body formed by sintering a ceramic system containing MgTiO3 and CaTiO3, a crystal phase in the ceramic body is composed of MgCaTiO3 crystal grains, and the average size of the crystal grains in the crystal phase is 0.35-8.7 [mu] m; in the ceramic body, the volume ratio of the crystal phase to the glass phase is 10: (1.2-1.8), and the dielectric constant of the ceramic body is 25.2-56.7. By adjusting the crystal size and the ratio of the glass phase to the crystal phase, the dielectric constant and the quality factor of the ceramic material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dielectric filter materials and manufacturing, and in particular to a ceramic material for a dielectric filter and a preparation method thereof, a dielectric filter, and a communication antenna. Background Art

[0002] A filter is a frequency-selective device that allows specific frequency components in a signal to pass through while greatly attenuating other frequency components. With the rapid development of wireless communication systems, filters are required to have the characteristics of low insertion loss, high suppression, high power handling, low cost, and miniaturization. Among them, the filter body is made of ceramic dielectric materials with high dielectric constants, and silver is plated on the surface of the dielectric block to play an electromagnetic shielding role. The miniaturized dielectric filter achieved in this way is now widely used in various RF modules because its size and weight are lower than traditional metal waveguide filters.

[0003] As 5G commercialization gradually matures, the pre-research of 6G has become an important direction for major equipment manufacturers. 6G applications have higher frequencies, larger bandwidths, and smaller sizes. They also require filters with higher Q values ​​to achieve better signal selectivity and lower noise levels. The performance of traditional ceramic filters in high frequency bands (such as above 6GHz) may be limited, including increased insertion loss, decreased out-of-band suppression capabilities, etc., and improving the Q value of ceramic filters faces great technical challenges. Therefore, lower-loss ceramic materials are needed to reduce signal attenuation, but at the same time maintain a high dielectric constant to achieve miniaturized design. Summary of the invention

[0004] In order to overcome the deficiencies of the prior art, the purpose of the present application is to provide a ceramic material for dielectric filters, which improves the dielectric constant and quality factor of the ceramic material by adjusting the crystal size and the ratio of the glass phase to the crystal phase, while reducing the dielectric loss.

[0005] To solve the above problems, the technical solutions adopted in this application are as follows:

[0006] An embodiment of the present application provides a ceramic material for a dielectric filter, which is a ceramic body sintered from a ceramic system comprising MgTiO3 and CaTiO3, wherein the crystal phase in the ceramic body is composed of MgCaTiO3 grains, and the average grain size in the crystal phase is 0.35-8.7 μm; in the ceramic body, the volume ratio of the crystal phase to the glass phase is 10:(1.2-1.8), and the dielectric constant of the ceramic body is 25.2-56.7.

[0007] As a further preferred solution, in the ceramic system described in the embodiments of the present application, the mass ratio of MgTiO3 to CaTiO3 is 100:(5-12).

[0008] As a further preferred solution, the particle size of MgTiO3 described in the embodiment of the present application is 0.8-10 μm, and the purity is greater than or equal to 95%; the particle size of CaTiO3 is 0.8-2.0 μm, and the purity is greater than or equal to 95%.

[0009] As a further preferred solution, the ceramic system described in the embodiment of the present application further includes Nd2O3 powder, and the added amount of Nd2O3 powder accounts for 2-5% of the weight of MgTiO3.

[0010] As a further preferred solution, the particle size of the Nd2O3 powder described in the embodiment of the present application is 100-500nm.

[0011] The present application also provides a method for preparing the ceramic material for the dielectric filter as described in the application, comprising:

[0012] Synthesizing the main crystal phase MgTiO3: selecting basic magnesium carbonate, titanium dioxide and zinc oxide with a purity greater than or equal to 95% as raw materials, respectively ball-milling them in a ball mill to a predetermined particle size; drying the ball-milled basic magnesium carbonate, titanium dioxide and zinc oxide powders and pre-calcining them to obtain a MgTiO3 pre-calcined frit;

[0013] Synthesizing subcrystalline CaTiO3: Calcium carbonate and titanium dioxide with a purity greater than or equal to 95% are respectively ball-milled in a ball mill to a predetermined particle size, and the ball-milled calcium oxide and titanium dioxide powders are dried and pre-calcined to obtain a CaTiO3 pre-calcined frit;

[0014] Granulation: The MgTiO3 pre-sintered frit and the CaTiO3 pre-sintered frit are mixed and put into a ball mill for ball milling to a predetermined particle size, and a granulation binder is added and then spray granulation is performed to obtain mixed particles;

[0015] Dry pressing: the mixed particles are placed into a metal mold cavity and dry pressed to form a ceramic body;

[0016] Sintering: The ceramic body is placed in a sintering furnace to form a ceramic body.

[0017] As a further preferred scheme, in the preparation method described in the embodiment of the present application, in the step of synthesizing the main crystalline phase MgTiO3, ZrO2 round balls with a particle size of 2-5 mm are used for ball milling for 6.5-8.5 hours; the pre-sintering temperature is 1210℃-1250℃, and the pre-sintering time is 6-8 hours.

[0018] As a further preferred scheme, in the preparation method described in the embodiment of the present application, the step of synthesizing the secondary crystalline phase CaTiO3 is to use ZrO2 round balls with a particle size of 2-5 mm for ball milling for 6-8 hours, the pre-sintering temperature is 1250℃-1280℃, and the pre-sintering time is 8-10 hours.

[0019] As a further preferred scheme, in the preparation method described in the embodiment of the present application, in the granulation step, Nd2O3 powder is added to the mixture obtained by mixing the MgTiO3 pre-sintered melt and the CaTiO3 pre-sintered melt, and then ball milling is performed.

[0020] As a further preferred solution, in the preparation method described in the embodiment of the present application, in the dry pressing step, a servo press is used for double-sided pressing, the pressure on each side is 120-180 MPa, and the holding time is 3-8 s; the ceramic green body density tolerance is controlled within ±0.02 g / cm 3 .

[0021] As a further preferred solution, in the preparation method described in the embodiment of the present application, the sintering process, the sintering temperature is set to 1420-1450°C; the sintering step includes

[0022] Heating stage: adopt staged heating, low temperature zone, from room temperature to 350℃ at 2-5℃ / min; medium temperature zone, adjust the heating rate to 6-10℃ / min from 350℃ to 900℃; high temperature zone, start heating from 900℃ at 10-15℃ / min, when the temperature reaches 1300℃, adjust the heating rate to 10-20℃ / min and directly heat to sintering temperature;

[0023] Insulation stage: When the green body is heated to the sintering temperature, it is kept at this temperature for 30-50 minutes, and then the temperature is reduced to 1330-1380℃ and kept for 20-40 minutes;

[0024] Cooling stage: After the insulation is completed, the temperature is lowered to 300℃ at a cooling rate of 20-25℃ / min, and then begins to cool naturally to room temperature.

[0025] The embodiment of the present application also provides a dielectric filter, including a ceramic dielectric body, a PCB board and a copper needle. The dielectric body is made of the ceramic material for the dielectric filter described in the embodiment of the present application; the front of the ceramic dielectric body is provided with a debugging blind hole, a coupling blind hole, an output port and an input port, the PCB board is welded to the back of the ceramic body, the copper needle is welded to the output port and the input port, and the upper end of the copper needle is flush with the surface of the PCB board.

[0026] The embodiment of the present application also provides a communication antenna, comprising the dielectric filter described in the embodiment of the present application.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. The ceramic material for dielectric filter described in the present application, the crystal phase in the ceramic body is composed of MgCaTiO3 grains, the average size of these grains is between 0.35-8.7μm, and the fine crystal phase structure helps to improve the dielectric properties and frequency response characteristics of the material, so that the dielectric filter can maintain stable performance in a wider frequency range.

[0029] 2. By controlling the volume ratio of the crystal phase to the glass phase in the ceramic material for the dielectric filter described in the present application, the mechanical strength, thermal stability and chemical stability of the material can be effectively improved, thereby extending the service life of the dielectric filter.

[0030] 3. The ceramic material for dielectric filter described in this application can effectively adjust the dielectric constant of the ceramic material by regulating the grain size and adjusting the ratio of the crystal phase to the glass phase, so that the dielectric constant meets the performance requirements of 5G and 6G filters for ceramic materials.

[0031] 4. The preparation method of the ceramic material for dielectric filter described in this application ensures the high purity, uniformity and excellent performance of the ceramic material through careful raw material selection, ball milling, pre-sintering, granulation, molding and sintering steps, providing a high-quality ceramic material foundation for the application of dielectric filters.

[0032] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0034] Figure 1 This is a SEM image of the ceramic material for the dielectric filter described in Example 1 of the present application.

[0035] Figure 2 This is a frequency response curve of the dielectric filter described in the embodiment of the present application. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0037] The term "comprising" and other equivalent descriptions involved in the specification and claims of this application are intended to cover non-exclusive inclusions, including both the contents clearly described in the specification and claims, and the steps or units that are not described in the specification and claims but are inherent in the product, method or structure.

[0038] The embodiment of the present application provides a ceramic material for dielectric filter, which is a ceramic body sintered from a ceramic system including MgTiO3 and CaTiO3, wherein the crystal phase in the ceramic body is composed of MgCaTiO3 grains. In the present application, the dielectric constant of the ceramic material will change with the change of the grain size. When the grain size is within a certain range, the small-grain ceramic has a higher density, which can reduce the adverse effects of defects such as pores on dielectric properties, so that the dielectric constant increases with the decrease of the grain size. However, when the grain size is reduced to a certain extent, the number of grain boundaries increases sharply, and the effects such as space charge polarization at the grain boundaries will have a negative impact on the dielectric constant, resulting in the dielectric constant no longer increasing or even possibly decreasing. At the same time, the change in grain size will affect the properties such as the density, porosity and grain boundary characteristics of the ceramic material, thereby affecting the quality factor. Smaller grain size helps to reduce defects such as pores, improve the density of ceramic materials, thereby reducing dielectric loss and improving the quality factor. Too small grain size may cause the grain boundary resistivity to decrease, increase leakage current and dielectric loss, and reduce the quality factor instead. Therefore, in the test of the present application, the average grain size in the crystal phase is controlled to be 0.35-8.7 μm, and the average grain size in the preferred crystal phase is 0.85-4.5 μm. In the embodiments of the present application, the dielectric constant of MgCaTiO3 ceramics is mainly determined by its crystal phase, because the ions in the crystal phase are arranged in an orderly manner and can form a stable dipole moment, thereby making a major contribution to the dielectric constant; when the volume ratio of the crystal phase increases, it means that the number of ions arranged in an orderly manner in the ceramic increases, and more orderly ion arrangements can form a stronger dipole moment, enhancing the polarization ability of the material, thereby improving the dielectric constant. However, the presence of the glass phase may indirectly affect the dielectric constant by affecting factors such as the density and porosity of the ceramic. When the volume ratio of the glass phase increases, the density of the ceramic will decrease, and the porosity will increase, resulting in a decrease in the dielectric constant. Therefore, in the embodiment of the present application, in the ceramic body, the volume ratio of the crystal phase to the glass phase is controlled to be 10:(1.2-1.8), and preferably, the volume ratio of the crystal phase to the glass phase is controlled to be 10:(1.2-1.5). In the embodiment of the present application, by adjusting the average grain size of the ceramic body and the volume ratio of the crystal phase to the glass phase, the dielectric constant of the obtained ceramic material is 25.2-56.7, which can meet the material requirements of the 6G filter and can produce a ceramic filter with higher performance. Preferably, the dielectric constant of the ceramic material is 32.5-50.2.

[0039] MgTiO3 itself has a lower dielectric constant, while CaTiO3 has a higher dielectric constant. Adding CaTiO3 to the MgTiO3 system can significantly improve the dielectric constant of the system, and can change the crystal structure and microstructure of the system, thereby increasing the polarization ability of the material. With the increase of the CaTiO3 doping amount, the volume density, dielectric constant and resonant frequency temperature coefficient of the ceramic will continue to increase; however, when the doping amount of CaTiO3 reaches a certain level, the growth of the dielectric constant will tend to saturate or even decrease. At the same time, since MgTiO3 has a lower dielectric loss, its Q value is relatively high. Although the addition of CaTiO3 can improve the dielectric constant of the system, the addition of CaTiO3 will also introduce more defects and impurities; so too high a CaTiO3 content will cause the quality factor of the system to decrease. Therefore, in some embodiments of the present application, in order to obtain a ceramic material whose dielectric constant, quality factor and loss can meet the application requirements, the mass ratio of MgTiO3 and CaTiO3 is 100: (5-12). In a preferred embodiment, the mass ratio of MgTiO3 to CaTiO3 is 100:(6-10).

[0040] In the study of this application, it was found that the size of MgTiO3 particles and CaTiO3 particles will affect the performance of ceramic materials to a certain extent. Nanoparticles have a larger specific surface area, which increases the contact area between particles, which is conducive to the action of polarization mechanism. As the particle size decreases, the dielectric constant of ceramic materials shows an increasing trend. However, when the particle size is too small, the dielectric constant will decrease due to surface effect and quantum size effect. In addition, the uniform distribution of nanoparticles and the higher sintering density help to reduce defects and pores inside the material, thereby reducing energy loss and improving the quality factor. As the particle size decreases, the quality factor will also increase; however, when the particle size is too small, the quality factor may decrease due to increased surface roughness and enhanced interaction between particles. Therefore, in order to ensure that the ceramic material has excellent performance, as a further preferred solution, in some embodiments of the present application, the MgTiO3 particle size is 0.8-10μm, preferably, the MgTiO3 particle size is 0.8-2.0μm; the CaTiO3 particle size is 0.8-2.0μm, preferably, the CaTiO3 particle size is 0.8-1.2μm. The improvement of purity helps to reduce impurities and defects in the material, thereby reducing dielectric loss and improving dielectric constant. Therefore, in the embodiment of the present application, the purity of MgTiO3 is greater than or equal to 95%; the purity of CaTiO3 is greater than or equal to 95%.

[0041] As additives, rare earth oxides can affect the microstructure and dielectric properties of ceramics by replacing some ions or forming solid solutions. The ceramic system described in the embodiments of the present application adds Nd2O3 powder. As a donor impurity, Nd2O3 can introduce additional free electrons or holes. These carriers will increase the polarization ability of the material, trigger the phase change of MgCaTiO3 ceramics or change its microstructure, such as grain size, density, etc.; changes in these factors will lead to changes in the dielectric constant. In addition, adding an appropriate amount of Nd2O3 can reduce dielectric loss by improving the microstructure of the ceramic (such as reducing pores, defects, etc.), thereby increasing the Q value. Therefore, in some embodiments of the present application, the amount of Nd2O3 powder added accounts for 2-5% of the weight of MgTiO3. The smaller Nd2O3 powder particle size has a larger specific surface area, which increases the contact area between the powder particles, helps the material transfer and reaction rate during the sintering process, and can play a role in reducing the sintering temperature of the ceramic; and the small particle size powder can be more evenly filled in the ceramic matrix, reducing the formation of pores and defects, and improving the density of the sintered body. In addition, the smaller Nd2O3 powder particle size helps to refine the ceramic grains, and the grain refinement can better disperse and resist the expansion of cracks, and improve the strength and toughness of the ceramic. Therefore, in the embodiment of the present application, the particle size of the Nd2O3 powder is 100-500nm. Preferably, the particle size of the Nd2O3 powder is 120-200nm.

[0042] The present application also provides a method for preparing the ceramic material for the dielectric filter as described in the application, comprising:

[0043] Synthesizing the main crystal phase MgTiO3: selecting basic magnesium carbonate, titanium dioxide and zinc oxide with a purity greater than or equal to 95% as raw materials, respectively ball-milling them in a ball mill to a predetermined particle size; drying the ball-milled basic magnesium carbonate, titanium dioxide and zinc oxide powders and pre-calcining them to obtain a MgTiO3 pre-calcined frit;

[0044] Synthesizing subcrystalline CaTiO3: Calcium carbonate and titanium dioxide with a purity greater than or equal to 95% are respectively ball-milled in a ball mill to a predetermined particle size, and the ball-milled calcium oxide and titanium dioxide powders are dried and pre-calcined to obtain a CaTiO3 pre-calcined frit;

[0045] Granulation: The MgTiO3 pre-sintered frit and the CaTiO3 pre-sintered frit are mixed and put into a ball mill for ball milling to a predetermined particle size, and a granulation binder is added and then spray granulation is performed to obtain mixed particles;

[0046] Dry pressing: the mixed particles are placed into a metal mold cavity and dry pressed to form a ceramic body;

[0047] Sintering: The ceramic body is placed in a sintering furnace to form a ceramic body.

[0048] Ball milling media plays a key role in crushing and mixing raw materials during the ball milling process. Its material, size, filling rate and other factors will affect the ball milling effect, and then affect the performance of ceramics. Ball milling media with smaller diameters can better penetrate into the particle pile, so that the particles can be more fully contacted and ground, thereby obtaining finer powders. Since the ball milling process is the collision and friction between the grinding balls and the particles that break the particles, as the ball milling time increases, the raw material particles gradually refine and the particle size becomes smaller; however, too long ball milling time may cause excessive particle refinement and agglomeration, which increases the particle size. In addition, appropriate ball milling time can obtain powders with uniform particle size distribution and large specific surface area. These powders are easier to densify during the sintering process, thereby improving the sintering density and mechanical properties of ceramics; appropriate ball milling time also helps to improve the dielectric constant and quality factor (Q value) of ceramics. In the preparation method described in the embodiment of the present application, in the step of synthesizing the main crystalline phase MgTiO3, ZrO2 round balls with a particle size of 2-5mm are used for ball milling for 6.5-8.5h. The temperature of the pre-sintering treatment is 1210℃-1250℃, and the pre-sintering time is 6-8h. When synthesizing the main crystal phase, basic magnesium carbonate and titanium dioxide are used as raw materials, and a small amount of zinc oxide is added as a dopant to introduce into the MgTiO3 system, and the dielectric properties and microwave properties of MgTiO3 are adjusted and optimized by changing the crystal structure or electronic structure of the material. The amount of zinc oxide added is 2-5wt% of the total amount of the reactants.

[0049] Similarly, in the process of synthesizing subcrystalline CaTiO3 and preparing MgCaTiO3 ceramics, it is also necessary to comprehensively consider the effects of the size of the ball milling medium and the ball milling time on the performance of the ceramic. As a further preferred scheme, in the preparation method described in the embodiment of the present application, the step of synthesizing subcrystalline CaTiO3 is to use ZrO2 round balls with a particle size of 2-5mm for 6-8h. The level of the pre-firing temperature will directly affect the phase change process of CaTiO3. The appropriate pre-firing temperature helps CaTiO3 to form a stable phase structure and reduce the generation of impurities; the appropriate pre-firing temperature also improves the sintering activity of the powder, promotes the growth and densification of grains during the sintering process, thereby improving the sintering performance of MgCaTiO3 ceramics. However, too high a pre-firing temperature may cause the powder particles to grow excessively, which in turn reduces the sintering activity. Therefore, in the present application, the temperature of the pre-firing treatment for synthesizing the subcrystalline CaTiO3 is set to 1250℃-1280℃. The length of the pre-burning time determines the extent of the reaction. Sufficient pre-burning time can ensure that CaTiO3 forms a stable phase structure, and makes the reaction more sufficient and reduces residues; for the MgCaTiO3 system, the extension of the pre-burning time helps the reaction between CaTiO3 and MgTiO3 or other components to be more thorough, thereby optimizing the composition and structure of the ceramic, improving the uniformity and sintering activity of the powder, and helping to form a uniform and dense ceramic body during the sintering process, reducing the adverse effects of pores and defects on dielectric properties. However, too long a pre-burning time can cause the growth and agglomeration of powder particles, which is not conducive to the improvement of the sintering effect. Therefore, in the present application, the pre-burning time of CaTiO3 powder is 8-10h.

[0050] As a further preferred scheme, in the preparation method described in the embodiment of the present application, in the granulation step, Nd2O3 powder is added to the mixture obtained by mixing the MgTiO3 pre-sintered melt and the CaTiO3 pre-sintered melt, and then ball milling is performed.

[0051] As a further preferred solution, in the preparation method described in the embodiment of the present application, preferably, a servo press is used for double-sided pressing. During double-sided pressing, both ends of the green body are subjected to pressure at the same time, so that the pressure can be more evenly transmitted to each part of the green body. Compared with single-sided pressing, double-sided pressing effectively reduces the pressure gradient, avoiding the situation where the pressure on the directly pressed end is too large and the pressure on other parts is insufficient; due to the uniform distribution of pressure, the particles inside the green body can be more evenly rearranged and deformed, reducing the stratification phenomenon caused by uneven pressure, which is crucial to improving the overall performance of ceramic products. In addition, double-sided pressing gives the green body a higher initial density, which helps to reduce the formation of pores and defects during the sintering process, promotes the growth and densification of grains, and not only enables the ceramic material to have better mechanical and electrical properties, but also helps to improve the overall performance stability and reliability of ceramic products. During the pressing process, as the pressure increases, the gap between the green body particles decreases, the green body density increases, and the high-density green body is easier to form a dense ceramic body during the sintering process, thereby improving the mechanical and electrical properties of the ceramic. In addition, as the pressing pressure increases, the density of the ceramic increases, and the dielectric constant will also increase accordingly; however, too high a pressure may cause defects inside the ceramic, which in turn reduces the dielectric constant. Appropriate pressure can also reduce the pores and defects inside the ceramic and reduce dielectric loss. Therefore, by reasonably controlling the pressing pressure, the performance of the density, microstructure, mechanical properties and dielectric properties of the ceramic can be optimized. In the embodiment of the present application, when double-sided pressing is performed, the two sides are pressed successively, and the front side is pressed first and then the back side is pressed, and the pressure is 120-180MPa; preferably, the pressure is 150-180MPa. In the embodiment of the present application, the holding time has an important influence on the performance of MgCaTiO3 ceramics. The appropriate holding time can ensure that the gas in the green body is fully discharged, reduce pores and defects, and thus improve the density and density of the ceramic; if the holding time is too short, the gas may not be completely discharged, resulting in bubbles and pores in the green body, affecting the density of the ceramic after sintering. During the holding stage, the pressure continues to be transmitted to all parts of the green body. Sufficient holding time can ensure that the pressure is fully transmitted to all areas of the green body, making the overall density of the green body more uniform. The mechanical properties of the ceramic material, such as compressive strength, flexural strength and fracture toughness, can be improved due to the optimization of the holding time. In addition, the appropriate holding time optimizes the dielectric properties of the ceramic by reducing pores and defects and increasing density. The dielectric constant may increase due to the increase in density, while the dielectric loss will decrease due to the reduction in defects. Therefore, the density, density, microstructure, mechanical properties and dielectric properties of the ceramic can be optimized by reasonably controlling the holding time. In some embodiments, the holding time is 3-8s. The density tolerance of the ceramic green body is controlled at ±0.02g / cm 3 .

[0052] As a further preferred solution, in the preparation method described in the embodiment of the present application, the sintering process, the sintering temperature is set to 1420-1450°C; the sintering step includes

[0053] Heating stage: adopt staged heating, low temperature zone, from room temperature to 350℃ at 2-5℃ / min, this stage is mainly slow heating to avoid cracking caused by thermal stress in the green body due to excessive temperature difference, at the same time, the low temperature zone also helps to gradually discharge volatile substances such as organic matter and moisture in the green body. In the medium temperature zone, adjust the heating rate to 6-10℃ / min from 350℃ to 900℃; in this stage, the green body begins to undergo a series of physical and chemical changes, such as the initial formation and growth of grains, and the gradual elimination of pores. A faster heating rate helps to promote these processes. In the high temperature zone, the temperature is raised from 900℃ at 10-15℃ / min. When the temperature reaches 1300℃, adjust the heating rate to 10-20℃ / min and directly heat to the sintering temperature; the high temperature zone is the key stage for green body densification and grain growth. A faster heating rate helps the green body quickly reach the sintering temperature, thereby shortening the sintering time and reducing energy consumption.

[0054] Insulation stage: When the green body is heated to the sintering temperature, it is kept at this temperature for 30-50 minutes. The main function of this stage is to fully densify the green body, further grow the grains, reduce the porosity, and thus improve the mechanical strength and hardness of the ceramic; then the temperature is reduced to 1330-1380℃ and kept for 20-40 minutes; the cooling and insulation at this stage helps to eliminate the residual stress in the green body and reduce the possibility of cracks in the ceramic during the cooling process.

[0055] Cooling stage: After the heat preservation is completed, the temperature is lowered to 300℃ at a cooling rate of 20-25℃ / min, and then naturally cooled to room temperature. Rapid cooling helps to reduce the exposure time of ceramics at high temperatures, thereby reducing the risk of abnormal grain growth; at the same time, the natural cooling stage can further eliminate the residual stress in the ceramics, making them more stable.

[0056] The embodiment of the present application also provides a dielectric filter, including a ceramic dielectric body, a PCB board and a copper needle. The dielectric body is made of the ceramic material for the dielectric filter described in the embodiment of the present application; the front of the ceramic dielectric body is provided with a debugging blind hole, a coupling blind hole, an output port and an input port, the PCB board is welded to the back of the ceramic body, the copper needle is welded to the output port and the input port, and the upper end of the copper needle is flush with the surface of the PCB board.

[0057] The embodiment of the present application also provides a communication antenna, comprising the dielectric filter described in the embodiment of the present application.

[0058] Example 1

[0059] See also Figure 1 This embodiment provides a ceramic material for a dielectric filter, which is a ceramic body sintered from a ceramic system containing MgTiO3 and CaTiO3. The crystal phase in the ceramic body is composed of MgCaTiO3 grains, and the average grain size in the crystal phase is 0.35 μm. In the ceramic body, the volume ratio of the crystal phase to the glass phase is 10:1.216, and the dielectric constant of the ceramic body is 56.7.

[0060] The ceramic material for the dielectric filter is prepared by the following method:

[0061] Synthesis of main crystal phase MgTiO3: Selecting 95% pure basic magnesium carbonate, titanium dioxide and zinc oxide as raw materials, respectively, using 2mm particle size ZrO2 round balls in a ball mill for 6.5 hours; drying the ball-milled basic magnesium carbonate, titanium dioxide and zinc oxide powders and pre-calcining them at a temperature of 1210°C for 8 hours to obtain MgTiO3 pre-calcined melt;

[0062] Synthesis of subcrystalline CaTiO3: Calcium oxide and titanium dioxide with a purity of 95% were ball-milled for 8 hours using ZrO2 balls with a particle size of 2 mm in a ball mill, and the ball-milled calcium oxide and titanium dioxide powders were dried and pre-calcined at a temperature of 1250°C for 10 hours to obtain a CaTiO3 pre-calcined melt;

[0063] Granulation: The MgTiO3 pre-sintered frit and the CaTiO3 pre-sintered frit are mixed in a mass ratio of 100:12, and then put into a ball mill and milled with 2 mm diameter ZrO2 balls to a particle size of 0.8 μm. After adding a granulation binder, spray granulation is performed to obtain mixed particles;

[0064] Dry pressing: the mixed particles are loaded into a metal mold cavity and pressed on both sides with a pressure of 120 MPa on each side and a holding time of 8 seconds to form a ceramic body;

[0065] Sintering: Place the ceramic body in a sintering furnace and sinter it in a step-by-step heating process. The sintering steps are as follows:

[0066] Heating stage: adopt staged heating, low temperature zone, from room temperature to 350℃ at 2℃ / min; medium temperature zone, adjust the heating rate to 8℃ / min from 350℃ to 900℃; high temperature zone, start heating from 900℃ at 10℃ / min, when the temperature reaches 1300℃, adjust the heating rate to 15℃ / min and directly heat to sintering temperature;

[0067] Insulation stage: When the green body is heated to the sintering temperature, it is kept at this temperature for 30 minutes, then the temperature is reduced to 1330℃ and kept for 40 minutes;

[0068] Cooling stage: After the insulation is completed, the temperature is lowered to 300°C at a cooling rate of 20°C / min, and then naturally cooled to room temperature.

[0069] Example 2

[0070] This embodiment provides a ceramic material for a dielectric filter, which is a ceramic body sintered from a ceramic system containing MgTiO3 and CaTiO3. The crystal phase in the ceramic body is composed of MgCaTiO3 grains, and the average grain size of the crystal phase is 4.6 μm. In the ceramic body, the volume ratio of the crystal phase to the glass phase is 10:1.617, and the dielectric constant of the ceramic body is 41.7.

[0071] The ceramic material for the dielectric filter is prepared by the following method:

[0072] Synthesis of main crystal phase MgTiO3: Selecting 95% pure basic magnesium carbonate, titanium dioxide and zinc oxide as raw materials, respectively, and ball milling them in a ball mill using 3mm particle size ZrO2 balls for 7 hours; drying the ball-milled basic magnesium carbonate, titanium dioxide and zinc oxide powders and pre-calcining them at a temperature of 1230°C for 6 hours to obtain MgTiO3 pre-calcined melt;

[0073] Synthesis of subcrystalline CaTiO3: Calcium oxide and titanium dioxide with a purity of 95% were ball-milled for 6 hours using 3 mm ZrO2 round balls in a ball mill, and the ball-milled calcium oxide and titanium dioxide powders were dried and pre-sintered at a temperature of 1260°C for 8 hours to obtain a CaTiO3 pre-sintered melt;

[0074] Granulation: The MgTiO3 pre-sintered frit and the CaTiO3 pre-sintered frit are mixed in a mass ratio of 100:8, and then put into a ball mill and milled with 3 mm diameter ZrO2 balls to a particle size of 1.2 μm. After adding a granulation binder, spray granulation is performed to obtain mixed particles;

[0075] Dry pressing: the mixed particles are placed into a metal mold cavity and pressed on both sides with a pressure of 150 MPa on each side and a holding time of 5 seconds to form a ceramic body;

[0076] Sintering: Place the ceramic body in a sintering furnace and sinter it in a step-by-step heating process. The sintering steps are as follows:

[0077] Heating stage: adopt staged heating, low temperature zone, from room temperature to 350℃ at 3℃ / min; medium temperature zone, adjust the heating rate to 6℃ / min from 350℃ to 900℃; high temperature zone, start heating from 900℃ at 12℃ / min, when the temperature reaches 1300℃, adjust the heating rate to 18℃ / min and directly heat to sintering temperature;

[0078] Insulation stage: When the green body is heated to the sintering temperature, it is kept at this temperature for 45 minutes, then the temperature is lowered to 1350℃ and kept for 30 minutes;

[0079] Cooling stage: After the insulation is completed, the temperature is lowered to 300°C at a cooling rate of 22°C / min, and then begins to cool naturally to room temperature.

[0080] Example 3

[0081] This embodiment provides a ceramic material for a dielectric filter, which is a ceramic body sintered from a ceramic system containing MgTiO3 and CaTiO3. The crystal phase in the ceramic body is composed of MgCaTiO3 grains, and the average grain size of the crystal phase is 8.7 μm. In the ceramic body, the volume ratio of the crystal phase to the glass phase is 10:1.793, and the dielectric constant of the ceramic body is 25.2.

[0082] The ceramic material for the dielectric filter is prepared by the following method:

[0083] Synthesis of main crystal phase MgTiO3: Selecting 95% pure basic magnesium carbonate, titanium dioxide and zinc oxide as raw materials, respectively, using 5mm diameter ZrO2 round balls in a ball mill for 8.5 hours; drying the ball-milled basic magnesium carbonate, titanium dioxide and zinc oxide powders and pre-calcining them at a temperature of 1250°C for 6 hours to obtain MgTiO3 pre-calcined melt;

[0084] Synthesis of subcrystalline CaTiO3: Calcium oxide and titanium dioxide with a purity of 95% were ball-milled for 8 hours using 5 mm ZrO2 round balls in a ball mill, and the ball-milled calcium oxide and titanium dioxide powders were dried and pre-sintered at a temperature of 1280°C for 8 hours to obtain a CaTiO3 pre-sintered melt;

[0085] Granulation: The MgTiO3 pre-sintered frit and the CaTiO3 pre-sintered frit are mixed in a mass ratio of 100:5, put into a ball mill and milled with 5 mm diameter ZrO2 round balls to a particle size of 2 μm, and then granulated by spraying after adding a granulation binder to obtain mixed particles;

[0086] Dry pressing: the mixed particles are placed in a metal mold cavity and pressed on both sides with a pressure of 180 MPa on each side and a holding time of 3 seconds to form a ceramic body;

[0087] Sintering: Place the ceramic body in a sintering furnace and sinter it in a step-by-step heating process. The sintering steps are as follows:

[0088] Heating stage: adopt staged heating, low temperature zone, from room temperature to 350℃ at 5℃ / min; medium temperature zone, adjust the heating rate to 10℃ / min from 350℃ to 900℃; high temperature zone, start heating from 900℃ at 15℃ / min, when the temperature reaches 1300℃, adjust the heating rate to 20℃ / min and directly heat to sintering temperature;

[0089] Insulation stage: When the green body is heated to the sintering temperature, it is kept at this temperature for 50 minutes, then the temperature is reduced to 1380℃ and kept for 20 minutes;

[0090] Cooling stage: After the insulation is completed, the temperature is lowered to 300°C at a cooling rate of 25°C / min, and then naturally cooled to room temperature.

[0091] Performance Testing

[0092] The ceramic materials described in the above embodiments 1-3 are processed into a ceramic filter, which includes a ceramic dielectric body, a PCB board and a copper needle. The dielectric body is made of the ceramic material for the dielectric filter described in the embodiment of the present application; the front of the ceramic dielectric body is provided with a debugging blind hole, a coupling blind hole, an output port and an input port, the PCB board is welded to the back of the ceramic body, the copper needle is welded to the output port and the input port, and the upper end of the copper needle is flush with the surface of the PCB board. The performance of the ceramic material and the ceramic filter is tested, and the test items and test results are shown in Table 1.

[0093] Table 1: Performance test results

[0094]

[0095]

[0096] In order to further verify the influence of the mass ratio of MgTiO3 to CaTiO3 on the performance of ceramic materials, on the basis of the scheme of the above-mentioned Example 1, different mass ratios of MgTiO3 to CaTiO3 were set, and the other steps and parameter settings were the same as those in the embodiment. A series of ceramic materials were prepared, and the performance of the ceramic materials was tested. The results are shown in Table 2.

[0097] Table 2: Effect of the mass ratio of MgTiO3 to CaTiO3 on ceramic properties

[0098]

[0099] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.

Claims

1. A ceramic material for a dielectric filter, characterized in that A ceramic body sintered from a ceramic system comprising MgTiO3 and CaTiO3, wherein the crystal phase in the ceramic body is composed of MgCaTiO3 grains, and the average grain size in the crystal phase is 0.35-8.7 μm; in the ceramic body, the volume ratio of the crystal phase to the glass phase is 10:(1.2-1.8), and the dielectric constant of the ceramic body is 25.2-56.

7.

2. The ceramic material for dielectric filter according to claim 1, characterized in that: In the ceramic system, the mass ratio of MgTiO3 to CaTiO3 is 100:(5-12).

3. The ceramic material for dielectric filter according to claim 1, characterized in that: The particle size of the MgTiO3 is 0.8-10 μm, and the purity is greater than or equal to 95%; the particle size of the CaTiO3 is 0.8-2.0 μm, and the purity is greater than or equal to 95%.

4. The ceramic material for dielectric filter according to any one of claims 1 to 3, characterized in that: The ceramic system also includes Nd2O3 powder, and the added amount of Nd2O3 powder accounts for 2-5% of the weight of MgTiO3.

5. The ceramic material for dielectric filter according to claim 4, characterized in that: The particle size of the Nd2O3 powder is 100-500nm.

6. A method for preparing a ceramic material for a dielectric filter according to any one of claims 1 to 5, characterized in that: include Synthesizing the main crystal phase MgTiO3: selecting basic magnesium carbonate, titanium dioxide and zinc oxide with a purity greater than or equal to 95% as raw materials, respectively ball-milling them in a ball mill to a predetermined particle size; drying the ball-milled basic magnesium carbonate, titanium dioxide and zinc oxide powders and pre-calcining them to obtain a MgTiO3 pre-calcined frit; Synthesizing subcrystalline CaTiO3: Calcium carbonate and titanium dioxide with a purity greater than or equal to 95% are respectively ball-milled in a ball mill to a predetermined particle size, and the ball-milled calcium oxide and titanium dioxide powders are dried and pre-calcined to obtain a CaTiO3 pre-calcined frit; Granulation: the MgTiO3 pre-sintered frit and the CaTiO3 pre-sintered frit are mixed and put into a ball mill for ball milling to a predetermined particle size, and a granulation binder is added and then spray granulation is performed to obtain mixed particles; Dry pressing: the mixed particles are placed into a metal mold cavity and dry pressed to form a ceramic body; Sintering: The ceramic body is sintered into a ceramic body in a sintering furnace.

7. The preparation method according to claim 6, characterized in that: In the step of synthesizing the main crystalline phase MgTiO3, ZrO2 round balls with a particle size of 2-5 mm are used for ball milling for 6.5-8.5 hours; the temperature of the pre-sintering treatment is 1210° C.-1250° C., and the pre-sintering time is 6-8 hours.

8. The preparation method according to claim 6, characterized in that: In the step of synthesizing the secondary crystalline phase CaTiO3, ZrO2 round balls with a particle size of 2-5 mm are used for ball milling for 6-8 hours, the pre-sintering temperature is 1250° C.-1280° C., and the pre-sintering time is 8-10 hours.

9. The preparation method according to claim 6, characterized in that: In the granulation step, Nd2O3 powder is added to the mixture obtained by mixing the MgTiO3 pre-sintered frit and the CaTiO3 pre-sintered frit and then ball milling is performed.

10. The preparation method according to claim 6, characterized in that: In the dry pressing step, a servo press is used for double-sided pressing, the molding pressure is 120-180 MPa, and the holding time is 3-8 seconds; the ceramic green body density tolerance is controlled within ±0.02 g / cm 3 .

11. The preparation method according to claim 6, characterized in that: During the sintering process, the sintering temperature is set to 1420-1450°C; the sintering steps include Heating stage: adopt staged heating, low temperature zone, from room temperature to 350℃ at 2-5℃ / min; medium temperature zone, adjust the heating rate to 6-10℃ / min from 350℃ to 900℃; high temperature zone, start heating from 900℃ at 10-15℃ / min, when the temperature reaches 1300℃, adjust the heating rate to 10-20℃ / min and directly heat to sintering temperature; Insulation stage: When the green body is heated to the sintering temperature, it is kept at this temperature for 30-50 minutes, and then the temperature is reduced to 1330-1380℃ and kept for 20-40 minutes; Cooling stage: After the insulation is completed, the temperature is lowered to 300℃ at a cooling rate of 20-25℃ / min, and then begins to cool naturally to room temperature.

12. A dielectric filter, comprising a ceramic dielectric body, a PCB board and a copper needle, characterized in that: The dielectric body is made of the ceramic material for dielectric filter as described in any one of claims 1 to 5; the front of the ceramic dielectric body is provided with a debugging blind hole, a coupling blind hole, an output port and an input port, the PCB board is welded on the back of the ceramic body, the copper needle is welded on the output port and the input port, and the upper end of the copper needle is flush with the surface of the PCB board.

13. A communication antenna, characterized in that: Comprising the dielectric filter as claimed in claim 12.

Citation Information

Patent Citations

  • Temperature-stable type low-loss microwave dielectric ceramic and preparing method thereof

    CN104961453A

  • Microwave dielectric ceramic and manufacturing method thereof

    CN111410528A

  • Microwave dielectric ceramic injection feed, microwave dielectric ceramic and preparation method of microwave dielectric ceramic

    CN112876270A

  • Microwave dielectric ceramic, preparation method thereof and microwave device

    CN112979304A

Cited By

  • High-strength and high-thermal-expansion ceramic shell material for chip packaging and preparation method thereof

    CN121135394A