Stable-dispersion ceramic slurry and preparation method thereof

By performing high-speed stirring and grinding in a horizontal sand mill, combined with the addition and cooling system of dispersant, the problems of long grinding time and uneven particle distribution in the preparation of ceramic slurry are solved, and efficient and uniform ceramic slurry is achieved Preparation improves product performance and production efficiency.

CN118955150APending Publication Date: 2024-11-15苏州芯合半导体材料有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411061163.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing ceramic slurry preparation methods, the ball milling method requires a long grinding time, resulting in increased energy consumption and uneven particle distribution, affecting product performance and quality.

Method used

High-speed stirring and grinding are used for high-speed stirring and grinding, feeding the material in sequence according to the proportion of components, pre-mixing to ensure uniform mixing, and adding dispersant during the grinding process, using the high-speed collision and shearing effect of the grinding ball and the material, combined with cooling The system controls the temperature to ensure dispersion stability and fine particle size distribution.

Benefits of technology

It significantly reduces grinding time, avoids particle grading problems, controls slurry temperature, improves physical performance and production efficiency, and ensures dispersion stability and product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955150A_ABST
    Figure CN118955150A_ABST
Patent Text Reader

Abstract

The invention is suitable for the technical field of ceramic slurry preparation, and provides stable-dispersion ceramic slurry and a preparation method thereof.The preparation method comprises the following steps that firstly, a water-based solvent is put into a horizontal sand mill, a stirring button of the horizontal sand mill is pressed down, and stirring is conducted at the set stirring frequency; sequentially feeding the components in the mixed powder from high to low according to the proportion of the components in the mixed powder, and pre-stirring for a certain time before each time of feeding; the sand mill is started, related pipelines are opened, and the sand mill continuously operates for a period of time; when the running time of the sand mill reaches half, a dispersing agent is fed through a feeding opening, and then sand milling is continued; after sanding is completed, the ground ceramic slurry is discharged out of the sand mill, then a binder and a release agent are added, and then dispersion granulation operation is carried out. The ceramic slurry which is stable in dispersion and small in particle size is successfully prepared. The method not only improves the preparation efficiency and the product quality of the ceramic slurry, but also provides convenience and guarantee for subsequent processing procedures.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic slurry preparation, and in particular relates to a dispersed and stable ceramic slurry and a preparation method thereof. Background Art

[0002] Ceramic splitters are widely used consumables in chip bonding, and play an important role in products that use chips, such as computers, electrical appliances, automobiles, and mobile phones. With the expansion of the scale of various industries and the rise of domestic products, the performance requirements for ceramic splitters are getting higher and higher. The front-end product in the preparation of ceramic splitters, ZTA ceramic slurry, affects the performance of ceramic splitters.

[0003] Existing methods for preparing ceramic slurries, such as ball milling, usually require a long grinding time to achieve the required powder fineness and uniformity. This not only increases the production cycle, but may also lead to an increase in energy consumption and reduce overall production efficiency. In mechanical pulverization processes such as ball milling, the particle gradation (i.e. the ratio of particles of different sizes) is often difficult to accurately control, which may lead to uneven distribution of particles in the slurry, thereby affecting the performance and quality of subsequent products.

[0004] Ceramic slurry is mainly composed of mixed ceramic powder, aqueous solvent, dispersant, binder, release agent, etc. Carboxylic acid preparation dispersant is a relatively important type of additive in ceramic slurry. Dispersant can generate a greater repulsive force between particles, thereby separating particles and accelerating the penetration of solvent between ceramic bodies to achieve the purpose of separating ceramic powder. Stably dispersed ceramic slurry is more conducive to subsequent granulation and particle distribution in product sintered bodies. Based on the above background, the present invention proposes a stably dispersed ceramic slurry and a preparation method thereof. Summary of the invention

[0005] The object of the present invention is to provide a dispersed and stable ceramic slurry and a preparation method thereof, aiming to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a dispersed and stable ceramic slurry comprises the following steps:

[0008] Step 1: First, add aqueous solvent into the horizontal sand mill, press the stirring button of the horizontal sand mill, set the stirring frequency for high-speed stirring to ensure that the solvent is evenly distributed in the machine and reaches a certain turbulent state, which is conducive to the uniform mixing and grinding of subsequent materials;

[0009] Step 2: Add materials in descending order according to the proportion of each component in the mixed powder. This order of adding materials helps to evenly distribute the main components and reduce the stratification phenomenon caused by density differences. Before each addition, pre-stir for a certain period of time to ensure that the newly added powder is fully mixed with the existing materials to form a uniform mixture, laying a good foundation for subsequent grinding;

[0010] Step 3: Turn on the sand mill and open the relevant pipelines. The sand mill will continue to operate for a period of time; the material will be ground to the required fineness by the high-speed collision and shearing effect between the grinding balls and the material. During this process, the cooling system of the sand mill will operate synchronously to control and dissipate the heat generated during the grinding process to prevent the material from deteriorating or agglomerating due to high temperature.

[0011] Step 4: When the sand mill has been running for half of its operation time, add dispersant through the feeding port and continue sand grinding. Adding dispersant at this time can make full use of the remaining grinding time, allowing the dispersant to fully act on the surface of the material to form a stable dispersion system.

[0012] Step 5: After sand grinding, the ground ceramic slurry is discharged from the sand mill. At this time, the slurry shows good dispersion stability and fine particle size distribution. Then add binder and release agent, and then perform dispersion granulation. Due to the adequacy of the previous grinding and dispersion treatment, the slurry is not prone to material agglomeration during the granulation process, thus ensuring the quality and performance of the final product.

[0013] Furthermore, in step 1, the stirring frequency is 40 to 50 Hz.

[0014] Furthermore, in step 2, the mixture is pre-stirred for 60 minutes before each feeding.

[0015] Furthermore, in step 3, the sand mill is continuously operated for 3 to 4 hours.

[0016] Furthermore, in step 4, the dispersant is a carboxylic acid dispersant or an ammonium root dispersant.

[0017] Furthermore, the addition ratio of the dispersant is 3-4%, which can effectively prevent the material from agglomerating, and will not introduce unnecessary impurities or affect the performance of the slurry due to excessive addition.

[0018] A dispersed and stable ceramic slurry is prepared according to the method for preparing a dispersed and stable ceramic slurry as described above.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1. The present invention directly completes the grinding, mixing and dispersion of powder in a sand mill, greatly reducing the operation time and eliminating the need to consider the particle grading problem in traditional ball milling.

[0021] 2. The present invention can perfectly solve the problem of slurry temperature increase in traditional ball milling through the refrigeration system during the sand milling process, making the slurry have better physical properties and easier production.

[0022] 3. After adding the dispersant, the present invention uses a high rotation speed to more easily break the strong agglomeration of fine particles, so that the solvent with the dispersant can fully wrap the powder and maintain stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0026] Embodiment 1: One embodiment of the present invention provides a method for preparing a dispersed and stable ceramic slurry, comprising the following steps:

[0027] Step 1: First, add aqueous solvent into the horizontal sand mill, press the stirring button of the horizontal sand mill, and set the stirring frequency to 45HZ for stirring.

[0028] Step 2: Add materials in descending order according to the proportion of each component in the mixed powder, and stir for 60 minutes before each addition;

[0029] Step 3: Turn on the sand grinder, set the sanding time to 3.5 hours, and keep the cooling system on.

[0030] Step 4: When the sand mill is running for 1.75 h, add 3.5% of the total weight of a carboxylic acid dispersant as a dispersant through the feed port.

[0031] Step 5: After sand grinding, the ground ceramic slurry is discharged from the sand mill, and then a binder and a release agent are added, and then a dispersion granulation operation is performed.

[0032] Embodiment 2: One embodiment of the present invention provides a method for preparing a dispersed and stable ceramic slurry, comprising the following steps:

[0033] Step 1: First, add aqueous solvent into the horizontal sand mill, press the stirring button of the horizontal sand mill, and set the stirring frequency to 48HZ for stirring.

[0034] Step 2: Add materials in descending order according to the proportion of each component in the mixed powder, and stir for 60 minutes before each addition;

[0035] Step 3: Turn on the sand grinder, set the sanding time to 3.4 hours, and keep the cooling system on.

[0036] Step 4: When the sand mill is running for 1.7 hours, add 3% of the total weight of a carboxylic acid dispersant as a dispersant through the feed port.

[0037] Step 5: After sand grinding, the ground ceramic slurry is discharged from the sand mill, and then a binder and a release agent are added, and then a dispersion granulation operation is performed.

[0038] Embodiment 3: One embodiment of the present invention provides a method for preparing a dispersed and stable ceramic slurry, comprising the following steps:

[0039] Step 1: First, add aqueous solvent into the horizontal sand mill, press the stirring button of the horizontal sand mill, and set the stirring frequency to 50HZ for stirring.

[0040] Step 2: Add materials in descending order according to the proportion of each component in the mixed powder, and stir for 60 minutes before each addition;

[0041] Step 3: Turn on the sand grinder, set the sanding time to 3.2 hours, and keep the cooling system on.

[0042] Step 4: When the sand mill is running for 1.6 hours, add 4% of the total weight of ammonium root dispersant as a dispersant through the feeding port.

[0043] Step 5: After sand grinding, the ground ceramic slurry is discharged from the sand mill, and then a binder and a release agent are added, and then a dispersion granulation operation is performed.

[0044] Embodiment 4: One embodiment of the present invention provides a method for preparing a dispersed and stable ceramic slurry, comprising the following steps:

[0045] Step 1: First, add aqueous solvent into the horizontal sand mill, press the stirring button of the horizontal sand mill, and set the stirring frequency to 42HZ for stirring.

[0046] Step 2: Add materials in descending order according to the proportion of each component in the mixed powder, and stir for 60 minutes before each addition;

[0047] Step 3: Turn on the sand grinder, set the sanding time to 3.8 hours, and keep the cooling system on.

[0048] Step 4: When the sand mill has been running for 1.9 hours, a carboxylic acid dispersant accounting for 3.8% of the total weight is added as a dispersant through the feed port.

[0049] Step 5: After sand grinding, the ground ceramic slurry is discharged from the sand mill, and then a binder and a release agent are added, and then a dispersion granulation operation is performed.

[0050] Embodiment 5: One embodiment of the present invention provides a method for preparing a dispersed and stable ceramic slurry, comprising the following steps:

[0051] Step 1: First, add aqueous solvent into the horizontal sand mill, press the stirring button of the horizontal sand mill, and set the stirring frequency to 40HZ for stirring.

[0052] Step 2: Add materials in descending order according to the proportion of each component in the mixed powder, and stir for 60 minutes before each addition;

[0053] Step 3: Turn on the sand grinder, set the sanding time to 4 hours, and keep the cooling system on.

[0054] Step 4: When the sand mill is running for 2 hours, add 3.5% of the total weight of ammonium root dispersant as a dispersant through the feeding port.

[0055] Step 5: After sand grinding, the ground ceramic slurry is discharged from the sand mill, and then a binder and a release agent are added, and then a dispersion granulation operation is performed.

[0056] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A method for preparing a dispersed and stable ceramic slurry, characterized in that: The following steps are involved: Step 1: First, add an aqueous solvent into the horizontal sand mill, press the stirring button of the horizontal sand mill, and set the stirring frequency for stirring; Step 2: Add materials in order from high to low according to the proportion of each component in the mixed powder, and stir for a certain time before each addition; Step 3: Turn on the sand mill and open the relevant pipelines. The sand mill continues to operate for a period of time; Step 4: When the sand mill is running for half of its operation time, add dispersant through the feeding port, and then continue sand milling; Step 5: After sand grinding, the ground ceramic slurry is discharged from the sand mill, and then a binder and a release agent are added, and then a dispersion granulation operation is performed.

2. The method for preparing a dispersed and stable ceramic slurry according to claim 1, characterized in that: In the step 1, the stirring frequency is 40 to 50 Hz.

3. The method for preparing a dispersed and stable ceramic slurry according to claim 1, characterized in that: In the step 2, the mixture is pre-stirred for 60 minutes before each feeding.

4. The method for preparing a dispersed and stable ceramic slurry according to claim 1, characterized in that: In step 3, the sand mill is continuously operated for 3 to 4 hours.

5. The method for preparing a dispersed and stable ceramic slurry according to claim 1, characterized in that: In the step 4, the dispersant is a carboxylic acid dispersant or an ammonium root dispersant.

6. The method for preparing a dispersed and stable ceramic slurry according to claim 5, characterized in that: The addition ratio of the dispersant is 3-4%.

7. A dispersed and stable ceramic slurry obtained by the method for preparing a dispersed and stable ceramic slurry according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Magnesium silicate-based microwave dielectric ceramic material as well as preparation method and application thereof

    CN111138176A

  • Preparation method of nanoparticles and application thereof

    CN112007739A

  • Method for preparing graphene reinforced nonmetal-based composite material by adopting step-by-step charging ball milling and hot pressed sintering

    CN113292322A

  • Preparation method of water-based ceramic slurry for coating and battery diaphragm

    CN114057430A

  • Preparation method of high-density boron carbide ceramic

    CN114538929A