Water-based adhesive and application thereof in electronic ceramic forming

By using epoxy modified polyacrylate emulsion and polyamine compounds in the aqueous casting process, the body-shaped crosslinking structure and hydrogen bonding reaction are formed, the problem of insufficient strength of ceramic sheets in the aqueous casting process is solved, and the problem of significantly improved The mechanical strength of ceramics is suitable for industrial applications.

CN118955151AActive Publication Date: 2024-11-15XINXING ELECTRONIC CERAMICS CO LTD
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
CN202411026729.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The strength of the ceramic sheet after film formation in the aqueous casting process is not high, which limits subsequent processing and industrial applications.

Method used

Epoxy modified polyacrylate emulsion and polyamine compounds are used to improve the mechanical strength of ceramic particles by forming a body-shaped crosslinking structure and hydrogen bond reaction.

Benefits of technology

It significantly improves the mechanical strength of the ceramic blank and is suitable for subsequent processing and industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004968759500000021
    Figure BDA0004968759500000021
  • Figure BDA0004968759500000022
    Figure BDA0004968759500000022
  • Figure BDA0004968759500000031
    Figure BDA0004968759500000031
Patent Text Reader

Abstract

The invention relates to the field of adhesives, in particular to a water-based adhesive and application in electronic ceramic molding, the water-based adhesive comprises epoxy modified polyacrylate emulsion and a polyamine compound, the mass ratio of the epoxy modified polyacrylate emulsion to the polyamine compound is 1: (0.01-0.05), and tests show that the water-based adhesive has the advantages that the water-based adhesive has excellent water-based adhesive performance; the alumina biscuit prepared by using the adhesive provided by the invention has high mechanical strength, and is beneficial to subsequent processing and industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of adhesives, in particular to a water-based adhesive and application thereof in electronic ceramic molding. Background Art

[0002] Since the emergence of the tape casting method in 1945, it has been widely used in the molding process of electronic ceramic materials. It is an important method for preparing large-area, thin-plane ceramic materials. According to the solvents used in the current tape casting process, it can be divided into two categories: non-aqueous series and aqueous series. From the research situation at home and abroad in recent years, the research on the tape casting process of the non-aqueous system has been relatively mature. The prepared electronic ceramic green sheets have uniform structure, high strength, good flexibility, easy cutting and processing, and have been widely used in industrial production. However, due to the use of a large amount of flammable and toxic organic solvents, adhesives, dispersants, etc. in the non-aqueous series of tape casting processes, it will cause certain harm to the human body and the environment. Therefore, the study of tape casting technology using water as a solvent instead of organic solvents has become an irreversible trend, but the strength of the ceramic green sheets after tape casting with water as a solvent is not high, which greatly limits the subsequent processing and industrial application. Summary of the invention

[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a water-based adhesive and its application in electronic ceramic molding.

[0004] The technical solutions adopted are as follows:

[0005] A water-based adhesive comprises epoxy-modified polyacrylate emulsion and polyamine compounds.

[0006] Furthermore, the mass ratio of the epoxy-modified polyacrylate emulsion to the polyamine compound is 1:0.01-0.05.

[0007] Furthermore, the preparation method of the epoxy-modified polyacrylate emulsion is as follows:

[0008] Add emulsifier and part of free radical initiator into water, stir and heat to 60-80°C, add acrylate monomer and remaining free radical initiator, keep the temperature for reaction for 5-10 hours and then return to room temperature.

[0009] Furthermore, the acrylic acid ester monomers include acrylic acid, methyl methacrylate and glycidyl methacrylate.

[0010] Furthermore, the mass ratio of acrylic acid, methyl methacrylate and glycidyl methacrylate is 5-10:0.5-1:1-5.

[0011] Furthermore, the free radical initiator is any one or more combinations of potassium persulfate, benzoyl peroxide, lauroyl peroxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, azobisisobutyronitrile, azobisisoheptanenitrile, and azobiscyanovaleric acid.

[0012] Furthermore, the structure of the polyamine compound is shown in Formula 1:

[0013]

[0014] R 1 , R 2 , R 3 Each independently is hydrogen, amino or the structural formula shown in Formula 2:

[0015]

[0016] And R 1 , R 2 , R 3 At least one of them is a structure shown in Formula 2, R 1 , R 2 , R 3 At most one of them is hydrogen.

[0017] Furthermore, R 1 , R 2 , R 3 At least two of them are the structural formula shown in Formula 2.

[0018] Furthermore, the polyamine compound is any one of the following compounds:

[0019]

[0020] Furthermore, the present invention also provides an application of a water-based adhesive in electronic ceramic molding.

[0021] Beneficial effects of the present invention:

[0022] The present invention provides a water-based adhesive, which is prepared by epoxy-modifying a polyacrylate emulsion, introducing an epoxy group with high cross-linking activity, and then forming a three-dimensional cross-linked structure polymer through the reaction of a polyamine compound and the epoxy group, so as to wrap ceramic particles as a whole, and solidify the polymer through reaction during the process of tape casting and drying to form a three-dimensional network shape, so that the mechanical strength of the prepared ceramic blank is greatly improved. At the same time, the amide bonds in the polyamine compound will undergo hydrogen bonding reactions to generate hydrogen bonding forces, which also improves the mechanical strength of the ceramic blank to a certain extent. The aluminum oxide blank prepared by using the adhesive of the present invention has high mechanical strength, which is conducive to subsequent processing and industrial application. DETAILED DESCRIPTION

[0023] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.

[0024] Embodiment 1:

[0025] A water-based adhesive comprises an epoxy-modified polyacrylate emulsion and a polyamine compound in a mass ratio of 1:0.05.

[0026] Wherein, the preparation method of epoxy modified polyacrylate emulsion is as follows:

[0027] Add 1.4g of emulsifier SDS and 0.2g of potassium persulfate to 150ml of water, stir and heat to 65°C, then add acrylate monomers consisting of 30g of acrylic acid, 2g of methyl methacrylate and 5g of glycidyl methacrylate and another 0.4g of potassium persulfate, keep the reaction warm for 8h and then return to room temperature, finally adjust the solid content to 10% with water.

[0028] Polyamine compounds are compounds with the following structure:

[0029]

[0030] Embodiment 2:

[0031] A water-based adhesive comprises an epoxy-modified polyacrylate emulsion and a polyamine compound in a mass ratio of 1:0.05.

[0032] Wherein, the preparation method of epoxy modified polyacrylate emulsion is as follows:

[0033] Add 1.4g of emulsifier SDS and 0.2g of potassium persulfate to 150ml of water, stir and heat to 65°C, then add acrylate monomers consisting of 30g of acrylic acid, 2g of methyl methacrylate and 5g of glycidyl methacrylate and another 0.4g of potassium persulfate, keep the reaction warm for 8h and then return to room temperature, finally adjust the solid content to 10% with water.

[0034] Polyamine compounds are compounds with the following structure:

[0035]

[0036] Embodiment 3:

[0037] A water-based adhesive comprises an epoxy-modified polyacrylate emulsion and a polyamine compound in a mass ratio of 1:0.05.

[0038] Wherein, the preparation method of epoxy modified polyacrylate emulsion is as follows:

[0039] Add 1.4g of emulsifier SDS and 0.2g of potassium persulfate to 150ml of water, stir and heat to 65°C, then add acrylate monomers consisting of 30g of acrylic acid, 2g of methyl methacrylate and 5g of glycidyl methacrylate and another 0.4g of potassium persulfate, keep the reaction warm for 8h and then return to room temperature, finally adjust the solid content to 10% with water.

[0040] Polyamine compounds are compounds with the following structure:

[0041]

[0042] Embodiment 4:

[0043] A water-based adhesive comprises an epoxy-modified polyacrylate emulsion and a polyamine compound in a mass ratio of 1:0.03.

[0044] Wherein, the preparation method of epoxy modified polyacrylate emulsion is as follows:

[0045] Add 1.4g of emulsifier SDS and 0.2g of potassium persulfate to 150ml of water, stir and heat to 65°C, then add acrylate monomers consisting of 30g of acrylic acid, 2g of methyl methacrylate and 5g of glycidyl methacrylate and another 0.4g of potassium persulfate, keep the reaction warm for 8h and then return to room temperature, finally adjust the solid content to 10% with water.

[0046] Polyamine compounds are compounds with the following structure:

[0047]

[0048] Embodiment 5:

[0049] A water-based adhesive comprises an epoxy-modified polyacrylate emulsion and a polyamine compound in a mass ratio of 1:0.01.

[0050] Wherein, the preparation method of epoxy modified polyacrylate emulsion is as follows:

[0051] Add 1.4g of emulsifier SDS and 0.2g of potassium persulfate to 150ml of water, stir and heat to 65°C, then add acrylate monomers consisting of 30g of acrylic acid, 2g of methyl methacrylate and 5g of glycidyl methacrylate and another 0.4g of potassium persulfate, keep the reaction warm for 8h and then return to room temperature, finally adjust the solid content to 10% with water.

[0052] Polyamine compounds are compounds with the following structure:

[0053]

[0054] Comparative Example 1:

[0055] The method is basically the same as Example 1, except that no polyamine compound is added.

[0056] Performance testing:

[0057] The aluminum oxide powder (D 50 3.4 μm, Alteo Company) was put into the ball mill of a planetary ball mill, and then the aqueous binders in Examples 1-5 and Comparative Example 1 were added respectively, the mass ratio of alumina powder to aqueous binder was 1:1, and the slurry was obtained by ball milling at a speed of 600 r / min for 5 hours, and then the slurry was defoamed on a vacuum defoamer, and then tape-casted on a tape-casting machine. The obtained tape-cast sheet was dried at 50°C for 48 hours and then demolded to obtain an alumina blank, which was used as a sample for performance testing;

[0058] The three-point bending method was used to determine the bending strength of the sample. The test equipment was a WDW-10 multifunctional material testing machine. The sample size was 25 mm × 5 mm × 5 mm. The loading rate was 0.05 mm / s. The test results are shown in Table 1 below:

[0059] Table 1:

[0060]

[0061] It can be seen from Table 1 above that the alumina blank prepared using the binder of the present invention has a higher mechanical strength;

[0062] By comparing the data of Example 1 with those of Examples 2 and 3, it can be seen that the increase in the number of amide bonds plays a positive role in improving the mechanical strength of the alumina blank;

[0063] By comparing the data of Example 1 with those of Examples 4 and 5, it can be seen that when the mass ratio of the epoxy-modified polyacrylate emulsion to the polyamine compound is 1:0.03, the mechanical strength of the alumina blank is the best;

[0064] By comparing the data of Example 1 with that of Comparative Example 1, it can be seen that the addition of polyamine compounds plays a positive role in improving the mechanical strength of the alumina blank.

[0065] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A water-based adhesive, It is characterized in that Including epoxy modified polyacrylate emulsion and polyamine compounds.

2. The aqueous adhesive according to claim 1, It is characterized in that The mass ratio of the epoxy modified polyacrylate emulsion to the polyamine compound is 1:0.01-0.

05.

3. The aqueous adhesive according to claim 1, It is characterized in that The preparation method of the epoxy modified polyacrylate emulsion is as follows: Add emulsifier and part of free radical initiator into water, stir and heat to 60-80°C, add acrylate monomer and remaining free radical initiator, keep the temperature for reaction for 5-10 hours and then return to room temperature.

4. The aqueous adhesive according to claim 3, It is characterized in that The acrylic acid ester monomers include acrylic acid, methyl methacrylate and glycidyl methacrylate.

5. The aqueous adhesive according to claim 4, It is characterized in that The mass ratio of acrylic acid, methyl methacrylate and glycidyl methacrylate is 5-10:0.5-1:1-5.

6. The aqueous adhesive according to claim 1, It is characterized in that The free radical initiator is any one or more combinations of potassium persulfate, benzoyl peroxide, lauroyl peroxide, di-tert-butyl peroxide, diisopropylbenzene peroxide, azobisisobutyronitrile, azobisisoheptanenitrile, and azobiscyanovaleric acid.

7. The aqueous adhesive according to claim 1, It is characterized in that The structure of the polyamine compound is shown in Formula 1: R 1 , R 2 , R 3 Each independently is hydrogen, amino or the structural formula shown in Formula 2: And R 1 , R 2 , R 3 At least one of them is a structural formula shown in Formula 2, R 1 , R 2 , R 3 At most one of them is hydrogen.

8. The aqueous adhesive according to claim 7, It is characterized in that R 1 , R 2 , R 3 At least two of them are the structural formula shown in Formula 2.

9. The aqueous adhesive according to claim 8, It is characterized in that The polyamine compound is any one of the following compounds:

10. Use of the aqueous adhesive according to any one of claims 1 to 9 in electronic ceramic molding.

Citation Information

Patent Citations

  • PROCESS FOR PREPARING NEW P-(P-ALKYL-BENZOYLOXY)-BENZOESSAUREPHENYLESTERS

    ATA395978A

  • Sealants, adhesives, sealants and bonding compounds and methods for their preparation

    BE833567A

  • Epoxy adhesive, automotive member, and method for manufacturing same

    CN107001893A

  • Alumina ceramic substrate and preparation method thereof

    CN116606124A

  • Polyurethane reaction adhesive, especially for bonding plastic with silicone

    DE19539653A1