Long-life electric furnace cover and preparation method thereof

By combining silicon carbide particles with vanadium-containing steel slag powder, the material composition and structure are regulated, and a long-life electric furnace cover with high thermal shock stability and slag corrosion resistance is solved, and the refractory materials of the electric furnace cover are easily damaged and vanadium-containing steel slag resources are not available. The problem of utilization has realized the durability and resource recycling of the electric furnace cover.

CN118955156AActive Publication Date: 2024-11-15YIXING XINGYE CHARGING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411027918.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The electric furnace cover is prone to damage under harsh conditions such as high temperature, erosion, and erosion, resulting in cracking and peeling of refractory materials, shortening service life, and the vanadium-containing steel slag resources cannot be effectively utilized, affecting process efficiency and environmental protection.

Method used

Mix 60-80% silicon carbide particles with 20-40% vanadium-containing steel slag powder. After granulation and heat treatment, combine mullite, corundum, explosion-proof fiber and other materials to form a long-life electric furnace through vibration molding and natural curing. The cover regulates the composition and structure of the material, improves thermal shock stability and resistance to slag corrosion.

Benefits of technology

The prepared electric furnace cover has high thermal shock stability and excellent slag corrosion resistance, which extends the service life and effectively utilizes vanadium-containing steel slag resources, improving the resource recycling efficiency of the process.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a long-life electric furnace cover and a preparation method thereof. Uniformly mixing 60-80% by mass of silicon carbide particles and 20-40% by mass of vanadium-containing steel slag powder to obtain a granulation material; granulating the granulation material, drying the obtained material particles at 70-90 DEG C for 5-10 hours, then carrying out heat treatment on the material particles at 600-800 DEG C for 1-3 hours, and screening the material particles to obtain a composite silicon carbide granulation material with the particle size of 1-0 mm; the preparation method comprises the following steps: uniformly mixing the following components in percentage by mass: 20-40% of 8-1mm mullite particles, 15-25% of 3-1mm tabular corundum, 15-25% of 1-0mm tabular corundum, 1-3% of silicon carbide particles, 3-5% of a composite silicon carbide granulation material, 1-5% of fused white corundum powder, 5-10% of corundum micro-powder, 1-5% of silicon micro-powder, 0.2-0.6% of explosion-proof fibers, 0.5-1% of a water reducing agent and 1-3% of calcium aluminate cement; adding 4-7% of water, uniformly mixing, and pouring into a mold for vibration molding; and naturally curing with a mold for 24 hours, demolding, naturally curing for 2-3 days, baking at 200-250 DEG C for 30-40 hours, and cooling to room temperature along with the furnace. The furnace cover is long in service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a long-life electric furnace cover and a preparation method thereof. Background technology:

[0002] Electric furnace steelmaking involves smelting steel using induction heating to generate an arc between graphite electrodes and the charge, melting alloys and scrap steel through arc radiation, convection, and heat conduction, followed by oxidation and reduction. This process offers advantages such as a short process, simple equipment, low energy consumption, high utilization rates, and significant energy conservation and emission reduction. However, the harsh conditions of the electric furnace steelmaking process, such as high temperatures, erosion, and corrosion, can severely damage the furnace's refractory materials, impacting efficiency. The furnace cover, a critical component of the furnace, must withstand complex conditions such as high temperatures, rapid heating and cooling, and splashing / erosion of high-temperature melt during operation. These conditions can easily cause cracking, flaking, and damage to the cover's refractory materials, reducing performance and lifespan. To address these issues, researchers have improved the structure, mechanical strength, and thermal shock stability of the electric furnace cover refractory materials by introducing hollow alumina balls, andalusite, and regulating mullite and binders. However, since the low-melting-point phase generated in the refractory matrix at high temperatures is difficult to control, the refractory materials suffer from unstable high-temperature performance and low resistance to high-temperature melt erosion, resulting in a reduced service life.

[0003] Vanadium-containing steel slag typically refers to the water-quenched slag produced after vanadium-titanium magnetite smelting in blast furnaces. It is considered a general solid waste. Blast furnaces produce up to 3 million tons of vanadium-containing steel slag annually, which is generally discarded as waste. Current research on the resource recovery of vanadium-containing steel slag primarily utilizes various methods to extract metallic elements such as vanadium, iron, and calcium. However, the effective utilization of the active components of vanadium-containing steel slag for resource recycling requires further research and engineering application.

[0004] The information disclosed in this background technology section is only intended to enhance understanding of the overall background of the invention and should not be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention:

[0005] The object of the present invention is to provide a long-life electric furnace cover and a preparation method thereof, thereby overcoming the above-mentioned defects in the prior art.

[0006] To achieve the above object, the present invention provides a long-life electric furnace cover and a preparation method thereof, comprising the following steps: (1) uniformly mixing 60-80% by mass of silicon carbide particles and 20-40% by mass of vanadium-containing steel slag powder to obtain granulated material;

[0007] (2) granulating the granulated material obtained in step (1), drying the obtained material particles at 70-90° C. for 5-10 hours, then heat treating the material particles at 600-800° C. for 1-3 hours, and sieving the material particles to obtain composite silicon carbide granulated material with a particle size of 1-0 mm;

[0008] (3) 20-40% of 8-1 mm mullite particles, 15-25% of 3-1 mm plate-shaped corundum, 15-25% of 1-0 mm plate-shaped corundum, 1-3% of silicon carbide particles, 3-5% of composite silicon carbide granules, 1-5% of fused white corundum powder, 5-10% of corundum micropowder, 1-5% of silicon micropowder, 0.2-0.6% of explosion-proof fiber, 0.5-1% of water reducer, 1-3% of calcium aluminate cement, and 4-7% of water are mixed uniformly by mass percentage, poured into a mold and vibrated to form;

[0009] (4) After natural curing for 24 hours with the mold, the mold is demoulded, and then naturally cured for 2-3 days, baked at 200-250℃ for 30-40 hours, and cooled to room temperature with the furnace to obtain a long-life electric furnace cover.

[0010] Preferably, in the technical solution, the particle size of the silicon carbide particles is less than 0.5 mm, and the mass percentage of silicon carbide in the silicon carbide particles is ≥97.0%.

[0011] Preferably, in the technical solution, the particle size of the vanadium-containing steel slag powder is less than 45 microns, and its components are as follows in percentage: V2O5 is 1.5-3%, SiO2<13%, and CaO is 35-40%.

[0012] Preferably, in the technical solution, 10-20% water mist is sprayed onto the granulated material during the granulation process.

[0013] Preferably, in the technical solution, the mass percentage of Al2O3 in the mullite particles is greater than 70.0%, and the mass percentage of Fe2O3 is less than 1.0%.

[0014] Preferably, in the technical solution, the mass percentage of Al2O3 in the tabular corundum is greater than 99%.

[0015] Preferably, in the technical solution, the particle size of the fused white corundum powder is ≤0.088 mm, and the mass percentage of Al2O3 in the fused white corundum powder is greater than 99%.

[0016] Preferably, in the technical solution, the particle size of the corundum micropowder is ≤0.002 mm, and the mass percentage of Al2O3 in the corundum micropowder is ≥99.5%.

[0017] Preferably, in the technical solution, the particle size of the silicon micropowder is ≤0.005 mm, and the mass percentage of SiO2 in the silicon micropowder is ≥94wt%.

[0018] Preferably, in the technical solution, the explosion-proof fiber has a length of 5-7 mm and a melting point of 160±5°C.

[0019] Preferably, in the technical solution, the water reducer is sodium tripolyphosphate or sodium hexametaphosphate.

[0020] Preferably, in the technical solution, the particle size of the calcium aluminate cement is ≤0.044 mm, and the mass percentage of Al2O3 in the calcium aluminate cement is ≥75%.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] By leveraging the vanadium-containing steel slag in the prefabricated composite silicon carbide granules to regulate the oxidation and reaction behavior of the silicon carbide particles, the composition and microstructure of the resulting refractory are controlled. This leverages silicon carbide's advantages in thermal shock stability and slag erosion resistance while mitigating its disadvantage of being susceptible to oxidation at high temperatures. The resulting long-life electric furnace cover exhibits high thermal shock stability and excellent slag erosion resistance. By regulating the distribution of phases such as corundum, mullite, and silicon carbide, and adjusting the distribution and development of different raw materials and phases within the refractory to strengthen the microstructure, the resulting long-life electric furnace cover exhibits moderate density and high mechanical strength. Specific implementation method:

[0023] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0024] Unless expressly stated otherwise, throughout the specification and claims, the term "comprise" or variations such as "include" or "comprising", etc., will be understood to include the stated elements or components but not to exclude other elements or other components.

[0025] Example 1

[0026] A long-life electric furnace cover and a preparation method thereof, comprising the following steps: (1) uniformly mixing 60% of silicon carbide particles and 40% of vanadium-containing steel slag powder according to mass percentage to obtain granulated material;

[0027] (2) granulating the granulated material obtained in step (1), drying the obtained material particles at 70° C. for 5 hours, then heat-treating the material particles at 600° C. for 3 hours, and sieving the material particles to obtain composite silicon carbide granulated materials with a particle size of 1-0 mm;

[0028] (3) 30% of 8-1 mm mullite particles, 25% of 3-1 mm plate-shaped corundum, 24% of 1-0 mm plate-shaped corundum, 2% of silicon carbide particles, 3% of composite silicon carbide granules, 2% of fused white corundum powder, 8% of corundum micropowder, 3% of silicon micropowder, 0.2% of explosion-proof fiber, 0.8% of sodium tripolyphosphate, 2% of calcium aluminate cement, and 5% of water were mixed uniformly by mass percentage, poured into a mold, and vibrated to form;

[0029] (4) After natural curing for 24 hours with the mold, the mold is demoulded, and then naturally cured for 3 days, baked at 220°C for 30 hours, and cooled to room temperature with the furnace to obtain a long-life electric furnace cover.

[0030] The long-life electric furnace cover prepared in this embodiment has been tested to have the following characteristics: bulk density of 2.85 g / cm3; flexural strength of 22 MPa at 110°C for 24 hours, and compressive strength of 60 MPa; flexural strength retention of 62% after 5 cycles of water cooling at 1100°C; and excellent resistance to slag erosion.

[0031] Example 2

[0032] A long-life electric furnace cover and a preparation method thereof, comprising the following steps: (1) uniformly mixing 60% of silicon carbide particles and 40% of vanadium-containing steel slag powder according to mass percentage to obtain granulated material;

[0033] (2) granulating the granulated material obtained in step (1), drying the obtained material particles at 90° C. for 10 hours, then heat-treating the material particles at 800° C. for 2 hours, and sieving the material particles to obtain composite silicon carbide granulated materials with a particle size of 1-0 mm;

[0034] (3) 28% of 8-1 mm mullite particles, 22% of 3-1 mm plate-shaped corundum, 20% of 1-0 mm plate-shaped corundum, 3% of silicon carbide particles, 5% of composite silicon carbide granules, 3% of fused white corundum powder, 10% of corundum micropowder, 5% of silicon micropowder, 0.5% of explosion-proof fiber, 0.5% of sodium tripolyphosphate, 3% of calcium aluminate cement, and 7% of water were mixed uniformly by mass percentage, poured into a mold, and vibrated to form;

[0035] (4) After natural curing for 24 hours with the mold, the mold is demoulded, and then naturally cured for 2 days, baked at 200°C for 40 hours, and cooled to room temperature with the furnace to obtain a long-life electric furnace cover.

[0036] The long-life electric furnace cover prepared in this embodiment has the following test results: bulk density 2.90g / cm3; flexural strength 28MPa at 110℃×24 hours, compressive strength 66MPa; flexural strength retention rate 75% after 1100℃ water cooling 5 times; and excellent resistance to slag erosion.

[0037] Example 3

[0038] A long-life electric furnace cover and a preparation method thereof, comprising the following steps: (1) uniformly mixing 80% of silicon carbide particles and 20% of vanadium-containing steel slag powder according to mass percentage to obtain granulated material;

[0039] (2) granulating the granulated material obtained in step (1), drying the obtained material particles at 80° C. for 8 hours, then heat-treating the material particles at 800° C. for 1 hour, and sieving the material particles to obtain composite silicon carbide granulated materials with a particle size of 1-0 mm;

[0040] (3) 37% of 8-1 mm mullite particles, 20% of 3-1 mm plate-shaped corundum, 15% of 1-0 mm plate-shaped corundum, 3% of silicon carbide particles, 5% of composite silicon carbide granules, 3% of fused white corundum powder, 9% of corundum micropowder, 4% of silicon micropowder, 0.5% of explosion-proof fiber, 0.5% of sodium hexametaphosphate, 3% of calcium aluminate cement, and 7% of water were mixed uniformly by mass percentage, poured into a mold and vibrated to form;

[0041] (4) After natural curing for 24 hours with the mold, the mold is demoulded, and then the mold is naturally cured for 2 days, baked at 250°C for 40 hours, and cooled to room temperature with the furnace to obtain a long-life electric furnace cover.

[0042] The long-life electric furnace cover prepared in this embodiment has been tested to have the following characteristics: bulk density of 2.83 g / cm3; flexural strength of 22 MPa and compressive strength of 58 MPa at 110°C for 24 hours; flexural strength retention of 65% after 5 cycles of water cooling at 1100°C; and excellent resistance to slag erosion.

[0043] Example 4

[0044] A long-life electric furnace cover and a preparation method thereof, comprising the following steps: (1) uniformly mixing 80% of silicon carbide particles and 20% of vanadium-containing steel slag powder according to mass percentage to obtain granulated material;

[0045] (2) granulating the granulated material obtained in step (1), drying the obtained material particles at 80° C. for 5 hours, then heat-treating the material particles at 600° C. for 2 hours, and sieving the material particles to obtain composite silicon carbide granulated materials with a particle size of 1-0 mm;

[0046] (3) 38% of 8-1 mm mullite particles, 22% of 3-1 mm plate-shaped corundum, 16% of 1-0 mm plate-shaped corundum, 1% of silicon carbide particles, 3% of composite silicon carbide granules, 3% of fused white corundum powder, 9% of corundum micropowder, 4% of silicon micropowder, 0.5% of explosion-proof fiber, 0.5% of sodium hexametaphosphate, 3% of calcium aluminate cement, and 6% of water were mixed uniformly by mass percentage, poured into a mold and vibrated to form;

[0047] (4) After natural curing for 24 hours with the mold, the mold is demoulded, and then naturally cured for 3 days, baked at 200°C for 30 hours, and cooled to room temperature with the furnace to obtain a long-life electric furnace cover.

[0048] The long-life electric furnace cover prepared in this embodiment has been tested to have the following characteristics: bulk density of 2.84 g / cm3; flexural strength of 26 MPa at 110°C for 24 hours, and compressive strength of 65 MPa; flexural strength retention of 63% after 5 cycles of water cooling at 1100°C; and excellent resistance to slag erosion.

[0049] The foregoing descriptions of specific exemplary embodiments of the present invention are for purposes of illustration and description. These descriptions are not intended to limit the invention to the precise forms disclosed, and it is apparent that many variations and modifications are possible in light of the foregoing teachings. The exemplary embodiments have been selected and described for the purpose of explaining the specific principles of the invention and their practical application, thereby enabling those skilled in the art to realize and utilize a variety of exemplary embodiments of the invention and various options and modifications. The scope of the invention is intended to be defined by the claims and their equivalents.

Claims

1. A long-life electric furnace cover, characterized in that: (1) 60-80% of silicon carbide particles and 20-40% of vanadium-containing steel slag powder are uniformly mixed according to mass percentage to obtain a granulated material; (2) granulating the granulated material obtained in step (1), drying the obtained material particles at 70-90° C. for 5-10 hours, then heat treating the material particles at 600-800° C. for 1-3 hours, and sieving the material particles to obtain composite silicon carbide granulated materials with a particle size of 1-0 mm; (3) 20-40% of 8-1 mm mullite particles, 15-25% of 3-1 mm plate-shaped corundum, 15-25% of 1-0 mm plate-shaped corundum, 1-3% of silicon carbide particles, 3-5% of composite silicon carbide granules, 1-5% of fused white corundum powder, 5-10% of corundum micropowder, 1-5% of silicon micropowder, 0.2-0.6% of explosion-proof fiber, 0.5-1% of water reducer, 1-3% of calcium aluminate cement, and 4-7% of water are mixed uniformly by mass percentage, poured into a mold and vibrated to form; (4) After natural curing for 24 hours with the mold, the mold is demolded, and then naturally cured for 2-3 days, baked at 200-250°C for 30-40 hours, and cooled to room temperature with the furnace to obtain a long-life electric furnace cover.

2. The long-life electric furnace cover according to claim 1, characterized in that: The particle size of the silicon carbide particles is less than 0.5 mm, and the mass percentage of silicon carbide in the silicon carbide particles is ≥97.0%.

3. The long-life electric furnace cover according to claim 1 is characterized in that: The particle size of the vanadium-containing steel slag powder is less than 45 microns, and its components are as follows: V2O5 is 1.5-3%, SiO2<13%, and CaO is 35-40%.

4. The long-life electric furnace cover according to claim 1 is characterized in that: The mass percentage of Al2O3 in the mullite particles is greater than 70.0%, and the mass percentage of Fe2O3 is less than 1.0%.

5. The long-life electric furnace cover according to claim 1, characterized in that: The mass percentage of Al2O3 in plate-like corundum is greater than 99%.

6. The long-life electric furnace cover according to claim 1, characterized in that: The particle size of the fused white corundum powder is ≤0.088 mm, and the mass percentage of Al2O3 in the fused white corundum powder is greater than 99%.

7. The long-life electric furnace cover according to claim 1, characterized in that: The particle size of the corundum micropowder is ≤0.002 mm, and the mass percentage of Al2O3 in the corundum micropowder is ≥99.5%.

8. The long-life electric furnace cover according to claim 1, characterized in that: The particle size of the silicon micropowder is ≤0.005 mm, and the mass percentage of SiO2 in the silicon micropowder is ≥94wt%.

9. The long-life electric furnace cover according to claim 1, characterized in that: The water reducing agent is sodium tripolyphosphate or sodium hexametaphosphate.

10. The long-life electric furnace cover according to claim 1, characterized in that: The particle size of calcium aluminate cement is ≤0.044 mm, and the mass percentage of Al2O3 in the calcium aluminate cement is ≥75%.

Citation Information

Patent Citations

  • Vanadium iron slag runner castable

    CN103145435A

  • Alumina electric furnace cover and preparation method thereof

    CN104355634A

  • Corundum electric furnace cover

    CN107032808A

  • High-performance electric furnace cover

    CN107162610A

  • Nano Al2O3-SiC composite powder, low-carbon pouring steel ladle sliding plate brick and preparation methods of nano Al2O3-SiC composite powder and low-carbon pouring steel ladle sliding plate brick

    CN114105659A