Silicon carbide-based composite ceramic coating and slurry sintering preparation method and application thereof
By setting the mullite base layer and the high-entropy rare earth silicate composite surface layer on the silicon carbide base layer, the problem of oxidation and water vapor reaction in a high-temperature combustion environment is solved, and the high-temperature service reliability and stability of silicon carbide is achieved , improves the service life of the burner.
Patent Information
- Application Number
- CN202411011336.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The oxidation and water vapor reaction of silicon carbide porous ceramics in high-temperature combustion environments lead to the formation of SiO2. The highly volatile Si(OH)4 affects its service life, limiting its application in medium and high-temperature industries.
The mullite base layer and a composite surface layer of high entropy rare earth silicate are arranged on the silicon carbide base layer, and the coating is prepared by slurry sintering method, which utilizes the chemical stability of mullite and the high-temperature water-oxygen corrosion resistance of rare earth silicates. , combined with the phase structural stability of high-entropy rare earth silicates, a coating system that resists thermal shock and water oxygen corrosion is formed.
It realizes the reliability and stability of high-temperature service of silicon carbide above 1300℃, improves the retention rate of mechanical properties, extends the service life of the burner, and is suitable for high-temperature water-oxygen corrosion environments.
Smart Images

Figure CN118955180A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous medium combustion, and in particular to a silicon carbide-based composite ceramic coating and a slurry sintering preparation method and application thereof. Background Art
[0002] Porous media combustion technology is a combustion technology that achieves ultra-low pollutant emissions and stable combustion. As its core component, the porous media combustion plate needs to have excellent thermal shock resistance and high-temperature oxidation resistance. Compared with other materials, silicon carbide porous ceramics have the advantages of low thermal expansion coefficient, high thermal conductivity and emissivity, and excellent thermal shock resistance. It is the first choice for porous media burners. However, silicon carbide porous ceramics face dual oxidation from high-temperature water vapor and combustion-supporting gas in the combustion environment. The SiO2 generated by the oxidation of silicon carbide reacts with water vapor to generate highly volatile Si(OH)4, which seriously affects the service life of silicon carbide.
[0003] Therefore, porous media materials have become the main bottleneck restricting the widespread application of porous media burners in medium and high temperature industries.
[0004] Applying a high-temperature water-oxygen corrosion-resistant coating on the surface of silicon carbide can isolate the substrate from the corrosive environment, which is an effective way to improve the surface stability of silicon carbide in the combustion environment. In addition, the coating can also increase the service temperature of the burner, meet its use requirements under different working conditions, and extend the service life of the burner.
[0005] Therefore, it is necessary to develop silicon carbide-based coatings that can meet the requirements of medium and high temperature fields and improve the application prospects of porous media materials. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a silicon carbide-based composite ceramic coating and a slurry sintering preparation method and application thereof. The present invention arranges a mullite base layer and a high-entropy rare earth silicate composite surface layer in sequence on a silicon carbide base layer, thereby providing a coating system that has good bonding with a silicon carbide substrate and excellent thermal shock resistance and water-oxygen corrosion resistance in a high-temperature environment above 1300°C, thereby improving the service reliability and stability of silicon carbide in a high-temperature gas environment, and can effectively improve the mechanical property retention rate of silicon carbide at high temperatures.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a silicon carbide-based composite ceramic coating, the silicon carbide-based composite ceramic coating comprising a mullite base layer disposed on the surface of silicon carbide, and a high-entropy rare earth silicate composite surface layer located on the mullite base layer; the high-entropy rare earth silicate composite surface layer comprises a main phase and a second phase, the main phase is a high-entropy rare earth monosilicate, and the second phase is a high-entropy rare earth disilicate;
[0009] The mullite base layer includes a mullite phase and amorphous silicon dioxide.
[0010] The design concept of the present invention is that mullite and silicon carbide substrate have similar thermal expansion coefficients and chemical compatibility, and have excellent chemical stability and high-temperature oxidation resistance. Therefore, the mullite bottom layer can isolate the surface layer from the substrate and block the diffusion of elements between the coating and the substrate under the premise of ensuring the overall performance of the coating. However, the activity of silicon dioxide in mullite is relatively strong. In a water-oxygen environment, SiO2 will react with water vapor to generate volatile Si(OH)4, resulting in holes in the coating. Rare earth silicate ceramics have good resistance to high-temperature water-oxygen corrosion. However, the structural stability of single-component rare earth silicates in a long-term, high-temperature environment is poor, and rare earth disilicates are prone to crystal transformation and abnormal grain growth, while rare earth monosilicates are prone to react with SiO2 to generate rare earth disilicates, and there are problems such as a large thermal expansion coefficient and mismatch with mullite. Cracks appear during the start-stop process of cyclic combustion, resulting in coating failure.
[0011] High entropy materials are a type of multicomponent solid solution formed by five or more components, which have high entropy effect, hysteresis diffusion effect, lattice distortion effect and "cocktail effect". Compared with single-component rare earth silicates, high entropy rare earth silicates have better phase structure stability due to their high configuration entropy. In order to make high entropy rare earth silicates have a thermal expansion coefficient that matches that of the mullite substrate and better resistance to high-temperature water and oxygen corrosion, the present invention is designed to combine high entropy rare earth monosilicates with and high entropy rare earth disilicates By compounding, a high-entropy rare earth silicate composite ceramic coating with excellent resistance to high-temperature water-oxygen corrosion and thermal shock performance is prepared, thereby realizing the large-scale application of silicon carbide-based porous ceramic burners above 1300°C.
[0012] Preferably, the content of amorphous silicon dioxide in the mullite base layer is 5 to 20%, for example, it can be 5%, 7%, 9%, 10%, 12%, 14%, 15%, 17%, 19% or 20%, but is not limited to the listed values. Other unlisted values within this range are also applicable, preferably 5 to 10%.
[0013] The present invention further preferably has a non-crystalline silicon dioxide content of 5-20% in the mullite bottom layer, which can better improve the adhesion with the substrate and ensure the density of the mullite bottom layer.
[0014] Preferably, the content of high entropy rare earth disilicate in the high entropy rare earth silicate composite surface layer is 10-25%, for example, it can be 10%, 12%, 14%, 15%, 17%, 19%, 20%, 22%, 24% or 25%, etc., but is not limited to the listed values. Other unlisted values within this range are also applicable, preferably 10-20%.
[0015] The present invention further preferably contains 10-25% high entropy rare earth disilicate in the high entropy rare earth silicate composite surface layer, which has a thermal expansion coefficient more matching that of the mullite bottom layer, thereby simultaneously improving its high temperature water oxygen corrosion resistance and thermal shock resistance.
[0016] Preferably, the chemical formula of the high entropy rare earth monosilicate is The chemical formula of the high entropy rare earth disilicate is Among them, RE i Each is any one of the rare earth elements Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu, n≥5 and 1≤i≤n.
[0017] Preferably, the thickness of the mullite base layer is 50 to 200 μm, for example, it can be 50 μm, 67 μm, 84 μm, 100 μm, 117 μm, 134 μm, 150 μm, 167 μm, 184 μm or 200 μm, but is not limited to the listed values, and other values not listed within the range are equally applicable; the thickness of the high-entropy rare earth silicate composite surface layer is 100 to 200 μm, for example, it can be 100 μm, 112 μm, 123 μm, 134 μm, 145 μm, 156 μm, 167 μm, 178 μm, 189 μm or 200 μm, but is not limited to the listed values, and other values not listed within the range are equally applicable.
[0018] Preferably, the density of the mullite base layer is 96% to 99%, for example, it can be 96%, 96.2%, 96.5%, 96.6%, 96.8%, 97%, 97.2%, 97.5%, 97.8%, 98%, 98.2%, 98.5%, 98.8% or 99%, etc.
[0019] In a second aspect, the present invention provides a slurry sintering preparation method of the silicon carbide-based composite ceramic coating according to the first aspect, the slurry sintering preparation method comprising:
[0020] (1) The silicon carbide substrate is immersed in the mullite base slurry, and the excess slurry is removed and dried.
[0021] (2) repeating step (1) at least once to obtain a mullite coating precursor;
[0022] (3) The mullite coating precursor in step (2) is subjected to a first calcination and a first cooling to obtain a first silicon carbide ceramic material containing a mullite bottom layer;
[0023] (4) Step (3) The first silicon carbide ceramic material is immersed in a high entropy rare earth silicate composite surface layer slurry, and then the excess slurry is removed and dried;
[0024] (5) repeating step (4) at least once to obtain a high-entropy rare earth silicate composite ceramic precursor material;
[0025] (6) The high-entropy rare earth silicate composite ceramic precursor material in step (5) is subjected to a second calcination and a second cooling to obtain a silicon carbide ceramic containing a silicon carbide-based composite ceramic coating.
[0026] The invention utilizes a slurry sintering method to prepare a mullite coating and a high-entropy rare earth silicate composite ceramic coating on the surface of a silicon carbide-based ceramic. The method has the advantages of being simple and easy to operate, requiring little investment in one-time equipment, and being suitable for large-scale production.
[0027] Preferably, the raw materials of the mullite base slurry include 250-450 mesh andalusite powder, 700-900 mesh corundum powder and 7500-9500 mesh silica powder.
[0028] It is worth noting that currently, high temperature environment barrier coatings are generally prepared by plasma spraying, but this method has high requirements on equipment and is costly. The present invention optimizes the particle size ratio of the main powder in the mullite base slurry, and forms a mullite base with excellent bonding on the surface of the silicon carbide substrate by slurry sintering, and then further forms a surface layer by impregnating a high entropy rare earth silicate composite surface layer slurry, which can further improve the phase stability of rare earth silicate and the corrosion resistance in a high temperature water and oxygen environment.
[0029] The study found that when the particle size of each component is too large, the coating after sintering has more pores and low oxygen permeability; when the powder particle size is ball-milled to a particle size of about 7500-8000 mesh, the coating after sintering is too dense and has no stress release space, and the coating shrinks and has cracks, and cannot completely cover the silicon carbide substrate; only when the components of andalusite powder, corundum powder and silica powder are compounded according to the above-mentioned particle size requirements, the coating after sintering has moderate porosity and appropriate space to release stress, is not easy to crack in a high-temperature combustion environment, and does not shrink. It can better cover the silicon carbide substrate and play an anti-oxidation protective role.
[0030] Specifically, the andalusite powder of 250-450 mesh can be, for example, 250 mesh, 273 mesh, 295 mesh, 317 mesh, 339 mesh, 362 mesh, 384 mesh, 406 mesh, 428 mesh or 450 mesh, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0031] The corundum powder of 700-900 mesh can be, for example, 700 mesh, 723 mesh, 745 mesh, 767 mesh, 789 mesh, 812 mesh, 834 mesh, 856 mesh, 878 mesh or 900 mesh, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0032] The silica powder of 7500-9500 mesh can be, for example, 7500 mesh, 7723 mesh, 7945 mesh, 8167 mesh, 8389 mesh, 8612 mesh, 8834 mesh, 9056 mesh, 9278 mesh or 9500 mesh, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0033] Preferably, the preparation of the mullite base slurry includes: subjecting an andalusite raw material with a particle size of 250 to 450 meshes to a first ball milling to obtain andalusite powder; mixing andalusite powder, corundum powder, silica powder, a first binder, a first curing agent, a first dispersant and ethanol, performing a second ball milling and sieve filtering to obtain the mullite base slurry.
[0034] The present invention preferably ball-mills the andalusite raw material, and matches the powder particle sizes with the corundum powder and the silicon dioxide powder, so as to ensure that the coating has moderate porosity and can improve the oxygen penetration resistance, and avoid the problem of the coating being too dense and having no stress release space. Finally, it is not easy to crack in a high-temperature combustion environment, and the coating does not shrink, and can better cover the silicon carbide substrate to play an anti-oxidation protective role.
[0035] Preferably, the mass ratio of andalusite powder:corundum powder:silicon dioxide powder:first binder:first curing agent:first dispersant:ethanol is (40-70):(10-30):(2-10):(20-60):(1-6):(2-10):(30-70).
[0036] Specifically, the andalusite powder is 40-70, for example, it can be 40, 44, 47, 50, 54, 57, 60, 64, 67 or 70, but is not limited to the listed values, and other values not listed in the range are also applicable; the corundum powder is 10-30, for example, it can be 10, 13, 15, 17, 19, 22, 24, 26, 28 or 30, but is not limited to the listed values, and other values not listed in the range are also applicable; the silicon dioxide powder is 2-10, for example, it can be 2, 2.9, 3.8, 4.7, 5.6, 6.5, 7.4, 8.3, 9.2 or 10, but is not limited to the listed values, and other values not listed in the range are also applicable; the first binder is 20-60, for example, it can be 20, 25, 29, 34, 38, 43, 47, 52, 56 or 60, etc., but not limited to the listed values, and other values not listed in the range are equally applicable; the first curing agent 1-6, for example, can be 1, 1.6, 2.2, 2.7, 3.3, 3.8, 4.4, 4.9, 5.5 or 6, etc., but not limited to the listed values, and other values not listed in the range are equally applicable; the first dispersant 2-10, for example, can be 2, 2.9, 3.8, 4.7, 5.6, 6.5, 7.4, 8.3, 9.2 or 10, etc., but not limited to the listed values, and other values not listed in the range are equally applicable; ethanol 30-70, for example, can be 30, 35, 39, 44, 48, 53, 57, 62, 66 or 70, etc., but not limited to the listed values, and other values not listed in the range are equally applicable.
[0037] Preferably, the first ball milling is performed in a jar mill.
[0038] Preferably, the rotation speed of the first ball mill is 180-220 r / min, for example, it can be 180 r / min, 185 r / min, 189 r / min, 194 r / min, 198 r / min, 203 r / min, 207 r / min, 212 r / min, 216 r / min or 220 r / min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0039] Preferably, the first ball milling time is 24 to 48 hours, for example, it can be 24 hours, 27 hours, 30 hours, 32 hours, 35 hours, 38 hours, 40 hours, 43 hours, 46 hours or 48 hours, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0040] Preferably, the particle size of the andalusite after the first ball milling is 1000-5000 mesh, for example, it can be 1000 mesh, 1200 mesh, 1300 mesh, 1400 mesh, 1500 mesh, 1600 mesh, 1700 mesh, 1800 mesh, 2000 mesh, 2200 mesh, 2300 mesh, 2500 mesh, 2800 mesh, 3000 mesh, 3200 mesh, 3500 mesh, 4000 mesh, 4500 mesh or 5000 mesh, etc.
[0041] The particle size range of the andalusite after the first ball milling of the present invention is distributed within the above range, so that the andalusite after ball milling can be better combined with other raw materials, and finally the thermal shock resistance and oxidation corrosion resistance of the silicon carbide-based composite ceramic coating are comprehensively improved.
[0042] Preferably, the second ball milling time is 6 to 24 hours, for example, it can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0043] Preferably, the rotation speed of the second ball mill is 180-220 r / min, for example, it can be 180 r / min, 185 r / min, 189 r / min, 194 r / min, 198 r / min, 203 r / min, 207 r / min, 212 r / min, 216 r / min or 220 r / min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0044] Preferably, the mesh size of the sieve filtration in step (1) is 100 to 200 meshes, for example, it can be 100 mesh, 112 mesh, 123 mesh, 134 mesh, 145 mesh, 156 mesh, 167 mesh, 178 mesh, 189 mesh or 200 mesh, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0045] Preferably, the removal of excess slurry in step (1) comprises centrifugation and purging performed sequentially.
[0046] Preferably, the drying in step (1) includes oven drying.
[0047] Preferably, the drying temperature in step (1) is 80-120°C, for example, it can be 80°C, 85°C, 89°C, 94°C, 98°C, 103°C, 107°C, 112°C, 116°C or 120°C, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0048] Preferably, the number of repetitions in step (2) is 1 to 5 times, for example, 1 time, 2 times, 3 times, 4 times or 5 times.
[0049] Preferably, the temperature of the first calcination in step (3) is 1500-1600°C, for example, it can be 1500°C, 1512°C, 1523°C, 1534°C, 1545°C, 1556°C, 1567°C, 1578°C, 1589°C or 1600°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0050] Preferably, the first calcination time in step (3) is 3 to 10 hours, for example, 3 hours, 3.8 hours, 4.6 hours, 5.4 hours, 6.2 hours, 6.9 hours, 7.7 hours, 8.5 hours, 9.3 hours or 10 hours, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0051] Preferably, the preparation of the high entropy rare earth silicate composite surface slurry in step (4) comprises:
[0052] The high entropy rare earth monosilicate powder, the high entropy rare earth disilicate powder, the second binder, the second curing agent, the second dispersant and ethanol are mixed, and the mixture is subjected to a third ball milling and sieve filtering to obtain the high entropy rare earth silicate composite surface layer slurry.
[0053] Preferably, the mass ratio of the high entropy rare earth monosilicate powder, the high entropy rare earth disilicate powder, the second binder, the second curing agent, the second dispersant and ethanol is (70-90):(10-30):(20-60):(1-6):(2-10):(30-70).
[0054] Specifically, the high entropy rare earth monosilicate powder is 70-90, for example, it can be 70, 73, 75, 77, 79, 82, 84, 86, 88 or 90, but is not limited to the listed values, and other values not listed in the range are also applicable; the high entropy rare earth disilicate powder is 10-30, for example, it can be 10, 13, 15, 17, 19, 22, 24, 26, 28 or 30, but is not limited to the listed values, and other values not listed in the range are also applicable; the second binder is 20-60, for example, it can be 20, 25, 29, 34, 38, 43, 47, 52, 56 or 60, but is not limited to the listed values, and other values not listed in the range are also applicable. The same applies; the second curing agent 1-6, for example, can be 1, 1.6, 2.2, 2.7, 3.3, 3.8, 4.4, 4.9, 5.5 or 6, but is not limited to the listed values, and other values not listed within the range are also applicable; the second dispersant 2-10, for example, can be 2, 2.9, 3.8, 4.7, 5.6, 6.5, 7.4, 8.3, 9.2 or 10, but is not limited to the listed values, and other values not listed within the range are also applicable; ethanol 30-70, for example, can be 30, 35, 39, 44, 48, 53, 57, 62, 66 or 70, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0055] Preferably, the rotation speed of the third ball mill is 180-220 r / min, for example, it can be 180 r / min, 185 r / min, 189 r / min, 194 r / min, 198 r / min, 203 r / min, 207 r / min, 212 r / min, 216 r / min or 220 r / min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0056] Preferably, the third ball milling time is 6 to 24 hours, for example, it can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0057] Preferably, the mesh size of the sieve filtration in step (4) is 100 to 200 meshes, for example, it can be 100 mesh, 112 mesh, 123 mesh, 134 mesh, 145 mesh, 156 mesh, 167 mesh, 178 mesh, 189 mesh or 200 mesh, but is not limited to the listed values, and other values not listed within the range are also applicable.
[0058] Preferably, the preparation process of the high entropy rare earth monosilicate powder and the high entropy rare earth disilicate powder each independently comprises:
[0059] S1, the rare earth oxide and the third dispersant are mixed and subjected to a fourth ball milling to form a precursor slurry.
[0060] S2, the precursor slurry is dried and sieved in sequence and then sintered to obtain high entropy rare earth silicate particles;
[0061] S3, the high entropy rare earth silicate particles are subjected to a fifth ball milling and sieving in air to obtain high entropy rare earth silicate powder;
[0062] Preferably, the rare earth oxide satisfies the chemical formula of high entropy rare earth monosilicate particles, and the molar ratio of RE:Si:O is 1:2:5, or the rare earth oxide satisfies the chemical formula of high entropy rare earth disilicate particles, and the molar ratio of RE:Si:O is 2:2:7.
[0063] Preferably, the third dispersant comprises water and / or ethanol.
[0064] Preferably, the fourth ball milling time is 6 to 24 hours, for example, it can be 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0065] Preferably, the rotation speed of the fourth ball mill is 300-400 r / min, for example, it can be 300 r / min, 310 r / min, 320 r / min, 330 r / min, 340 r / min, 345 r / min, 350 r / min, 360 r / min, 380 r / min, 390 r / min or 400 r / min, etc.
[0066] Preferably, the heating rate of the sintering synthesis is 5 to 10°C / min, for example, it can be 5°C / min, 5.6°C / min, 6.2°C / min, 6.7°C / min, 7.3°C / min, 7.8°C / min, 8.4°C / min, 8.9°C / min, 9.5°C / min or 10°C / min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0067] Preferably, the synthesis temperature of the sintering synthesis is 1500-1650°C, for example, it can be 1500°C, 1517°C, 1534°C, 1550°C, 1567°C, 1584°C, 1600°C, 1617°C, 1634°C or 1650°C, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0068] Preferably, the synthesis time of the sintering synthesis is 0.5 to 20 h, for example, it can be 0.5 h, 2.7 h, 4.9 h, 7 h, 9.2 h, 11.4 h, 13.5 h, 15.7 h, 17.9 h or 20 h, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0069] Preferably, the fifth ball milling time is 6 to 20 hours, for example, it can be 6 hours, 8 hours, 10 hours, 11 hours, 13 hours, 14 hours, 16 hours, 17 hours, 19 hours or 20 hours, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0070] Preferably, the rotation speed of the fifth ball mill is 300-400 r / min, for example, it can be 300 r / min, 312 r / min, 323 r / min, 334 r / min, 345 r / min, 356 r / min, 367 r / min, 378 r / min, 389 r / min or 400 r / min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0071] Preferably, the sieving in step S3 is through a 400-mesh sieve.
[0072] Preferably, the first binder and the second binder each independently include a resin having a residual carbon value greater than 35%, and the resin includes any one of epoxy resin, phenolic resin, polyacrylic resin, polyvinyl butyral, furfural resin or phenol furfural resin, or a combination of at least two thereof, wherein typical but non-limiting combinations are a combination of epoxy resin and phenolic resin, a combination of polyacrylic resin and phenolic resin, a combination of epoxy resin and polyacrylic resin, a combination of polyvinyl butyral and phenolic resin, and a combination of polyvinyl butyral and phenol furfural resin.
[0073] Preferably, the first curing agent and the second curing agent each independently include any one of citric acid, p-toluenesulfonic acid, pentosan or oxalic acid, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of citric acid and p-toluenesulfonic acid, a combination of oxalic acid and p-toluenesulfonic acid, a combination of citric acid and oxalic acid, and a combination of pentosan and p-toluenesulfonic acid.
[0074] Preferably, the first dispersant and the second dispersant each independently include any one of castor oil, triolein, Tween 20 or organobentonite, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of castor oil and triolein, a combination of Tween 20 and triolein, a combination of castor oil and Tween 20, a combination of organobentonite and triolein, and a combination of castor oil and organobentonite.
[0075] Preferably, the silicon carbide substrate has a porous structure, and the porous shape includes any one of a triangle, a triangle with rounded vertices, a circle, an ellipse, a regular polygon, a variant polygon or a graded polygon, or a combination of at least two of them, wherein a typical but non-limiting combination is a combination of a triangle and a triangle with rounded vertices, a combination of a circle and a triangle with rounded vertices, a combination of a triangle and an ellipse, a combination of a triangle and a regular polygon, a combination of a variant polygon and a regular polygon, and a combination of a graded polygon and a regular polygon.
[0076] In a third aspect, the present invention provides a silicon carbide-based composite ceramic coating as described in the first aspect for use in a porous medium burner in a medium to high temperature range, wherein the temperature in the medium to high temperature range is preferably ≥ 1300°C.
[0077] The silicon carbide-based composite ceramic coating provided in the first aspect of the present invention has excellent performance, strong thermal shock resistance and high-temperature water-oxygen corrosion resistance, and can be effectively used in fields with temperatures ≥1300°C.
[0078] Compared with the prior art, the present invention has at least the following beneficial effects:
[0079] (1) The silicon carbide-based composite ceramic coating provided by the present invention uses andalusite, white corundum and nano-SiO2 as raw materials, and the prepared mullite contains a part of SiO2 glass phase, which can improve the density of the mullite coating and the adhesion to the substrate.
[0080] (2) The high-entropy rare earth silicate of the silicon carbide-based composite ceramic coating provided by the present invention has a high configurational entropy, which can further improve the phase stability of the rare earth silicate and the corrosion resistance in a high-temperature water-oxygen environment; and through the composite of high-entropy rare earth disilicate and high-entropy rare earth monosilicate, it has a thermal expansion coefficient that is more matched with the mullite bottom layer, thereby simultaneously improving its high-temperature water-oxygen corrosion resistance and thermal shock resistance. Under preferred conditions, it can achieve more than 30 times at 1500°C without cracks, and the oxidation weight gain rate is within 0.782%, which can better meet the burner's requirements for high-temperature water-oxygen corrosion resistance at more than 1300°C;
[0081] (3) The preparation method of the silicon carbide-based composite ceramic coating provided by the present invention utilizes a slurry sintering method to prepare a mullite coating and a high-entropy rare earth silicate composite ceramic coating on the surface of a silicon carbide-based ceramic. This method has the advantages of being simple and easy to operate, requiring little investment in one-time equipment, and being suitable for large-scale production, and can achieve an excellent combination of the coating and the substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0082] Figure 1 This is the surface XRD spectrum of the silicon carbide-based composite ceramic coating prepared in Example 2 of the present invention.
[0083] Figure 2This is a SEM element analysis diagram of the mullite bottom layer prepared in Example 2 of the present invention.
[0084] Figure 3 is a SEM image of andalusite after ball milling in Example 1 of the present invention.
[0085] Figure 4 3 is a SEM image of the mullite bottom layer prepared in Example 1 of the present invention.
[0086] Figure 5 is a SEM image of the andalusite without ball milling in Example 4 of the present invention.
[0087] Figure 6 3 is a SEM image of the mullite bottom layer prepared in Example 4 of the present invention.
[0088] Figure 7 is a SEM image of andalusite after ball milling in Example 5 of the present invention.
[0089] Figure 8 3 is a SEM image of the mullite bottom layer prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0090] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0091] It should be understood that, in the description of the present invention, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Thus, a feature defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "plurality" means two or more.
[0092] Example 1
[0093] This embodiment provides a method for preparing a silicon carbide-based composite ceramic coating, the preparation method comprising the following steps:
[0094] S1, Preparation of mullite base layer
[0095] S1.1, prepare mullite base slurry:
[0096] The andalusite raw material with a particle size of 250 mesh was first ball-milled in a pot mill at 180 r / min for 48 h to obtain andalusite powder with a particle size of 1200-3000 mesh;
[0097] The materials were uniformly mixed in a mass ratio of andalusite powder: corundum powder: silica powder: first binder: first curing agent: first dispersant: ethanol = 70:20:10:20:4:6:50, ball milled in a pot mill at 200 r / min for 10 h, and filtered through a 200-mesh sieve to obtain a mullite bottom layer slurry;
[0098] The particle size of the corundum powder is 200 mesh, and the particle size of the silicon dioxide powder is 8000 mesh; the first binder is a resin with a residual carbon value greater than 35%, and the resin is a mixture of epoxy resin (specific brand: E-20) and polyacrylic resin (specific brand: PPB-MP-300-M), and the mass ratio is epoxy resin: polyacrylic resin = 1:1; the first curing agent is p-toluenesulfonic acid; the first dispersant is triolein;
[0099] S1.2, slurry coating and curing: immerse the silicon carbide skeleton with a porous structure into the mullite bottom slurry. After the immersion is complete, take it out and centrifuge it to remove the excess slurry, and use compressed air to blow it evenly. The pressure of the compressed air is 0.5MPa, and it is dried and cured at 100℃ to obtain a porous structure skeleton with a primary bottom slurry coating;
[0100] Repeat the above step S1.2 5 times to obtain a mullite coating precursor;
[0101] S1.3, heat treatment: heat-treat the mullite bottom layer precursor at 1500° C. for 4 hours, and after cooling to room temperature, obtain a first silicon carbide ceramic material containing a mullite bottom layer.
[0102] S2, Preparation of high entropy ytterbium silicate composite ceramic coating
[0103] S2.1, preparation of high entropy rare earth silicate composite surface slurry:
[0104] S2.1.1, 6.73g of neodymium oxide, 7.25g of gadolinium oxide, 7.46g of dysprosium oxide, 7.65g of erbium oxide, 7.88g of ytterbium oxide and 12.02g of silicon oxide were mixed and evenly put into an agate ball mill, and anhydrous ethanol was added as a medium, and the ball milling was carried out at 350r / min for 12 hours. The dried powder was subjected to pressureless sintering synthesis in a muffle furnace. The parameters are as follows: the temperature was raised to 1550°C at a rate of 10°C / min, and the temperature was kept for 4 hours. After the reaction was completed, the high-entropy rare earth monosilicate particles were obtained; the high-entropy rare earth monosilicate particles were ball milled at 350r / min for 12 hours in air and sieved to obtain high-entropy rare earth monosilicate powder, the particle size of which was 350 mesh and the purity was greater than 99.9%.
[0105] S2.1.2, 6.73g of neodymium oxide, 7.25g of gadolinium oxide, 7.46g of dysprosium oxide, 7.65g of erbium oxide, 7.88g of ytterbium oxide and 6g of silicon oxide were mixed and evenly put into an agate ball mill, and anhydrous ethanol was added as a medium, and the ball mill was carried out at 350r / min for 12 hours. The dried powder was subjected to pressureless sintering synthesis in a muffle furnace. The parameters are as follows: the temperature was raised to 1550°C at a rate of 10°C / min, and the temperature was kept for 4 hours. After the reaction was completed, the high-entropy rare earth double silicate particles were obtained; the high-entropy rare earth double silicate particles were ball milled at 350r / min for 12 hours in air and sieved to obtain high-entropy rare earth double silicate powder, the particle size of the high-entropy rare earth double silicate powder was 350 mesh, and the purity was greater than 99.9%.
[0106] S2.1.3, according to the mass ratio of high entropy rare earth monosilicate powder: high entropy rare earth disilicate powder: second binder: second curing agent: second dispersant: ethanol = 80:20:30:2:8:60, the materials are uniformly mixed, ball milled at 200 r / min for 12 h, and filtered through a 200 mesh sieve to obtain a surface layer slurry;
[0107] The second binder is a resin with a residual carbon value greater than 35%, the resin is an alcohol-soluble phenolic resin (specific brand: FQ-9), the second curing agent is p-toluenesulfonic acid; and the second dispersant is organic bentonite.
[0108] S2.2, slurry coating and curing: immerse the first silicon carbide ceramic material in the high entropy rare earth silicate composite surface slurry, remove excess slurry, and use compressed air to blow it evenly. The pressure of the compressed air is 0.5MPa, and the material is dried and cured at 80°C to obtain a porous structural skeleton of the primary surface slurry coating;
[0109] Repeat the above step S2.2 three times to obtain a high-entropy rare earth silicate composite ceramic precursor material.
[0110] S2.3, heat treatment: heat-treat the high-entropy rare earth silicate composite ceramic precursor material at 1550° C. for 3 hours, and after cooling to room temperature, obtain a silicon carbide ceramic material coated with a mullite-high-entropy rare earth silicate composite material.
[0111] Thermal shock test: first heat the muffle furnace to 1500℃, then put the silicon carbide ceramic material coated with mullite-high entropy rare earth silicate composite material, silicon carbide ceramic material coated with mullite-Yb2Si2O7, silicon carbide ceramic material coated with mullite-Yb2SiO5, silicon carbide ceramic material coated with mullite and uncoated samples into the furnace for 10 minutes, then take them out and soak them in cold water below 20℃ for 30 minutes, take them out and dry them, and observe whether there are cracks with a high-power microscope. If there are no cracks, continue the water-cooled thermal shock process. Repeat the thermal shock 50 times and observe the results.
[0112] Anti-oxidation performance test: Silicon carbide ceramic samples coated with mullite-high entropy rare earth silicate composite materials (size: 800mm×30mm×20mm, weight 18.59g), mullite-Yb2Si2O7 coated silicon carbide ceramic materials (size: 800mm×30mm×20mm), weight 17.25g), mullite-Yb2SiO5 coated silicon carbide ceramic materials (size: 800mm×30mm×20mm), weight 17.25g), mullite coated silicon carbide ceramic materials and uncoated silicon carbide ceramic materials (size: 800mm×30mm×20mm), weight 15.63g) were burned for 200h (working section frequency 42.08Hz, working wind opening 33.0%, working gas opening: 2.5%), and the oxidation weight gain rate was calculated.
[0113] The results are shown in Table 1.
[0114] Table 1
[0115]
[0116] Example 2
[0117] This embodiment provides a method for preparing a silicon carbide-based composite ceramic coating, the preparation method comprising the following steps:
[0118] S1, Preparation of mullite base layer
[0119] S1.1, prepare mullite base slurry:
[0120] The andalusite raw material with a particle size of 450 mesh was first ball-milled in a pot mill at 200 r / min for 30 h to obtain andalusite powder with a particle size of 2100-4500 mesh;
[0121] The materials were uniformly mixed in a mass ratio of andalusite powder: corundum powder: silica powder: first binder: first curing agent: first dispersant: ethanol = 45:10:2:20:4:6:60, ball milled in a pot mill at 200 r / min for 16 h, and filtered through a 100-mesh sieve to obtain a mullite bottom layer slurry;
[0122] The particle size of the corundum powder is 325 mesh, and the particle size of the silicon dioxide powder is 800 mesh; the first binder is a resin with a residual carbon value greater than 35%, and the resin is an acrylic resin (specific brand: BR-80); the first curing agent is citric acid; the first dispersant is triolein;
[0123] S1.2, slurry coating and curing: immerse the silicon carbide skeleton with a porous structure into the mullite bottom slurry. After the immersion is complete, take it out and centrifuge it to remove the excess slurry, and use compressed air to blow it evenly. The pressure of the compressed air is 0.5MPa, and it is dried and cured at 120℃ to obtain a porous structure skeleton with a primary bottom slurry coating;
[0124] Repeat the above step S1.2 three times to obtain a mullite coating precursor;
[0125] S1.3, heat treatment: heat-treat the mullite bottom layer precursor at 1550° C. for 3 hours, and after cooling to room temperature, obtain a first silicon carbide ceramic material containing a mullite bottom layer.
[0126] S2, Preparation of high entropy ytterbium silicate composite ceramic coating
[0127] S2.1, preparation of high entropy rare earth silicate composite surface slurry:
[0128] S2.1.1, 1.38g of scandium oxide, 2.26g of yttrium oxide, 3.83g of erbium oxide, 3.86g of thulium oxide, 3.94g of ytterbium oxide, 3.98g of lutetium oxide and 7.21g of silicon oxide were mixed and evenly put into an agate ball mill, and anhydrous ethanol was added as a medium, and the ball milling was carried out at 350r / min for 6 hours. The dried powder was subjected to pressureless sintering synthesis in a muffle furnace. The parameters are as follows: the temperature was raised to 1600℃ at a rate of 5℃ / min, and the temperature was kept for 2 hours. After the reaction was completed, the high-entropy rare earth monosilicate particles were obtained; the high-entropy rare earth monosilicate particles were ball milled at 400r / min for 10 hours in air and sieved to obtain high-entropy rare earth monosilicate powder, the particle size of the high-entropy rare earth monosilicate powder was 325 mesh, and the purity was greater than 99.9%.
[0129] S2.1.2, 1.38g of scandium oxide, 2.26g of yttrium oxide, 3.83g of erbium oxide, 3.86g of thulium oxide, 3.94g of ytterbium oxide, 3.98g of lutetium oxide and 3.61g of silicon oxide were mixed and evenly put into an agate ball mill, and anhydrous ethanol was added as a medium, and the ball milling was carried out at 350r / min for 6 hours. The dried powder was subjected to pressureless sintering synthesis in a muffle furnace. The parameters are as follows: the temperature was raised to 1600℃ at a rate of 5℃ / min, and the temperature was kept for 2 hours. After the reaction was completed, the high-entropy rare earth double silicate particles were obtained; the high-entropy rare earth double silicate particles were ball milled at 400r / min for 10 hours in air and sieved to obtain high-entropy rare earth double silicate powder, the particle size of the high-entropy rare earth double silicate powder was 325 mesh, and the purity was greater than 99.9%.
[0130] S2.1.3, according to the mass ratio of high entropy rare earth monosilicate powder: high entropy rare earth disilicate powder: second binder: second curing agent: second dispersant: ethanol = 90:10:40:6:5:40, the materials are uniformly mixed, ball milled at 220 r / min for 12 h, and filtered through a 200 mesh sieve to obtain a surface layer slurry;
[0131] The second binder is a resin with a residual carbon value greater than 35%, the resin is an alcohol-soluble phenolic resin (specific brand: 2123), the second curing agent is p-toluenesulfonic acid; and the second dispersant is organic bentonite.
[0132] S2.2, slurry coating and curing: immerse the first silicon carbide ceramic material in the high entropy rare earth silicate composite surface layer slurry, and after the immersion is complete, take it out and centrifuge it to remove the excess slurry, and use compressed air to blow it evenly. The pressure of the compressed air is 0.5MPa, and it is dried and cured at 80°C to obtain a porous structural skeleton of the primary surface slurry coating;
[0133] Repeat the above step S2.2 three times to obtain a high-entropy rare earth silicate composite ceramic precursor material.
[0134] S2.3, heat treatment: heat-treat the high-entropy rare earth silicate composite ceramic precursor material at 1475° C. for 4 hours, and after cooling to room temperature, obtain a silicon carbide ceramic material coated with a mullite-high-entropy rare earth silicate composite material.
[0135] The surface XRD spectrum of the silicon carbide ceramic material coated with mullite-high entropy rare earth silicate composite ceramic prepared in this embodiment is as follows: Figure 1 As shown in Figure 1, according to the diffraction pattern, it can be calculated that the rare earth ytterbium silicate composite coating is composed of 90 mol.% rare earth monosilicate phase and 10 mol.% rare earth disilicate phase. The SEM image of the mullite bottom layer is shown in Figure 1. Figure 2 As shown, the number 8 indicates an amorphous substance, indicating that the mullite bottom layer of this embodiment contains amorphous silicon dioxide, and the number 9 indicates a mullite phase. The silicon carbide ceramic material coated with mullite-rare earth silicate composite ceramic prepared in this embodiment is subjected to a thermal shock resistance test: first, the muffle furnace is heated to 1550°C, and then the silicon carbide ceramic material coated with mullite-high entropy rare earth silicate composite material, the silicon carbide ceramic material coated with mullite-Yb2SiO5 and the silicon carbide ceramic material without coating are placed in the furnace for insulation for 10 minutes, then taken out and immersed in cold water below 20°C for 30 minutes, taken out and dried, and observed with a high-power microscope to see if cracks appear. If there are no cracks, continue the cycle of water-cooled thermal shock process. Test results: 1550°C repeated thermal shock 30 times, no cracks were observed.
[0136] Anti-oxidation performance test: Silicon carbide ceramic material coated with mullite-high entropy rare earth silicate composite material (size: 800mm×30mm×20mm, weight 15.63g), mullite-Yb2SiO5 coated silicon carbide ceramic material (size: 800mm×30mm×20mm, weight 16.38g) and uncoated silicon carbide ceramic material (size: 800mm×30mm×20mm, weight 14.11g) were burned for 100h (working section frequency 40Hz, working wind opening 30%, working gas opening: 2.7%), and the oxidation weight gain rate was calculated.
[0137] Table 2
[0138]
[0139] Example 3
[0140] This embodiment provides a method for preparing a silicon carbide-based composite ceramic coating, the preparation method comprising the following steps:
[0141] S1, Preparation of mullite base layer
[0142] S1.1, prepare mullite base slurry:
[0143] The andalusite raw material with a particle size of 300 mesh was first ball-milled in a pot mill at 220 r / min for 24 h to obtain andalusite powder with a particle size of 1000-1800 mesh;
[0144] The materials were uniformly mixed in a mass ratio of andalusite powder: corundum powder: silica powder: first binder: first curing agent: first dispersant: ethanol = 60:15:2:50:4:8:60, ball-milled in a pot mill at 180 r / min for 24 h, and filtered through a 100-mesh sieve to obtain a mullite bottom layer slurry;
[0145] The particle size of the corundum powder is 325 mesh, and the particle size of the silicon dioxide powder is 800 mesh; the first binder is a resin with a residual carbon value greater than 35%, and the resin is an acrylic resin (brand ACR201); the first curing agent is oxalic acid; and the first dispersant is castor oil.
[0146] S1.2, slurry coating and curing: immerse the silicon carbide skeleton with a porous structure into the mullite bottom slurry. After the immersion is complete, take it out and centrifuge it to remove the excess slurry, and use compressed air to blow it evenly. The pressure of the compressed air is 0.5MPa, and it is dried and cured at 120℃ to obtain a porous structure skeleton with a primary bottom slurry coating;
[0147] Repeat the above step S1.2 three times to obtain a mullite coating precursor;
[0148] S1.3, heat treatment: heat-treat the mullite bottom layer precursor at 1525° C. for 4 hours, and after cooling to room temperature, obtain a first silicon carbide ceramic material containing a mullite bottom layer.
[0149] S2, Preparation of high entropy ytterbium silicate composite ceramic coating
[0150] S2.1, preparation of high entropy rare earth silicate composite surface slurry:
[0151] S2.1.1. Mix 10.09 g of neodymium oxide, 10.46 g of samarium oxide, 10.56 g of europium oxide, 10.88 g of gadolinium oxide, 11.19 g of dysprosium oxide, 11.34 g of holmium oxide, 11.48 g of erbium oxide, 11.58 g of thulium oxide and 28.84 g of silicon oxide, put them into an agate ball mill, add anhydrous ethanol as a medium, and ball mill at 300 r / min for 12 hours. The dried powder is synthesized by pressureless sintering in a muffle furnace. The parameters are as follows: heating to 1650° C. at a speed of 8° C. / min, keeping the temperature for 1 hour, cooling to room temperature with the furnace after the pressureless sintering synthesis is completed, and obtaining high-entropy rare earth monosilicate particles; the high-entropy rare earth monosilicate particles are ball-milled at 300 r / min for 12 hours in air and sieved to obtain high-entropy rare earth monosilicate powder, the particle size of the high-entropy rare earth monosilicate powder is 325 mesh, and the purity is greater than 99.9%.
[0152] S2.1.2. Mix 10.09 g of neodymium oxide, 10.46 g of samarium oxide, 10.56 g of europium oxide, 10.88 g of gadolinium oxide, 11.19 g of dysprosium oxide, 11.34 g of holmium oxide, 11.48 g of erbium oxide, 11.58 g of thulium oxide and 14.42 g of silicon oxide, and put them into an agate ball mill. Add anhydrous ethanol as a medium, and ball mill at 300 r / min for 12 hours. The dried powder is synthesized by pressureless sintering in a muffle furnace. The parameters are as follows: heating to 1650° C. at a speed of 8° C. / min, keeping the temperature for 1 hour, cooling to room temperature with the furnace after the reaction is completed, and obtaining high-entropy rare earth double silicate particles; the high-entropy rare earth double silicate particles are ball-milled at 300 r / min for 12 hours in air and sieved to obtain high-entropy rare earth double silicate powder, the particle size of the high-entropy rare earth double silicate powder is 325 mesh, and the purity is greater than 99.9%.
[0153] S2.1.3, according to the mass ratio of high entropy rare earth monosilicate powder: high entropy rare earth disilicate powder: second binder: second curing agent: second dispersant: ethanol = 70:10:50:2:8:55, the materials are uniformly mixed, ball milled at 200 r / min for 18 h, and filtered through a 200 mesh sieve to obtain a surface layer slurry;
[0154] The second binder is a resin with a residual carbon value greater than 35%, the resin is phenol furfural resin (specific brand F15), the second curing agent is pentosan, and the second dispersant is organic bentonite.
[0155] S2.2, slurry coating and curing: immerse the first silicon carbide ceramic material in the high entropy rare earth silicate composite surface slurry, and after the immersion is complete, take it out and centrifuge it to remove the excess slurry, and use compressed air to blow it evenly. The pressure of the compressed air is 0.5MPa, and it is dried and cured at 110°C to obtain a porous structural skeleton of the first surface slurry coating;
[0156] Repeat the above step S2.2 three times to obtain a high-entropy rare earth silicate composite ceramic precursor material.
[0157] S2.3, heat treatment: heat-treat the high-entropy rare earth silicate composite ceramic precursor material at 1550° C. for 2 hours, and after cooling to room temperature, obtain a silicon carbide ceramic material coated with a mullite-high-entropy rare earth silicate composite material.
[0158] The silicon carbide ceramic material coated with the mullite-rare earth silicate composite material prepared in this embodiment is subjected to a thermal shock resistance test: first, the muffle furnace is heated to 1600°C, and then the silicon carbide ceramic material coated with the mullite-rare earth silicate composite material, the silicon carbide ceramic material coated with mullite-90wt.% Yb2SiO5+10wt.% Yb2Si2O7, and the silicon carbide ceramic material without coating are placed in the furnace for 10 minutes of heat preservation, and then taken out and immersed in cold water below 20°C for 30 minutes, taken out and dried, and observed with a high-power microscope to see if cracks appear. If there are no cracks, continue the water-cooled thermal shock process. Repeat the thermal shock at 1600°C for 20 times.
[0159] Anti-oxidation performance test: Silicon carbide ceramic material coated with mullite-rare earth silicate composite material (size: 800mm×30mm×20mm, weight 20.18g), silicon carbide ceramic material coated with mullite-90wt.% Yb2SiO5+10wt.% Yb2Si2O7 (size: 800mm×30mm×20mm, weight 20.25g) and uncoated silicon carbide ceramic material (size: 800mm×30mm×20mm, weight 18.35g) were burned for 100h (working section frequency 41.8Hz, working wind opening 31.0%, working gas opening: 2.8%), and the oxidation weight gain rate was calculated.
[0160] The results are shown in Table 3.
[0161] Table 3
[0162]
[0163] Example 4
[0164] This embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method is the same as that of Embodiment 1, except that the andalusite raw material is not ball-milled and 250-mesh andalusite powder is directly used, and will not be described in detail here.
[0165] Example 5
[0166] This embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method is the same as that of Embodiment 1, except that the andalusite raw material is ball-milled to a particle size of 7500 meshes by a planetary ball mill, and will not be described in detail herein.
[0167] The SEM image of andalusite after ball milling in Example 1 is as follows Figure 3 As shown, the SEM image of the unmilled andalusite in Example 4 is as follows Figure 5 As shown, the SEM image of the andalusite after ball milling in Example 5 is as follows Figure 7 As shown, the SEM images of the mullite bottom layer finally obtained in Example 1, Example 4 and Example 5 are respectively as shown in Figure 4 , Figure 6 and Figure 8 As shown above, it can be seen that the present invention can improve the density of the mullite base layer and reduce the pores to improve the thermal shock resistance of the coating by ball-milling only the andalusite powder to a coarse and fine mixed powder state. On the other hand, it can also avoid the situation where all the powders are too small, resulting in the coating being too dense and having no room for thermal expansion and contraction during the thermal shock test, which ultimately causes the coating to fall off.
[0168] Example 6
[0169] The present embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method is the same as that of Embodiment 1 except that the mass ratio of high entropy rare earth monosilicate powder to high entropy rare earth disilicate powder is 1:1, and thus will not be described in detail herein.
[0170] Example 7
[0171] The present embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method is the same as that of Embodiment 1, except that the mass ratio of high-entropy rare earth monosilicate powder to high-entropy rare earth disilicate powder is 10:1, and thus will not be described in detail.
[0172] Example 8
[0173] The present embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method is the same as that of Embodiment 1, except that the mass fraction of andalusite powder is 30, and the rest remain unchanged, and will not be described again.
[0174] Example 9
[0175] The present embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method is the same as that of Embodiment 1, except that the mass fraction of andalusite powder is 80, and the rest remains unchanged, and will not be described again.
[0176] Example 10
[0177] This embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method replaces the high entropy rare earth monosilicate powder with Y 0.25 Nd 0.25 Eu 0.25 Er 0.25 Except for SiO5 powder, the rest are the same as those in Example 1 and will not be described again.
[0178] Embodiment 11
[0179] This embodiment provides a method for preparing a silicon carbide-based composite ceramic coating. The preparation method replaces the high entropy rare earth double silicate powder with Dy 0.25 Sc 0.25 Eu 0.25 Er 0.25 Except for Si2O7 powder, the rest are the same as those in Example 1 and will not be described again.
[0180] In Examples 4 to 11, the thermal shock resistance and oxidation weight gain rate were tested using the same method as in Example 1. The results are shown in Table 4.
[0181] Table 4
[0182] Cracks after 50 thermal shocks at 1500℃ Oxidation weight gain rate Example 4 Coating peeling -2.3% Example 5 There are cracks 0.8% Example 6 There are cracks 1.3% Example 7 Cracks and peeling coating -3.1% Example 8 There are cracks 2.1% Example 9 There are cracks 1.2% Example 10 No cracks 1.5% Embodiment 11 No cracks 1.3%
[0183] From Tables 1 to 4, we can see the following points:
[0184] (1) It can be seen from Examples 1 to 3 that the method for preparing the silicon carbide-based composite ceramic coating provided by the present invention is to prepare the silicon carbide-based composite ceramic coating by slurry coating, which not only has low investment cost and low equipment requirements, but also can achieve no cracks for more than 30 times at 1500°C, and the oxidation weight gain rate is within 0.782%, which can better meet the requirements of the burner for high temperature water-oxygen corrosion resistance at more than 1300°C;
[0185] (2) Combining Example 1 and Examples 4 to 5, it can be seen that in Example 1, only the andalusite powder is ball-milled. Compared with Example 4 in which 250 mesh and no andalusite powder is directly used without ball-milling and in Example 5 in which the andalusite raw material, corundum powder and silica powder are all ball-milled to a particle size of 7500 mesh, in Example 2, no cracks are generated after 50 times of thermal shock at 1500°C, and the oxidation weight gain rate is only 0.25%. In Example 4, after 50 times of thermal shock at 1500°C, the coating peels off, and the oxidation weight gain rate is -2.3% (due to the peeling of the coating, the dead weight is reduced). In Example 5, after 50 times of thermal shock at 1500°C, cracks appear in the coating, and the oxidation weight gain rate reaches 0.8%. This shows that the present invention preferably only ball-mills the andalusite powder and controls it within a specific particle size range, while the other powders still maintain a larger particle size range, which can better improve the bonding strength between the coating and the ceramic, avoid the occurrence of cracks at high temperatures and prevent the coating from falling off;
[0186] (3) Combining Example 1 and Examples 6 to 7, it can be seen that the content of high-entropy rare earth disilicate in Example 6 is too high, and porous and cracked rare earth monosilicate is easily generated on the surface of the coating after corrosion, and the corrosive medium diffuses into the interior of the coating along the defects, reducing the high-temperature water-oxygen corrosion resistance; the content of high-entropy rare earth monosilicate in Example 7 is too high, and it is easy to react with SiO2 to generate high disilicate, and the thermal expansion coefficient increases, which is not matched with the mullite coating, and finally causes the coating to peel off and fail. This shows that the present invention needs to use high-entropy rare earth monosilicate as the main phase and high-entropy rare earth disilicate as the second phase, and the mass ratio of the two is controlled within a specific range, in order to better improve the performance of the coating;
[0187] (4) It can be seen from the combination of Example 1 and Examples 8 to 9 that in Example 1, the ratio of andalusite: corundum powder: silica powder: first binder: first curing agent: first dispersant: ethanol is controlled to be 70:20:10:20:4:6:50. In Example 1, no cracks are generated after 50 times of thermal shock at 1500°C, and the oxidation weight gain rate is only 0.25%. In Examples 8 to 9, the mass fraction of andalusite is adjusted to 30 or 80 while other factors remain unchanged, which ultimately leads to cracks after 50 times of thermal shock at 1500°C, and the oxidation weight gain rates in Examples 8 to 9 are 2.1% and 1.2%, respectively. This shows that the amount of andalusite added in the present invention has a great influence on the thermal shock resistance and oxidation corrosion resistance of the coating. It is preferred to control the amount of andalusite added within a specific range, which can better improve the thermal shock resistance and oxidation corrosion resistance of the coating;
[0188] (5) It can be seen from Example 1 and Examples 10 to 11 that Example 1 contains a high-entropy rare earth silicate containing five rare earth elements, while Examples 10 to 11 contain only four rare earth elements. From the data, it can be seen that Examples 10 to 11 did not produce cracks after 50 thermal shocks at 1500°C, but the oxidation weight gain rate increased compared to Example 1. This shows that the present invention further preferably uses a high-entropy rare earth silicate of at least five rare earth elements, which has better oxidation corrosion resistance.
[0189] The present invention illustrates the detailed features of the present invention through the above embodiments, but the present invention is not limited to the above detailed features, that is, it does not mean that the present invention must rely on the above detailed features to be implemented. Those skilled in the art should understand that any improvement to the present invention, equivalent replacement of the technical features selected by the present invention, addition of auxiliary technical features, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A silicon carbide-based composite ceramic coating, characterized in that: The silicon carbide-based composite ceramic coating comprises a mullite base layer arranged on the surface of silicon carbide, and a high-entropy rare earth silicate composite surface layer located on the mullite base layer; the high-entropy rare earth silicate composite surface layer comprises a main phase and a second phase, the main phase is a high-entropy rare earth monosilicate, and the second phase is a high-entropy rare earth disilicate; The mullite base layer includes a mullite phase and amorphous silicon dioxide.
2. The silicon carbide-based composite ceramic coating according to claim 1, characterized in that: The content of amorphous silicon dioxide in the mullite bottom layer is 5-20%, preferably 5-10%.
3. The silicon carbide-based composite ceramic coating according to claim 1 or 2, characterized in that: The content of high entropy rare earth disilicate in the high entropy rare earth silicate composite surface layer is 10-25%, preferably 10-20%; Preferably, the chemical formula of the high entropy rare earth monosilicate is The chemical formula of the high entropy rare earth disilicate is Among them, RE i It is any one of the rare earth elements Sc, Y, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb or Lu, n≥5 and 1≤i≤n.
4. The silicon carbide-based composite ceramic coating according to claim 1, characterized in that: The thickness of the mullite bottom layer is 50 to 200 μm; the thickness of the high entropy rare earth silicate composite surface layer is 100 to 200 μm; Preferably, the density of the mullite bottom layer is 96% to 99%.
5. A slurry sintering preparation method for a silicon carbide-based composite ceramic coating according to any one of claims 1 to 4, characterized in that: The slurry sintering preparation method comprises: (1) The silicon carbide substrate is immersed in the mullite base slurry, and the excess slurry is removed and dried in turn; (2) repeating step (1) at least once to obtain a mullite coating precursor; (3) The mullite coating precursor in step (2) is subjected to a first calcination and a first cooling to obtain a first silicon carbide ceramic material containing a mullite bottom layer; (4) Step (3) The first silicon carbide ceramic material is immersed in a high entropy rare earth silicate composite surface layer slurry, and then the excess slurry is removed and dried; (5) repeating step (4) at least once to obtain a high-entropy rare earth silicate composite ceramic precursor material; (6) The high-entropy rare earth silicate composite ceramic precursor material in step (5) is subjected to a second calcination and a second cooling to obtain a silicon carbide ceramic containing a silicon carbide-based composite ceramic coating.
6. The preparation method according to claim 5, characterized in that: The raw materials of the mullite bottom slurry include 250-450 mesh andalusite powder, 700-900 mesh corundum powder and 7500-9500 mesh silicon dioxide powder; Preferably, the preparation of the mullite bottom layer slurry comprises: subjecting a raw material of andalusite with a particle size of 250 to 450 meshes to a first ball milling to obtain andalusite powder; mixing andalusite powder, corundum powder, silicon dioxide powder, a first binder, a first curing agent, a first dispersant and ethanol, and subjecting the mixture to a second ball milling and sieve filtering to obtain the mullite bottom layer slurry; Preferably, the mass ratio of andalusite powder:corundum powder:silicon dioxide powder:first binder:first curing agent:first dispersant:ethanol is (40-70):(10-30):(2-10):(20-60):(1-6):(2-10):(30-70); Preferably, the first ball milling is carried out in a jar mill; Preferably, the rotation speed of the first ball mill is 180-220 r / min; Preferably, the first ball milling time is 24 to 48 hours; Preferably, the particle size of the andalusite after the first ball milling is 1000 to 5000 mesh; Preferably, the second ball milling time is 6 to 24 hours; Preferably, the rotation speed of the second ball mill is 180-220 r / min; Preferably, the mesh size of the sieve filtration in step (1) is 100 to 200 meshes; Preferably, the removing of excess slurry in step (1) comprises centrifugation and purging performed sequentially; Preferably, the drying in step (1) includes drying; Preferably, the drying temperature in step (1) is 80-120°C; Preferably, the number of repetitions in step (2) is 1 to 5 times; Preferably, the temperature of the first calcination in step (3) is 1500-1600°C; Preferably, the first calcination time in step (3) is 3 to 10 hours.
7. The preparation method according to claim 6, characterized in that: The preparation of the high entropy rare earth silicate composite surface slurry in step (4) comprises: Mixing high entropy rare earth monosilicate powder, high entropy rare earth disilicate powder, a second binder, a second curing agent, a second dispersant and ethanol, performing a third ball milling and sieve filtering to obtain the high entropy rare earth silicate composite surface layer slurry; Preferably, the mass ratio of the high entropy rare earth monosilicate powder, the high entropy rare earth disilicate powder, the second binder, the second curing agent, the second dispersant and ethanol is (70-90):(10-30):(20-60):(1-6):(2-10):(30-70); Preferably, the rotation speed of the third ball mill is 180-220 r / min; Preferably, the third ball milling time is 6 to 24 hours; Preferably, the mesh size of the sieve filtration in step (4) is 100 to 200 meshes.
8. The preparation method according to claim 7, characterized in that: The preparation process of the high entropy rare earth monosilicate powder and the high entropy rare earth disilicate powder each independently comprises: S1, rare earth oxide and the third dispersant are mixed and subjected to a fourth ball milling to form a precursor slurry; S2, the precursor slurry is dried and sieved in sequence and then sintered to obtain high entropy rare earth silicate particles; S3, the high entropy rare earth silicate particles are subjected to a fifth ball milling and sieving in air to obtain high entropy rare earth silicate powder; Preferably, the third dispersant comprises water and / or ethanol; Preferably, the fourth ball milling time is 6 to 24 hours; Preferably, the rotation speed of the fourth ball mill is 300-400 r / min; Preferably, the heating rate of the sintering synthesis is 5 to 10°C / min; Preferably, the synthesis temperature of the sintering synthesis is 1500-1650°C; Preferably, the sintering synthesis time is 0.5 to 20 hours; Preferably, the fifth ball milling time is 6 to 20 hours; Preferably, the rotation speed of the fifth ball mill is 300-400 r / min.
9. The preparation method according to claim 7, characterized in that: The first binder and the second binder each independently comprise a resin having a carbon residue value greater than 35%, wherein the resin comprises any one of epoxy resin, phenolic resin, polyacrylic resin, polyvinyl butyral, furfural resin or a combination of at least two of phenol furfural resins; Preferably, the first curing agent and the second curing agent each independently include any one of citric acid, p-toluenesulfonic acid, pentosan or oxalic acid, or a combination of at least two thereof; Preferably, the first dispersant and the second dispersant each independently include any one or a combination of at least two of castor oil, triolein, Tween 20 or organobentonite; Preferably, the silicon carbide substrate has a porous structure.
10. Use of the silicon carbide-based composite ceramic coating according to any one of claims 1 to 4 in a porous medium burner in a medium-high temperature range, wherein the temperature in the medium-high temperature range is preferably ≥ 1300°C.
Citation Information
Patent Citations
Preparation method of composite material of barium strontium aluminum containing silicate / mullite / SiC three-layer composite structural coating
CN105503272A
Ultra-high temperature multi-layer gradient composite environmental barrier coating and preparation method thereof
CN106977234A
Rare earth silicate environment shield coating with multi-layer structure and preparation method thereof
CN110983233A
High-entropy rare earth silicate ceramic coating material and preparation method thereof
CN117383919A
Thermal and / or environmental barrier coating system
US20200199027A1
Cited By
Boron-free long-life dry vibration material for induction furnace and preparation method of boron-free long-life dry vibration material
CN121494587A
Boron-free long-life dry vibrating material for induction furnace and preparation method thereof
CN121494587B