Method for catalytically degrading polyester by using basic ionic liquid

By promoting the degradation of polyester under mild conditions by a specific structure, the problems of high temperature and high pressure and high catalyst cost in the prior art are solved, and efficient and low-energy consumption of polyester recycling and recycling are achieved.

CN118955281AActive Publication Date: 2024-11-15DONGHUA UNIV

Patent Information

Application Number
CN202411034989.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing polyethylene terephthalate recovery methods have problems such as high temperature and high pressure, equipment corrosion, high catalyst cost, difficulty in recycling and complex post-processing, making it difficult to achieve large-scale application.

Method used

Using alkaline ionic liquid with a specific structure as a catalyst, alcohol or amine as reactants, catalyze the degradation of polyester under mild conditions (50℃~120℃), using the ester bond interaction between cations and polyester and anions with alcohol or The nucleophilic effect of amines promotes the rapid degradation of polyester.

Benefits of technology

It achieves efficient degradation of polyester under mild conditions, with a yield of 94.6% of the degradation target product, and the catalyst can be recycled, reducing energy consumption and industrial application costs, and simplifying the post-treatment process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955281A_ABST
    Figure CN118955281A_ABST
Patent Text Reader

Abstract

The invention provides a method for catalytically degrading polyester by using basic ionic liquid, which comprises the following steps of: catalytically degrading the polyester by using the basic ionic liquid as a catalyst and alcohol or amine as a reactant; the basic ionic liquid is a mixture selected from one or more of the following structural general formulas: X < + > Y <->, in the formula, X < + > is an organic alkali cation, and Y <-> is a phenolic anion. Compared with the existing catalyst, the method provided by the invention has the advantages that the chemical recovery of polyester (especially PET) under mild conditions (the reaction temperature is 50-120 DEG C, especially 70-80 DEG C) is realized, and the yield of the degraded target product can reach 94.6%. The basic ionic liquid can interact with ester bonds of the polyester through cations, and anions can generate pi-pi interaction with benzene rings of the polyester while having nucleophilic interaction with alcohol or amine, so that rapid degradation of the polyester is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of green catalysis and chemical recycling degradation, and specifically relates to a method for catalyzing the degradation of polyester using alkaline ionic liquid, in particular to a method for rapidly degrading polyethylene terephthalate under mild conditions using alkaline ionic liquid. Background Art

[0002] Polyester is a general term for polymers obtained by polycondensation of polyols and polyacids. It is a type of engineering plastic with excellent performance and wide applications. Polyester includes polyester resin and polyester elastomer. Polyester resin includes polyethylene terephthalate (PET), polybutylene terephthalate (PBT) and polyarylate (PAR). Polyester elastomer (TPEE) is generally polymerized from dimethyl terephthalate, 1,4-butanediol and polybutanol. The chain segment includes hard segment and soft segment, and is a thermoplastic elastomer.

[0003] Polyethylene terephthalate (PET) is a common thermoplastic polymer material and a polyester plastic. It is usually known as a plastic bottle. PET is widely used in fiber materials, textile fabrics, clothing, beverage bottles, food containers, films and sheets.

[0004] At present, the main methods for recycling polyesters such as polyethylene terephthalate are physical recycling and chemical recycling. Physical recycling refers to the process of washing, crushing, remelting, regranulating or making films of waste PET. The advantages of physical recycling are that the recycling method is simple, the investment is small, and existing equipment can be used. However, the performance of PET after physical recycling is greatly reduced, and it is difficult to meet the needs of the food industry, fiber industry, etc., and the application field is limited. Chemical recycling is not limited by the source of PET raw materials. PET composite materials or low-quality PET waste can be recycled and can be recycled many times. The recycled products are of high quality and widely used, and can fundamentally realize the closed-loop circulation of PET. Therefore, people are more considering using chemical methods to recycle waste PET.

[0005] Chemical recovery methods are mainly divided into hydrolysis, alcoholysis, aminolysis / ammoniolysis, etc. The hydrolysis method generally uses water as a degradation agent, and depolymerizes PET to generate the corresponding terephthalic acid (PTA) under acidic or alkaline conditions through high temperature and high pressure. However, equipment corrosion problems need to be considered under acidic and alkaline conditions, and PTA purification is difficult under neutral conditions. For example, the Chinese invention patent with publication number CN113149825A discloses a method for catalytic degradation of polyethylene terephthalate, comprising the following steps: (1) mixing polyethylene terephthalate fragments and a catalyst evenly to obtain a mixture; (2) heating the mixture, causing a degradation reaction under the combined action of water vapor and the catalyst, and obtaining a solid phase product and a liquid phase product after the reaction is completed; wherein the catalyst is a zinc compound. The application degrades waste PET into terephthalic acid and ethylene glycol, and the reaction temperature is controlled within 300°C. The yields of the degradation products terephthalic acid and ethylene glycol can reach 90-99wt% and 91-99wt%, respectively. This method requires high temperature conditions when degrading PET, and the catalyst is easy to corrode the equipment. The equipment requirements are high, the reaction conditions are harsh, and it is difficult to achieve large-scale application. In addition, the products obtained by the hydrolysis method often contain oligomeric byproducts such as dimers and trimers. For example, the Chinese invention patent with publication number CN 117603036 A discloses a method of using high-pressure carbon dioxide gas as a catalyst for the hydrolysis reaction of PET. Carbon dioxide and water form carbonic acid at high temperature. Under the conditions of 3MPa and 200°C, the calculated yields of terephthalic acid and ethylene glycol of the hydrolysis products are 64.9% and 70.6% respectively; this method also has the problems of high temperature, high pressure and high energy consumption. The alcoholysis method refers to a method in which a monohydric alcohol or a polyhydric alcohol is transesterified with polyethylene terephthalate under certain temperature and pressure conditions to obtain the corresponding esterified monomer and ethylene glycol. For example, a Chinese invention patent with publication number CN 102731310A discloses a method for alcoholysis of polyethylene terephthalate using a first transition series metal ion liquid as a catalyst, a diol as a solvent, a catalyst dosage of 0.1% to 20% of the solvent mass, a reaction temperature of 80°C to 250°C, a pressure of 1 atm, and a reaction time of 1 min to 9 h. This method achieves highly selective PET conversion, but the method has the problems of high cost of metal ion liquid catalysts, difficulty in reuse, and many post-processing problems, making it difficult to use on a large scale.

[0006] Therefore, there is an urgent need for a method with mild degradation conditions, high yield, simple post-treatment, no use of other organic solvents and co-catalysts, and recyclable catalysts to achieve the recovery and high value-added conversion of waste polyethylene terephthalate. Summary of the invention

[0007] In order to solve the above technical problems, the object of the present invention is to provide a method for catalytic degradation of polyester using alkaline ionic liquid, so as to achieve rapid degradation of polyester under mild conditions.

[0008] In order to achieve the above technical objectives, the present invention provides a method for catalytic degradation of polyester using alkaline ionic liquid, using alkaline ionic liquid as a catalyst and alcohol or amine as a reactant to catalytically degrade polyester; the alkaline ionic liquid is a mixture of one or more selected from the following general structural formulas:

[0009] X + Y - ,

[0010] Where, X + is an organic base cation, Y - It is a phenol anion.

[0011] Optimally, X + Includes the following chemical structure formula:

[0012]

[0013] In the formula, R1 and R2 are independently selected from one of C1-C8 alkyl, alkoxy, cycloalkyl, alkenyl, phenyl and benzyl.

[0014] Furthermore, Y - The general chemical structure is:

[0015]

[0016] In the formula, R3, R4, R5, R6 and R7 are independently selected from one of C1-C8 alkyl, alkoxy, cycloalkyl, alkenyl, phenyl, benzyl and halogen, and the halogen includes fluorine, chlorine, bromine and iodine.

[0017] Optimally, the alcohol is a mixture of one or more selected from methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol and butanediol.

[0018] Optimally, the amine is a mixture of one or more selected from methylamine, ethylamine, propylamine, butylamine, ethylenediamine, propylenediamine and butylenediamine.

[0019] Optimally, the reaction temperature of the catalytic degradation is 50°C to 120°C, the reaction time is 1h to 8h, and the reaction pressure is normal pressure or autogenous pressure.

[0020] Furthermore, the molar ratio of the reactant to the polyester is 10:1 to 80:1.

[0021] Furthermore, the molar ratio of the catalyst to the polyester is 0.1-5.

[0022] Optimally, the polyester is a mixture of one or more selected from the group consisting of polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polybutylene terephthalate and polyarylate.

[0023] Optimally, the alkaline ionic liquid is prepared by stirring reaction of an organic base or XOH with a phenolic compound at room temperature.

[0024] The method for catalytic degradation of polyester using alkaline ionic liquids of the present invention uses alkaline ionic liquids of specific structures as catalysts and alcohols or amines as reactants to catalytically degrade polyesters, and does not require the use of other organic solvents and co-catalysts. Compared with the currently available catalysts, the chemical recovery of polyester (especially PET) under mild conditions (reaction temperature of 50°C to 120°C, especially 70°C to 80°C) is achieved, and the yield of degradation target products can reach 94.6%. This is because these alkaline ionic liquids of specific structures can interact with the ester bond of the polyester through cations, and the anions can interact with the alcohols or amines nucleophilically while generating π-π interactions with the benzene rings of the polyester, and such multiple interactions promote the rapid degradation of the polyester.

[0025] The alkaline ionic liquid catalyst disclosed in the present invention can react with a variety of nucleophilic reagents, showing good universality and recyclability. Compared with other types of alkaline catalysts reported, the catalyst synthesis is cleaner and more efficient, degrading polyester under relatively mild conditions, reducing energy consumption, and showing good prospects for industrial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is a chemical principle diagram of the present invention for utilizing alkaline ionic liquid to catalyze the degradation of polyester.

[0027] Figure 2 These are the H NMR spectrum and IR spectrum of the alkaline ionic liquid in Example 1.

[0028] Figure 3 These are the H NMR spectrum and IR spectrum of dimethyl terephthalate prepared in Example 2. DETAILED DESCRIPTION

[0029] The present invention discloses a method for catalyzing the degradation of polyester using alkaline ionic liquids, wherein the alkaline ionic liquids are used as catalysts and alcohols or amines are used as reactants to catalyze the degradation of polyester; the alkaline ionic liquids are a mixture of one or more selected from the following general structural formulas: + Y - , where X + is an organic base cation, Y - It is a phenolic anion. Taking the case of polyethylene terephthalate as an example, the degradation principle can be found in Figure 1 . Using alkaline ionic liquids with specific structures as catalysts and alcohols or amines as reactants to catalyze the degradation of polyester, no other organic solvents and co-catalysts are needed. Compared with the currently available catalysts, chemical recovery of polyester (especially PET) under mild conditions (reaction temperature of 50°C to 120°C, especially 70°C to 80°C) is achieved, and the yield of the target degradation product can reach 94.6%. This is because these alkaline ionic liquids with specific structures can interact with the ester bond of polyester through cations, and anions can interact with alcohols or amines nucleophilically while generating π-π interactions with the benzene rings of polyester. Such multiple interactions promote the rapid degradation of polyester.

[0030] The alkaline ionic liquid catalyst disclosed in the present invention can react with a variety of nucleophilic reagents, showing good universality and recyclability. Compared with other types of alkaline catalysts reported, the catalyst synthesis is cleaner and more efficient, degrading polyester under relatively mild conditions, reducing energy consumption, and showing good prospects for industrial application.

[0031] X + Preferably, the following chemical structure is included:

[0032]

[0033] In the formula, R1 and R2 are independently selected from one of C1-C8 alkyl, alkoxy, cycloalkyl, alkenyl, phenyl and benzyl. R1 and R2 are independently selected from phenyl, benzyl, C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl or C8 alkyl, more preferably C1 alkyl-C4 alkyl or phenyl.

[0034] Y - The general chemical structure is:

[0035]

[0036] In the formula, R3, R4, R5, R6 and R7 are independently selected from one of C1-C8 alkyl, alkoxy, cycloalkyl, alkenyl, phenyl, benzyl and halogen, wherein the halogen includes fluorine, chlorine, bromine and iodine. R3, R4, R5, R6 and R7 are independently preferably phenyl, benzyl, C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl or C8 alkyl, more preferably C1 alkyl-C2 alkyl, alkoxy or phenyl. More specifically, Y -Including but not limited to the following examples: phenol, hydroquinone, p-(c, m) tert-butylphenol, propofol, p-(c, m) methylphenol, p-(c, m) ethylphenol, p-(c, m) methoxyphenol, p-(c, m) nitrophenol, p-(c, m) fluorophenol, p-(c, m) chlorophenol, p-(c, m) bromophenol, p-(c, m) iodophenol, eugenol, magnolol and p-(c, m) allylphenol; in this case, Y - It is the group formed by removing a hydrogen ion from phenol, hydroquinone, p-(c-, m-)tert-butylphenol, propofol, p-(c-, m-)methylphenol, p-(c-, m-)ethylphenol, p-(c-, m-)methoxyphenol, p-(c-, m-)nitrophenol, p-(c-, m-)fluorophenol, p-(c-, m-)chlorophenol, p-(c-, m-)bromophenol, p-(c-, m-)iodophenol, eugenol, magnolol or p-(c-, m-)allylphenol.

[0037] The alcohol is a mixture of one or more selected from methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol and butanediol. The amine is a mixture of one or more selected from methylamine, ethylamine, propylamine, butylamine, ethylenediamine, propylenediamine and butanediamine.

[0038] The reaction temperature of the catalytic degradation is 50°C to 120°C, the reaction time is 1h to 8h, and the reaction pressure is normal pressure or autogenous pressure. The aforementioned reaction conditions can be any value within the aforementioned range, such as the reaction temperature can be 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, but preferably 70°C to 80°C; the reaction time can be 1h, 2h, 3h, 4h, 5h, 6h, 7h or 8h, but preferably 3h to 5h;

[0039] The molar ratio of the reactant to the polyester is 10:1 to 80:1 (i.e., the amount of alcohol or amine used is 10-80 times the molar amount of polyester), for example, it can be 10 times, 20 times, 30 times, 40 times, 50 times, 60 times, 70 times or 80 times; but preferably 30 to 50 times.

[0040] The molar ratio of the catalyst to the polyester is 0.1 to 5 (i.e., the catalyst molar ratio is 0.1 to 5 times the polyester molar ratio), for example, 0.1, 0.2, 0.5, 1, 2, 3, 4 or 5 times; but preferably 0.5 to 2 times.

[0041] The alkaline ionic liquid is prepared by stirring reaction of an organic base or XOH with a phenolic compound at room temperature.

[0042] The polyester is a mixture of one or more selected from polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polybutylene terephthalate and polyarylate.

[0043] After the reaction is completed, the degradation rate of polyester (taking polyethylene terephthalate, PET, as an example below) and the selectivity of the product are calculated according to the following formulas:

[0044]

[0045]

[0046] Wherein, A represents the initial mass of the added PET, and B represents the mass of the undegraded PET.

[0047] The preferred embodiments of the present invention will be described in detail below.

[0048] Example 1

[0049] This embodiment provides a series of alkaline ionic liquids and preparation methods thereof. Specifically, different alkaline ionic liquids are prepared by a simple neutralization reaction between an organic base and a series of phenolic compounds.

[0050] Taking 1,8-diazabicyclo[5.4.0]undec-7-enephenol ([HDBU][PhO]) as an example: 1,8-diazabicyclo[5.4.0]undec-7-ene and phenol (PhO) were dissolved in anhydrous ethanol (100 mL) at a molar ratio of 1:1 (in this embodiment, 1 mmol of each was used), stirred at room temperature for 24 hours, and the solvent was removed by a vacuum rotary evaporator, and then dried in a vacuum oven at 60°C for 24 hours to obtain the target ionic liquid [HDBU][PhO]; its H NMR spectrum and IR spectrum are shown in FIG. Figure 2 shown.

[0051] By replacing appropriate raw materials and adopting the same preparation method, other alkaline ionic liquids involved in the present invention (see the aforementioned general chemical formula) can be obtained.

[0052] Example 2

[0053] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is as follows:

[0054] Take the alkaline ionic liquid ([HDBU][PhO], used as a catalyst), methanol (as a reactant) and polyethylene terephthalate (powder) prepared in Example 1, and add them into a 15 mL pressure bottle (wherein, polyethylene terephthalate 0.576 g (3 mmol), methanol 4.8 g (0.15 mol), catalyst [HDBU][PhO] (3 mmol) in sequence; after sealing, control the reaction temperature at 70 ° C. and react for 3 hours; cool to room temperature, add 50 mL of acetonitrile to dissolve, and filter: the filter cake is unreacted polyethylene terephthalate, and the filtrate is vacuum-rotated to remove the solvent; then add water to obtain a white solid precipitate, which is dimethyl terephthalate, and its nuclear magnetic hydrogen spectrum and infrared spectrum are as shown Figure 3 The aqueous phase was subjected to reduced pressure distillation to remove water and ethylene glycol, and then dried in a vacuum oven to recover the catalyst. Under these conditions, the degradation rate of polyethylene terephthalate was 89.2% and the yield of dimethyl terephthalate monomer was 83.4% as calculated by the above formula.

[0055] Example 3

[0056] This embodiment provides a method for degrading polyester using alkaline ionic liquid as catalyst, which is basically the same as that in Example 2, except that the catalyst is changed to 1,5,7-triazabicyclo[4.4.0]dec-5-ene-p-methylphenol ([HTBD][4-MePhO]). Under these conditions, the polyethylene terephthalate degradation rate is calculated to be 100%, and the yield of monomer dimethyl terephthalate is 94.6%.

[0057] Example 4

[0058] This embodiment provides a method for degrading polyester using alkaline ionic liquid as catalyst, which is basically the same as that in Example 2, except that the catalyst is changed to 1,1,3,3-tetramethylguanidine-p-methylphenol ([HTMG][4-MePhO]). Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 59.0%, and the yield of monomer dimethyl terephthalate is 56.3%.

[0059] Example 5

[0060] This embodiment provides a method for degrading polyester using alkaline ionic liquid as catalyst, which is basically the same as that in Example 2, except that the catalyst is changed to 1,5-diazabicyclo[4.3.0]non-5-ene-p-methylphenol ([HDBN][4-MePhO]). Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 79.2%, and the yield of monomer dimethyl terephthalate is 73.9%.

[0061] Example 6

[0062] This embodiment provides a method for degrading polyester using alkaline ionic liquid catalysis, which is basically the same as that in Example 2, except that the catalyst is changed to 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene-p-methylphenol ([HMTBD][4-MePhO]). Under these conditions, the polyethylene terephthalate degradation rate is calculated to be 91.0%, and the yield of monomer dimethyl terephthalate is 85.5%.

[0063] Example 7

[0064] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquids, which is basically the same as that in Example 2, except that the catalyst is changed to tetrabutylphosphine-p-methylphenol ([P 4444 Under these conditions, the degradation rate of polyethylene terephthalate was calculated to be 74.8%, and the yield of dimethyl terephthalate monomer was 72.2%.

[0065] Example 8

[0066] This embodiment provides a method for degrading polyester using alkaline ionic liquid as catalyst, which is basically the same as that in Example 2, except that the catalyst is changed to 1-ethyl-3-methylimidazole-p-methylphenol ([Emim][4-MePhO]). Under these conditions, the degradation rate of polyethylene terephthalate is calculated to be 62.1%, and the yield of monomer dimethyl terephthalate is 58.2%.

[0067] Example 9

[0068] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the reaction temperature is controlled to be 80° C. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 100%, and the yield of monomer dimethyl terephthalate is 93.6%.

[0069] Example 10

[0070] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the reaction temperature is controlled to be 60° C. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 84.3%, and the yield of monomer dimethyl terephthalate is 75.7%.

[0071] Embodiment 11

[0072] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the reaction temperature is controlled to be 50° C. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 52.1%, and the yield of monomer dimethyl terephthalate is 50.3%.

[0073] Example 12

[0074] This embodiment provides a method for degrading polyester by catalysis of alkaline ionic liquid, which is basically the same as that in Example 3, except that the reaction temperature is controlled to be 120° C. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 100%, and the yield of monomer dimethyl terephthalate is 94.5%.

[0075] Embodiment 13

[0076] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the methanol is adjusted to 2.88 g. Under this condition, the polyethylene terephthalate degradation rate is calculated to be 100%, and the yield of monomer dimethyl terephthalate is 94.3%.

[0077] Embodiment 14

[0078] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the methanol is adjusted to 1.92 g. Under this condition, the polyethylene terephthalate degradation rate is calculated to be 97.9%, and the yield of monomer dimethyl terephthalate is 90.1%.

[0079] Embodiment 15

[0080] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the methanol is adjusted to 0.96 g. Under this condition, the polyethylene terephthalate degradation rate is calculated to be 92.2%, and the yield of monomer dimethyl terephthalate is 88.1%.

[0081] Example 16

[0082] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the methanol is adjusted to 7.68 g. Under this condition, the polyethylene terephthalate degradation rate is calculated to be 100%, and the yield of monomer dimethyl terephthalate is 93.8%.

[0083] Embodiment 17

[0084] This example provides a method for catalyzing the degradation of polyester using alkaline ionic liquids, which is basically the same as that in Example 3, except that the amount of the catalyst [HTBD][4-MePhO] is changed to 3.3 mmol. Under these conditions, the polyethylene terephthalate degradation rate is calculated to be 100%, and the yield of the monomer dimethyl terephthalate is 93.6%.

[0085] Embodiment 18

[0086] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the amount of catalyst [HTBD][4-MePhO] is changed to 2.4 mmol. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 90.6%, and the yield of monomer dimethyl terephthalate is 82.8%.

[0087] Embodiment 19

[0088] This example provides a method for catalyzing the degradation of polyester using alkaline ionic liquids, which is basically the same as that in Example 3, except that the amount of the catalyst [HTBD][4-MePhO] is changed to 0.3 mmol. Under these conditions, the polyethylene terephthalate degradation rate is calculated to be 72.2%, and the yield of the monomer dimethyl terephthalate is 68.9%.

[0089] Embodiment 20

[0090] This example provides a method for catalyzing the degradation of polyester using alkaline ionic liquids, which is basically the same as that in Example 3, except that the amount of the catalyst [HTBD][4-MePhO] is changed to 15 mmol. Under these conditions, the polyethylene terephthalate degradation rate is calculated to be 100%, and the yield of the monomer dimethyl terephthalate is 94.5%.

[0091] Embodiment 21

[0092] This embodiment provides a method for degrading polyester by catalysis of alkaline ionic liquid, which is basically the same as that in embodiment 3, except that polyethylene terephthalate is replaced by polypropylene terephthalate. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 100%, and the yield of monomer dimethyl terephthalate is 90.6%.

[0093] Embodiment 22

[0094] This embodiment provides a method for degrading polyester by catalysis of alkaline ionic liquid, which is basically the same as that in embodiment 3, except that polyethylene terephthalate is replaced by polybutylene terephthalate. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 100%, and the yield of monomer dimethyl terephthalate is 81.1%.

[0095] Examples 23-27

[0096] Examples 23-27 respectively provide a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that the catalyst is replaced with the ionic liquid catalyst recovered in Example 3 (the catalysts in Examples 23-27 are respectively recycled 1 to 5 times). The final results are shown in Table 1.

[0097] Table 1 Results of polyester degradation experiments in Examples 23-27

[0098]

[0099] Embodiment 28

[0100] This embodiment provides a method for degrading polyester using alkaline ionic liquid catalysis, which is basically the same as that in Example 3, except that methanol is replaced with ethylamine. Under this condition, the degradation rate of polyethylene terephthalate is calculated to be 100%, and the yield of monomer N,N'-diethylterephthalamide is 96%.

[0101] Embodiment 29

[0102] This embodiment provides a method for catalyzing the degradation of polyester using alkaline ionic liquid, which is basically the same as that in Example 3, except that methanol is replaced by ethanolamine. Under this condition, it is calculated that the degradation rate of polyethylene terephthalate is 100%, and the yield of monomer N,N'-bis(2-hydroxyethyl)terephthalamide is 87%.

[0103] Comparative Example 1

[0104] This example provides a method for catalyzing the degradation of polyester using alkaline ionic liquids, which is basically the same as that in Example 3, except that the catalyst is changed to 1,8-diazabicyclo[5.4.0]undec-7-enoic acid ([HDBU][OAc]), and under the same conditions, no monomer dimethyl terephthalate is detected.

[0105] Comparative Example 2

[0106] This example provides a method for catalyzing the degradation of polyester using alkaline ionic liquids, which is basically the same as that in Example 3, except that the catalyst is changed to 1,8-diazabicyclo[5.4.0]undec-7-ene hydrochloride zinc chloride ([HDBU][ZnCl3]). Under the same conditions, no monomer dimethyl terephthalate is detected.

[0107] According to the above results, it is fully demonstrated that the alkaline ionic liquid catalyst in the present invention exhibits a good catalytic effect on the degradation of polyesters such as polyethylene terephthalate. The entire process of the above embodiments is under relatively mild conditions, and polyethylene terephthalate and other polyesters are precisely and controllably degraded into monomer compounds, and the reaction temperature is controlled at 70°C to 80°C, achieving low energy consumption, a simple catalyst preparation process, no other solvents and co-catalysts involved, and simple post-processing. The overall economic cost is low, the catalyst recycling performance is good, and the cost of industrial application is greatly reduced. The method of the present invention fully realizes the effective recovery and recycling of polyesters such as polyethylene terephthalate.

[0108] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for catalyzing the degradation of polyester using alkaline ionic liquids, Features: Using alkaline ionic liquid as a catalyst and alcohol or amine as a reactant to catalyze the degradation of polyester; the alkaline ionic liquid is a mixture of one or more selected from the following general structural formulas: X + AND - , In the formula, X + is an organic base cation, Y - It is a phenol anion.

2. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 1, It is characterized in that X + Includes the following chemical structure formula: In the formula, R 1 and R 2 Each of the groups is independently selected from the group consisting of C1-C8 alkyl, alkoxy, cycloalkyl, alkenyl, phenyl and benzyl.

3. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 1 or 2, It is characterized in that Y - The general chemical structure is: In the formula, R 3 , R 4 , R 5 , R 6 and R 7 Each of the above groups is independently selected from the group consisting of C1-C8 alkyl, alkoxy, cycloalkyl, alkenyl, phenyl, benzyl and halogen, wherein the halogen includes fluorine, chlorine, bromine and iodine.

4. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 1, Features: The alcohol is a mixture of one or more selected from methanol, ethanol, propanol, butanol, ethylene glycol, propylene glycol and butanediol.

5. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 1, Features: The amine is a mixture of one or more selected from methylamine, ethylamine, propylamine, butylamine, ethylenediamine, propylenediamine and butylenediamine.

6. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 1, Features: The reaction temperature of the catalytic degradation is 50° C. to 120° C., the reaction time is 1 h to 8 h, and the reaction pressure is normal pressure or autogenous pressure.

7. The method for degrading polyester by catalysis using alkaline ionic liquid according to claim 1 or 6, Features: The molar ratio of the reactant to the polyester is 10:1 to 80:

1.

8. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 7, Features: The molar ratio of the catalyst to the polyester is 0.1 to 5.

9. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 1, Features: The alkaline ionic liquid is prepared by stirring reaction of an organic base or XOH with a phenolic compound at room temperature.

10. The method for catalyzing the degradation of polyester using alkaline ionic liquid according to claim 1, Features: The polyester is a mixture of one or more selected from polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polybutylene terephthalate and polyarylate.

Citation Information

Patent Citations

  • Polyethylene terephthalate alcoholysis method with catalyst of first transition series metal ionic liquid

    CN102731310A

  • Method for catalytic alcoholysis of polyethylene glycol terephthalate with super-strong alkaline ionic liquid

    CN104774154A

  • Method for catalyzing and recycling waste polyester material by acetate ionic liquid

    CN116675603A

Cited By

  • Method for catalyzing polyester depolymerization by alkoxide

    CN121377995A

  • Method for catalyzing degradation of polyester into high value-added chemicals by using basic ionic liquid