Polysubstituted pyridine derivative compound and application thereof

By using multi-substituted pyridine derivative compounds as electron transport materials, the problem of low mobility of electron transport materials in the prior art is solved, and the efficient luminescence and long life of organic electroluminescent devices is achieved, the driving voltage is reduced, and the driving voltage is improved. Display effect.

CN118955362APending Publication Date: 2024-11-15YANTAI XIANHUA CHEM TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310548496.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing electronic transport materials have low mobility in organic electroluminescent devices, which limits the development of device performance, especially luminous efficiency and service life.

Method used

It provides a polysubstituted pyridine derivative compound as an electron transport material, which has high interatomic bond energy and good thermal stability, can effectively reduce the driving voltage, and expand the electron cloud conjugation through the pyridine as a central structure to increase the electron migration rate.

Benefits of technology

Higher luminescence efficiency and service life in organic electroluminescent devices are achieved, reducing driving voltage and improving display effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955362A_ABST
    Figure CN118955362A_ABST
Patent Text Reader

Abstract

The invention discloses a compound as shown in formula (I), which has high bond energy between atoms and good thermal stability, is beneficial to solid-state accumulation between molecules, has a proper energy level between adjacent levels, and is beneficial to injection and migration of excitons. When the compound is used as an electron transport material, the driving voltage of an organic electroluminescent device can be effectively reduced, the luminous efficiency is improved, and the service life is prolonged. The invention also provides an electron transport material containing the compound shown in the formula (I), an organic electroluminescent device and a display device. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organic light-emitting display, and in particular to a multi-substituted pyridine derivative compound and application thereof. Background Art

[0002] Electroluminescence (EL) refers to the phenomenon that luminescent materials emit light under the action of electric field, stimulated by current and voltage. It is a luminescence process that directly converts electrical energy into light energy. Organic electroluminescent displays (hereinafter referred to as OLEDs) have a series of advantages such as autonomous luminescence, low-voltage DC drive, full curing, wide viewing angle, light weight, simple composition and process. Compared with liquid crystal displays, organic electroluminescent displays do not require backlight sources, have large viewing angles, low power consumption, and their response speed can reach 1000 times that of liquid crystal displays, but their manufacturing cost is lower than that of liquid crystal displays with the same resolution. Therefore, organic electroluminescent devices have a very broad application prospect.

[0003] Compared with inorganic light-emitting materials, organic electroluminescent materials have many advantages, such as good processing performance, can be formed into films on any substrate by evaporation or spin coating, can realize flexible display and large-area display, can adjust the optical properties, electrical properties and stability of materials by changing the molecular structure, etc., and there is a lot of room for material selection. In the most common OLED device structure, the following types of organic materials are usually included: hole injection materials, hole transport materials, electron transport materials, and luminescent materials (including host materials and guest materials). At present, electron transport materials, as an important functional material, have a direct impact on the mobility of electrons and ultimately affect the luminous efficiency of OLEDs. The low mobility of commercial electron transport materials is an important limiting factor in the development of device performance. It is worth doing more exploration to develop materials with higher mobility. Summary of the invention

[0004] The purpose of the present application is to provide a compound which, when used as an electron transport material, can improve the working efficiency and extend the service life of an organic electroluminescent device.

[0005] The first aspect of the present application provides a compound of formula (I):

[0006]

[0007] in,

[0008] Ar 1 ,Ar 2 Selected from C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C30 heteroarylene;

[0009] R is selected from hydrogen, C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30 heteroarylene;

[0010] L 1 ,L 2 Selected from chemical bonds, unsubstituted or Rc-substituted C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30 heteroarylene;

[0011] X 1 -X 3 is selected from C or N, and at least one is selected from N; Y 1 -Y 3 is selected from C or N, and at least one is selected from N;

[0012] The heteroatoms on the arylene group or the heteroarylene group are each independently selected from O, S or N;

[0013] The substituents Rc of each group are each independently selected from deuterium, halogen, nitro, cyano, C1-C4 alkyl, phenyl, biphenyl, terphenyl or naphthyl.

[0014] The second aspect of the present application provides an electron transport material, which comprises at least one of the compounds provided in the first aspect of the present application.

[0015] The third aspect of the present application provides an organic electroluminescent device, which comprises at least one of the electron transport materials provided in the second aspect of the present application.

[0016] A fourth aspect of the present application provides a display device, which includes the organic electroluminescent device provided by the third aspect of the present application.

[0017] The compound provided by the present application has a parent structure of a multi-substituted pyridine fragment, high bond energy between atoms, good thermal stability, and is conducive to solid-state stacking between molecules. When used as an electron transport material, it has a suitable energy level between adjacent layers, which is conducive to the injection and migration of excitons, and can effectively reduce the driving voltage. At the same time, the fragment with pyridine as the central structure is conducive to the distribution of LUMO energy levels, expands the electron cloud conjugation, has a high electron migration rate, and can achieve good luminous efficiency and service life in organic electroluminescent devices. The compound of the present application has a larger conjugated plane, is conducive to molecular stacking, exhibits good thermodynamic stability, and is manifested as a long life in the device. The organic electroluminescent device of the present application includes the compound of the present application as an electron transport material, which can effectively reduce the driving voltage, improve the luminous efficiency, and extend the service life of the organic electroluminescent device. The display device provided by the present application has an excellent display effect.

[0018] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A schematic diagram of the structure of a typical organic electroluminescent device is shown. DETAILED DESCRIPTION

[0020] The following specific embodiments illustrate the implementation of the present invention, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. Although the description of the present invention will be introduced in conjunction with the preferred embodiment, this does not mean that the features of this invention are limited to this implementation. On the contrary, the purpose of introducing the invention in conjunction with the implementation is to cover other options or modifications that may extend based on the claims of the present invention. In order to provide a deep understanding of the present invention, the following description will include many specific details. The present invention can also be implemented without using these details. In addition, in order to avoid confusion or blurring the focus of the present invention, some specific details will be omitted in the description. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

[0021] In a first aspect, the present application provides a compound of formula (I):

[0022]

[0023] in,

[0024] Ar 1 ,Ar 2 Selected from C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30heteroarylene;

[0025] R is selected from hydrogen, C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30 heteroarylene;

[0026] L 1 ,L 2 Selected from chemical bonds, unsubstituted or Rc-substituted C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30 heteroarylene;

[0027] X 1 -X 3 is selected from C or N, and at least one is selected from N; Y 1 -Y 3 is selected from C or N, and at least one is selected from N;

[0028] The heteroatoms on the arylene group or the heteroarylene group are each independently selected from O, S or N;

[0029] The substituents Rc of each group are each independently selected from deuterium, halogen, nitro, cyano, C1-C4 alkyl, phenyl, biphenyl, terphenyl or naphthyl.

[0030] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

[0031] Preferably, L 1 and L 2 Each independently selected from a chemical bond, a C6-C 18 Arylene, unsubstituted or Rc-substituted C3-C 18 Heteroarylene.

[0032] More preferably, Ar 1 ,Ar 2 A subunit selected from the following compounds which are unsubstituted or substituted with Rc: benzene, biphenyl, terphenyl, naphthalene, phenanthrene, triphenylene, fluorene, pyridine, pyridazine, pyrimidine, pyrazine, quinoline, isoquinoline, quinazoline, quinoxaline, cinnoline, naphthyridine, triazine, pyridopyrazine, dibenzofuran, aza-dibenzofuran, dibenzothiophene, aza-dibenzothiophene, 9,9-dimethylfluorene, spirofluorene.

[0033] For example, the compound of formula (I) can be selected from the compounds shown in the following A1 to A20:

[0034]

[0035]

[0036] The compound of formula (I) provided in the present application has high bond energy between atoms, good thermal stability, and is conducive to solid-state stacking between molecules. In addition, the preparation process of the compound of formula (I) provided in the present application is simple and easy, and the raw materials are easily available, which is suitable for industrial production.

[0037] The second aspect of the present application provides an electron transport material, which comprises at least one of the compounds provided in the first aspect of the present application.

[0038] When the compound of the present application is used as an electron transport material, it has a matching energy level between adjacent layers, which is conducive to the injection and migration of electrons and can effectively reduce the driving voltage. At the same time, it has a high electron migration rate and can achieve good luminous efficiency and service life in an organic electroluminescent device. It also has a large conjugated plane, which is conducive to molecular stacking and shows good thermodynamic stability. Use in an organic electroluminescent device can extend its service life.

[0039] The third aspect of the present application provides an organic electroluminescent device, which comprises at least one of the electron transport materials provided in the second aspect of the present application. Therefore, the organic electroluminescent device provided in the present application has low driving voltage, high luminous efficiency and long service life.

[0040] In the present application, there is no particular limitation on the type and structure of the organic electroluminescent device, and it can be any organic electroluminescent device of different types and structures known in the art, as long as the electron transport material provided in the present application can be used.

[0041] The organic electroluminescent device of the present application may be a light-emitting device with a top-emitting structure, which may include an anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer, and a transparent or semi-transparent cathode in sequence on a substrate.

[0042] The organic electroluminescent device of the present application may also be a light-emitting device with a bottom emission structure, which may include a transparent or semi-transparent anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer and a cathode structure in sequence on a substrate.

[0043] The organic electroluminescent device of the present application may also be a light-emitting device with a double-sided light-emitting structure, which may include a transparent or semi-transparent anode, a hole injection layer, a hole transport layer, a light-emitting layer, an electron transport layer, an electron injection layer and a transparent or semi-transparent cathode structure in sequence on a substrate.

[0044] In addition, there may be an electron blocking layer between the hole transport layer and the light-emitting layer, there may be a hole blocking layer between the light-emitting layer and the electron transport layer, and a light extraction layer may be provided on the transparent electrode on the light-emitting side. However, the structure of the organic electroluminescent device of the present application is not limited to the above-mentioned specific structure, and the above-mentioned layers may be omitted or increased if necessary. The present application has no particular restrictions on the thickness of the above-mentioned layers, as long as the purpose of the present application can be achieved. For example, the organic electroluminescent device may include an anode made of metal, a hole injection layer (5nm to 20nm), a hole transport layer (80nm to 140nm), an electron blocking layer (5nm to 20nm), a light-emitting layer (150nm to 400nm), a hole blocking layer (5nm to 20nm), an electron transport layer (300nm to 800nm), an electron injection layer (5nm to 20nm), a transparent or semi-transparent cathode, and a light extraction layer (50nm to 90nm) on a substrate in sequence.

[0045] Figure 1 A schematic diagram of a typical organic electroluminescent device is shown, wherein, from bottom to top, a substrate 1, a reflective anode electrode 2, a hole injection layer 3, a hole transport layer 4, a light-emitting layer 5, an electron transport layer 6, an electron injection layer 7, and a cathode electrode 8 are arranged in sequence.

[0046] Understandably, Figure 1 Only a typical structure of an organic electroluminescent device is schematically shown, and the present application is not limited to this structure. The electron transport material of the present application can be used in any type of organic electroluminescent device.

[0047] For convenience, the following reference Figure 1 The organic electroluminescent device of the present application is described, but this does not mean any limitation on the protection scope of the present application. It can be understood that all organic electroluminescent devices that can use the electron transport material of the present application are within the protection scope of the present application.

[0048] In the present application, the substrate 1 is not particularly limited, and conventional substrates used in organic electroluminescent devices in the prior art may be used, such as glass, polymer materials, and glass and polymer materials with thin film transistor (TFT) components.

[0049] In the present application, the reflective anode material 2 is not particularly limited and can be selected from transparent conductive materials such as indium tin oxide (ITO), indium zinc oxide (IZO), tin dioxide (SnO2), zinc oxide (ZnO) known in the prior art, or metal materials such as silver and its alloys, aluminum and its alloys, or organic conductive materials such as poly (3,4-ethylenedioxythiophene) (PEDOT), or multilayer structures of the above materials.

[0050] In the present application, the material of the hole injection layer 3 is not particularly limited, and can be made of hole injection layer materials known in the art. For example, at least one of the known hole transport materials (HTM) is selected as the hole injection material.

[0051] In the present application, the hole injection layer 3 may further include a p-type dopant, and the type of the p-type dopant is not particularly limited, and various p-type dopants known in the art may be used. For example, the p-type dopant may be selected from but not limited to at least one of the following p-1 to p-3 compounds:

[0052]

[0053] In the present application, the amount of the p-type dopant is not particularly limited and may be an amount known to those skilled in the art.

[0054] In the present application, the material of the hole transport layer 4 is not particularly limited, and can be made of hole transport materials (HTM) known in the art. The number of layers of the hole transport layer 4 is not particularly limited, and can be adjusted according to actual needs, as long as it can meet the purpose of the present application, for example, 1 layer, 2 layers, 3 layers, 4 layers or more layers.

[0055] For example, the HTM for the hole injection layer material and the HTM for the hole transport layer material may be selected from, but not limited to, at least one of the following HT-1 to HT-31 compounds:

[0056]

[0057]

[0058] In the present application, the light-emitting layer 5 may include a blue light-emitting layer, a green light-emitting layer or a red light-emitting layer. The light-emitting material in the light-emitting layer 5 is not particularly limited, and various light-emitting materials known to those skilled in the art may be used. For example, the material of the light-emitting layer 5 may include a host material and a guest material.

[0059] In the present application, the host material may be selected from but not limited to at least one of the following BH-1 to BH-10 compounds:

[0060]

[0061] In the present application, the guest material is not particularly limited, and at least one of the light-emitting layer guest materials known in the art can be used. For example, the light-emitting layer guest material can be selected from but not limited to at least one of the following BD-1 to BD-9 compounds:

[0062]

[0063] In the present application, the amount of the guest material in the light-emitting layer is not particularly limited and can be an amount known to those skilled in the art.

[0064] In the present application, the electron transport layer 6 comprises at least one of the electron transport materials of the present application, and the electron transport layer 6 may also comprise a combination of at least one of the electron transport materials of the present application and at least one of the known electron transport materials. The number of layers of the electron transport layer 6 is not particularly limited and can be adjusted according to actual needs, as long as the purpose of the present application can be met, for example, 1 layer, 2 layers, 3 layers, 4 layers or more layers.

[0065] For example, the known electron transport material may be selected from, but not limited to, at least one of the following ET-1 to ET-57 compounds:

[0066]

[0067]

[0068]

[0069] In the present application, the electron transport layer 6 may further include an n-type dopant. The type of the n-type dopant is not particularly limited, and various n-type dopants known in the art may be used. For example, the following n-type dopants may be used:

[0070]

[0071] In the present application, the amount of the n-type dopant is not particularly limited and can be an amount known to those skilled in the art.

[0072] In the present application, the material of the electron injection layer 7 is not particularly limited, and electron injection materials known in the art can be used, for example, including but not limited to at least one of the materials such as LiQ, LiF, NaCl, CsF, Li2O, Cs2CO3, BaO, Na, Li, Ca, etc. in the prior art.

[0073] In the present application, the material of the cathode electrode 8 is not particularly limited, and can be selected from but not limited to magnesium-silver mixture, LiF / Al, ITO, Al and other metals, metal mixtures, oxides and the like.

[0074] The fourth aspect of the present application provides a display device, which includes the organic electroluminescent device provided in the third aspect of the present application. The display device includes but is not limited to a display, a television, a tablet computer, a mobile communication terminal, etc.

[0075] The method for preparing the organic electroluminescent device of the present application is not particularly limited, and any method known in the art may be used. For example, the present application may be prepared by the following preparation method:

[0076] (1) cleaning the reflective anode electrode 2 on the top-emitting OLED device substrate 1 by using a cleaning machine through steps such as chemical cleaning, water cleaning, brushing, high-pressure water cleaning, and air knife cleaning, and then performing a heat treatment;

[0077] (2) vacuum evaporating a hole injection material on the reflective anode electrode 2 to form a hole injection layer 3;

[0078] (3) vacuum evaporating a hole transport material on the hole injection layer 3 to form a hole transport layer 4;

[0079] (4) vacuum evaporating a light-emitting layer 5 on the hole transport layer 4, wherein the light-emitting layer 5 contains a host material and a guest material;

[0080] (5) vacuum evaporating an electron transport material on the light emitting layer 5 to form an electron transport layer 6;

[0081] (6) vacuum evaporating an electron injection material on the electron transport layer 6 to form an electron injection layer 7;

[0082] (7) A cathode material is vacuum-deposited on the electron injection layer 7 to form a cathode electrode 8 .

[0083] The above only describes a typical structure of an organic electroluminescent device and its preparation method. It should be understood that the present application is not limited to this structure. The electron transport material of the present application can be used in an organic electroluminescent device of any structure, and the organic electroluminescent device can be prepared by any preparation method known in the art.

[0084] The synthesis method of the compound of the present application is not particularly limited, and any method known to those skilled in the art can be used for synthesis. The following examples illustrate the synthesis process of the compound of the present application.

[0085] Synthesis Example 1: Synthesis of Compound A1:

[0086]

[0087] Add 100mmol of 2-bromo-5-chloropyridine, 100mmol of 2-naphthaleneboronic acid, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M1. (MS: 239.7)

[0088] Add 100 mmol of M1, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M2. (MS: 331.2)

[0089] Add 100 mmol of 2,6-dibromopyridine, 200 mmol of M2, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A1. (MS: 485.6)

[0090] 1 H NMR(400MHz,Chloroform)δ9.29(s,2H),8.85(s,2H),8.35(d,J=8.8Hz,2H),8.26(d,J=8.8 Hz,2H),8.15(d,J=8.4Hz,1H),8.10-7.95(m,8H),7.65-7.51(m,4H),7.42(d,J=8.0Hz,2H).

[0091] Synthesis Example 2: Synthesis of Compound A7:

[0092]

[0093] Add 100mmol of 2-bromo-5-chloropyridine, 100mmol of phenylboric acid, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M1. (MS: 189.6)

[0094] Add 100 mmol of M1, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M2. (MS: 281.1)

[0095] Add 100mmol of M1, 200mmol of M2, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M3. (MS: 419.9)

[0096] Add 100 mmol of M2, 100 mmol of M3, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A7. (MS: 538.6)

[0097] 1 H NMR (400MHz, Chloroform) δ9.29 (s, 2H), 9.24 (s, 1H), 8.88 (s, 2H), 8.70 (d, J = 9.2Hz, 1H), 8.35 (d,J=7.6Hz,5H),8.22(d,J=7.2Hz,2H),8.01(d,J=8.0Hz,2H),7.60-7.43(m,7H),7.25(s,4H).

[0098] Synthesis Example 3: Synthesis of Compound A9:

[0099]

[0100] Add 100mmol of 2-bromo-5-chloropyridine, 100mmol of 2-naphthaleneboronic acid, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1. (MS: 189.6)

[0101] Add 100 mmol of M1, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M2. (MS: 281.1)

[0102] Add 100 mmol of M2, 100 mmol of p-chlorobromobenzene, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M3. (MS: 265.7)

[0103] Add 100 mmol of M3, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4. (MS: 357.2)

[0104] Add 100 mmol of M4, 200 mmol of 2,6-dibromopyridine, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A9. (MS: 537.7)

[0105] 1 H NMR(400MHz,Chloroform)δ8.92(s,2H),8.69(d,J=10.0Hz,4H),8.33(d,J=9.2Hz,4H),8.01(d,J=8.0Hz,2H), 7.91(d,J=9.6Hz,2H),7.61-7.48(m,6H),7.31-7.20(m,4H),7.15(d,J=10.0Hz,1H),6.74(d,J=10.0Hz,2H),.

[0106] Synthesis Example 4: Synthesis of Compound A10:

[0107]

[0108] Add 100mmol of 2-bromo-5-chloropyridine, 100mmol of 2-naphthaleneboronic acid, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M1. (MS: 189.6)

[0109] Add 100 mmol of M1, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M2. (MS: 281.1)

[0110] Add 100 mmol of M2, 100 mmol of 2-bromo-5-chloropyridine, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M3. (MS: 266.7)

[0111] Add 100 mmol of M3, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4. (MS: 358.2)

[0112] Add 100 mmol of M4, 200 mmol of 2,6-dibromopyridine, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A10. (MS: 539.8)

[0113] 1 H NMR(400MHz,Chloroform)δ9.46(s,2H),9.27(s,2H),8.55(d,J=7.6Hz,2H),8.33(d,J=7.2H z,4H),8.25-8.03(m,5H),8.01(d,J=7.6Hz,2H),7.58-7.46(m,6H),7.42(d,J=10.0Hz,2H).

[0114] Synthesis Example 5: Synthesis of Compound A13:

[0115]

[0116] Add 100mmol of 2-bromo-5-chloropyridine, 100mmol of phenylboric acid, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M1. (MS: 189.6)

[0117] Add 100 mmol of M1, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M2. (MS: 281.1)

[0118] Add 100mmol of 2,6-dibromo-4-chloropyridine, 200mmol of M2, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M3. (MS: 419.9)

[0119] Add 100 mmol of 5-chlorophenanthroline, 100 mmol of p-chlorophenylboric acid, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4. (MS: 290.7)

[0120] Add 100 mmol of M4, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M5. (MS: 382.3)

[0121] Add 100 mmol of M3, 100 mmol of M5, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A13. (MS: 639.7)

[0122] 1 H NMR(400MHz,Chloroform)δ9.30(s,1H),8.88(s,1H),8.82(d,J=8.0Hz,1H),8.65(d,J=8.0Hz,1H),8.38-8.30(m,4H),8.25 (d,J=8.4Hz,2H),8.15-8.06(m,2H),8.01(d,J=8.4Hz,2H),7.89(s,1H),7.60-7.45(m,6H),7.45-7.31(m,2H),7.26(s,4H).

[0123] Synthesis Example 6: Synthesis of Compound A19:

[0124]

[0125] Add 100mmol of 2-bromo-5-chloropyridine, 100mmol of phenylboric acid, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M1. (MS: 189.6)

[0126] Add 100 mmol of M1, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M2. (MS: 281.1)

[0127] Add 100 mmol of M2, 100 mmol of 2-bromo-5-chloropyridine, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M3. (MS: 266.7)

[0128] Add 100 mmol of M3, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M4. (MS: 358.2)

[0129] Add 100 mmol of M4, 100 mmol of 2,6-dibromo-4-chloropyridine, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M5. (MS: 421.7)

[0130] Add 100mmol of 2-bromo-5-chloropyridine, 100mmol of pyridine-3-boric acid, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M6. (MS: 190.6)

[0131] Add 100 mmol of M6, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M7. (MS: 282.1)

[0132] Add 100mmol of M7, 100mmol of 2-bromo-5-chloropyridine, 41.4g of potassium carbonate (300mmol), 800ml of tetrahydrofuran (THF) and 200ml of water to the reaction flask, and add 1mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12h. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and the obtained solid is recrystallized and purified with toluene to obtain white powder M8. (MS: 266.7)

[0133] Add 100 mmol of M8, 100 mmol of biboric acid pinacol ester, 41.4 g of potassium carbonate (300 mmol), 800 ml of dioxane, and 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4) to the reaction flask, and react at 100°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M9. (MS: 358.2)

[0134] Add 100 mmol of M5, 100 mmol of M9, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder M10. (MS: 573.1)

[0135] Add 100 mmol of M10, 100 mmol of phenylboric acid, 41.4 g of potassium carbonate (300 mmol), 800 ml of tetrahydrofuran (THF) and 200 ml of water to the reaction flask, and add 1 mol% of tetrakis(triphenylphosphine)palladium (Pd(PPh3)4), and react at 60°C for 12 hours. After the reaction is completed, stop the reaction, cool the reactant to room temperature, add water, filter, wash with water, and purify the obtained solid by recrystallization with toluene to obtain white powder A19. (MS: 614.7)

[0136] 1H NMR(400MHz,Chloroform)δ9.63(s,1H),9.10(s,1H),8.92(s,1H),8.74–8.62(m,6H),8.33(d,J=10.0Hz,2H),8.25–8.1 7(m,4H),8.01(d,J=10.4Hz,1H),7.92(d,J=8.4Hz,1H),7.75(d,J=8.8Hz,2H),7.58-7.35(m,7H),7.25(s,J=8.4Hz,4H).

[0137] Other compounds of the present application can be synthesized by selecting suitable raw materials according to the ideas of the above-mentioned synthesis examples 1-6, or by selecting any other suitable method and raw materials for synthesis.

[0138] Example 1

[0139] The glass plate coated with the ITO transparent conductive layer was ultrasonically treated in a commercial cleaning agent, rinsed in deionized water, ultrasonically degreased in an acetone-ethanol mixed solvent, baked in a clean environment to completely remove the water, cleaned with ultraviolet light and ozone, and bombarded with a low-energy cation beam;

[0140] Then, the glass substrate with the anode is placed in a vacuum chamber and evacuated to less than 10 -5 A hole injection layer is vacuum-deposited on the anode layer film. The hole injection layer includes hole injection layer material HT-11 and p-type dopant p-1. The deposition is performed by a multi-source co-evaporation method. The deposition rate of the hole injection layer material HT-11 is adjusted to 0.1 nm / s, the deposition rate of the p-type dopant p-1 is adjusted to 3% of the deposition rate of the hole injection layer material HT-11, and the deposition film thickness is 10 nm. The hole injection layer material HT-11 and the p-type dopant p-1 are as follows:

[0141]

[0142] Then, a hole transport material HT-5 was vacuum-deposited on the hole injection layer as a hole transport layer, wherein the evaporation rate was 0.1 nm / s, the evaporation film thickness was 80 nm, and the hole transport material HT-5 was as follows:

[0143]

[0144] Then, a light-emitting layer is vacuum-deposited on the hole transport layer. The light-emitting layer includes a main material BH-2 and a fluorescent dopant BD-1. The deposition is performed by a multi-source co-evaporation method. The deposition rate of the main material BH-2 is adjusted to 0.1 nm / s, the deposition rate of the fluorescent dopant BD-1 is adjusted to 3% of the deposition rate of the main material BH-2, and the deposition film thickness is 30 nm. The main material BH-2 and the fluorescent dopant BD-1 are as follows:

[0145]

[0146] Then, an electron transport layer is vacuum evaporated on the light-emitting layer. The electron transport material is compound A1, which is evaporated with LiQ to form the electron transport layer. The evaporation rate of compound A1 is 0.1 nm / s, the evaporation ratio of compound A1 to LiQ is 50:50, and the evaporation film thickness is 30 nm. The electron transport material A1 is as follows:

[0147]

[0148] Then, LiF with a thickness of 5 nm was vacuum-deposited on the electron transport layer as an electron injection layer, wherein the evaporation rate was 0.1 nm / s;

[0149] Finally, an Al layer with a thickness of 150 nm was vacuum evaporated on the electron injection layer as a cathode electrode of the organic electroluminescent device, wherein the evaporation rate was 0.1 nm / s.

[0150] Embodiment 2-6

[0151] Except that the electron transport materials are replaced by A7, A9, A10, A13 and A19 respectively, the rest is the same as Example 1. See Table 1 for details.

[0152] Comparative Example 1

[0153] Except that ET-13 is selected as the electron transport material, the rest is the same as Example 1; ET-13 is as follows:

[0154]

[0155] The organic electroluminescent device prepared by the above process was subjected to the following performance tests:

[0156] At the same brightness, the driving voltage, current efficiency and device life of the organic electroluminescent devices prepared in Examples 1-6 and Comparative Example 1 were measured using a digital source meter and a brightness meter. Specifically, the voltage was increased at a rate of 0.1 V per second, and the brightness of the organic electroluminescent device was measured when it reached 1000 cd / m 2The voltage at which the light is on is the driving voltage, and the current density at this time is measured at the same time; the ratio of brightness to current density is the current efficiency; the life test of LT95 is as follows: use a brightness meter at 1000cd / m 2 At the same brightness, the current is kept constant and the brightness of the organic electroluminescent device is measured to drop to 950cd / m 2 The time is in hours. The results are shown in Table 1.

[0157] Table 1 Performance results of organic electroluminescent devices

[0158]

[0159] As can be seen from Table 1, the compounds A1, A7, A9, A10, A13, and A19 prepared in the present application are used as electron transport materials in organic electroluminescent devices, which can effectively reduce the driving voltage, improve the current efficiency, and extend the service life of the device. The materials of the present invention have significant performance improvements in improving efficiency and extending life, and are electron transport materials with good performance.

[0160] Example 7

[0161] The glass plate coated with the ITO transparent conductive layer was ultrasonically treated in a commercial cleaning agent, rinsed in deionized water, ultrasonically degreased in an acetone-ethanol mixed solvent, baked in a clean environment to completely remove the water, cleaned with ultraviolet light and ozone, and bombarded with a low-energy cation beam;

[0162] Then, the glass substrate with the anode is placed in a vacuum chamber and evacuated to less than 10 -5 A hole injection layer is vacuum-deposited on the anode layer film. The hole injection layer includes hole injection layer material HT-11 and p-type dopant p-1. The deposition is performed by a multi-source co-evaporation method. The deposition rate of the hole injection layer material HT-11 is adjusted to 0.1 nm / s, the deposition rate of the p-type dopant p-1 is adjusted to 3% of the deposition rate of the hole injection layer material HT-11, and the deposition film thickness is 10 nm. The hole injection layer material HT-11 and the p-type dopant p-1 are as follows:

[0163]

[0164] Then, a hole transport material HT-5 was vacuum-deposited on the hole injection layer as a hole transport layer, wherein the evaporation rate was 0.1 nm / s, the evaporation film thickness was 80 nm, and the hole transport material HT-5 was as follows:

[0165]

[0166] Then, a light-emitting layer is vacuum-deposited on the hole transport layer. The light-emitting layer includes a main material BH-2 and a fluorescent dopant BD-1. The deposition is performed by a multi-source co-evaporation method. The deposition rate of the main material BH-2 is adjusted to 0.1 nm / s, the deposition rate of the fluorescent dopant BD-1 is adjusted to 3% of the deposition rate of the main material BH-2, and the deposition film thickness is 30 nm. The main material BH-2 and the fluorescent dopant BD-1 are as follows:

[0167]

[0168] Then, an electron transport layer is vacuum evaporated on the light-emitting layer. The electron transport material is compound ET-13 and LiQ evaporated to form the electron transport layer. The evaporation rate of compound ET-13 is 0.1 nm / s, the evaporation ratio of compound ET-13 to LiQ is 50:50, and the evaporation film thickness is 30 nm. ET-13 is as follows:

[0169]

[0170] The above is the first light-emitting unit;

[0171] On the first light-emitting unit, the A1 compound and metal Yb were evaporated at a rate ratio of (99:1) to form an n-type charge generation layer of 10nm, and then the hole injection layer material HT-11 and the p-type dopant p-1 were evaporated at a rate ratio of (99:1) to form a 10nm layer;

[0172] Vapor depositing a second light-emitting unit identical to the first light-emitting unit on the charge generation layer;

[0173] Then, LiF with a thickness of 0.5 nm was vacuum-deposited on the electron transport layer as an electron injection layer, wherein the evaporation rate was 0.1 nm / s;

[0174] Finally, an Al layer with a thickness of 150 nm was vacuum evaporated on the electron injection layer as a cathode electrode of the organic electroluminescent device, wherein the evaporation rate was 0.1 nm / s.

[0175] Examples 8-12

[0176] Except that the charge generation layer is replaced by A7, A9, A10, A13, A19 respectively, the rest is the same as Example 7. See Table 2 for details.

[0177] Comparative Example 2

[0178] Except that ET-G is used as the material of the charge generation layer instead of A1, the rest is the same as Example 1; ET-G is as follows:

[0179]

[0180] The organic electroluminescent device prepared by the above process was subjected to the following performance tests:

[0181] At the same brightness, the driving voltage, current efficiency and device life of the organic electroluminescent devices prepared in Examples 7-12 and Comparative Example 2 were measured using a digital source meter and a brightness meter. Specifically, the voltage was increased at a rate of 0.1 V per second, and the brightness of the organic electroluminescent device was measured when it reached 1000 cd / m 2 The voltage at which the light is on is the driving voltage, and the current density at this time is measured at the same time; the ratio of brightness to current density is the current efficiency; the life test of LT95 is as follows: use a brightness meter at 1000cd / m 2 At the same brightness, the current is kept constant and the brightness of the organic electroluminescent device is measured to drop to 950cd / m 2 The time is in hours. The results are shown in Table 2.

[0182] Table 2 Performance results of organic electroluminescent devices

[0183]

[0184] As can be seen from Table 2, the compounds A1, A7, A9, A10, A13, and A19 prepared in the present application are used as charge generating materials in organic electroluminescent devices, which can effectively reduce the driving voltage, improve the current efficiency, and extend the service life of the device. The materials of the present invention have significant performance improvements in improving efficiency and extending life, and are electron transport materials with good performance.

[0185] The above description is only a preferred embodiment of the present application and is not intended to limit the protection scope of the present application. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application are included in the protection scope of the present application.

Claims

1. A polysubstituted pyridine derivative compound, characterized in that: It has the structural formula (I): in, Ar 1 ,Ar 2 Selected from C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30 heteroarylene; R is selected from hydrogen, C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30 heteroarylene; L 1 ,L 2 Selected from chemical bonds, unsubstituted or Rc-substituted C6-C 30 Arylene, unsubstituted or Rc-substituted C5-C 30 heteroarylene; X 1 -X 3 is selected from C or N, and at least one is selected from N; Y 1 -Y 3 is selected from C or N, and at least one is selected from N; The heteroatoms on the arylene group or the heteroarylene group are each independently selected from O, S or N; The substituents Rc of each group are each independently selected from deuterium, halogen, nitro, cyano, C1-C4 alkyl, phenyl, biphenyl, terphenyl or naphthyl.

2. The polysubstituted pyridine derivative compound according to claim 1, characterized in that: The R is selected from the subunits of the following compounds which are chemically bonded, unsubstituted or substituted by Rc: benzene, biphenyl, terphenyl, naphthalene, phenanthrene, triphenylene, fluorene, pyridine, pyridazine, pyrimidine, pyrazine, quinoline, isoquinoline, quinazoline, quinoxaline, cinnoline, naphthyridine, triazine, phenanthroline, dibenzofuran, aza-dibenzofuran, dibenzothiophene, aza-dibenzothiophene, 9,9-dimethylfluorene, and spirofluorene.

3. The polysubstituted pyridine derivative compound according to claim 1, characterized in that: The Ar 1 ,Ar 2 A subunit selected from the following compounds which are unsubstituted or substituted with Rc: benzene, biphenyl, terphenyl, naphthalene, phenanthrene, triphenylene, fluorene, pyridine, pyridazine, pyrimidine, pyrazine, quinoline, isoquinoline, quinazoline, quinoxaline, cinnoline, naphthyridine, triazine, pyridopyrazine, dibenzofuran, aza-dibenzofuran, dibenzothiophene, aza-dibenzothiophene, 9,9-dimethylfluorene, spirofluorene.

4. The polysubstituted pyridine derivative compound according to claim 1, characterized in that: The L 1 ,L 2 A subunit selected from the following compounds which are chemically bonded, unsubstituted or substituted with Rc: benzene, biphenyl, terphenyl, naphthalene, phenanthrene, triphenylene, fluorene, pyridine, pyridazine, pyrimidine, pyrazine, quinoline, isoquinoline, quinazoline, quinoxaline, cinnoline, naphthyridine, pyridopyrazine, dibenzofuran, aza-dibenzofuran, dibenzothiophene, aza-dibenzothiophene, 9,9-dimethylfluorene, spirofluorene.

5. The polysubstituted pyridine derivative compound according to claim 1, characterized in that: The compound of formula (I) is selected from the following compounds A1 to A20:

6. An electron transport material, characterized in that Contains at least one of the polysubstituted pyridine derivative compounds described in any one of claims 1 to 5.

7. An organic electroluminescent device, characterized in that: Contains at least one of the electron transport materials described in claim 6.

8. A display device, characterized in that: An organic electroluminescent device comprising the organic electroluminescent device according to claim 7.

Citation Information

Cited By

  • Compound containing phenanthroline and application thereof

    CN117986252A