Bipolar organic material, preparation method, application, positive pole piece and sodium ion battery

By using bipolar organic materials with hydroxyl and furan ring structures in sodium ion batteries, the problems of poor structural stability and high cost of the positive electrode materials of sodium ion batteries are solved, and high specific capacity and good cycle stability are achieved. Commercialization process of sodium ion batteries.

CN118955437AInactive Publication Date: 2024-11-15DEEPAL AUTOMOBILE TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411043822.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The positive electrode materials of existing sodium ion batteries have poor structural stability, high cost and potential environmental and health risks. The organic electrode materials are easily soluble in sodium ion batteries and have low electron conductivity, resulting in rapid capacity decay and poor rate performance.

Method used

Using a bipolar organic material with hydroxy units and furan rings in its chemical structure, the material is prepared by a specific preparation method, including the use of 2,5-dimethoxybenzene boric acid, cesium carbonate and tetrakis(tria) Phenylphosphine) palladium is mixed, 2,5-dibromofuran and tetrahydrofuran are added, and then heated and refluxed, followed by addition of cerium ammonium nitrate solution for reaction, and the bipolar organic material is obtained by recrystallization.

Benefits of technology

This bipolar organic material has excellent discharge capacity and cycle stability, high structural stability, low cost and environmentally friendly, and can adapt to the deintercalation of ions of different sizes, which significantly improves the specific capacity and rate performance of sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955437A_ABST
    Figure CN118955437A_ABST
Patent Text Reader

Abstract

The invention relates to a bipolar organic material, a preparation method and application thereof, a positive pole piece and a sodium ion battery. The structure of the bipolar organic material is shown as a formula I, the invention also provides a preparation method of the bipolar organic material, which comprises the following steps: mixing 2, 5-dimethoxyphenylboronic acid, cesium carbonate and tetrakis (triphenylphosphine) palladium, adding tetrahydrofuran and water, and heating and refluxing to obtain an intermediate; acetonitrile is added into the intermediate, ceric ammonium nitrate is added after cooling, heating reaction, separation and recrystallization are performed, and the compound is obtained. The invention also provides application of the bipolar organic material as an electrode active material. The invention also provides a positive pole piece adopting the bipolar organic material as a positive active material. The invention also provides a sodium ion battery adopting the positive pole piece as a positive pole. According to the invention, the problems of poor structural stability and potential environmental and health risks of the existing inorganic electrode material are solved, and the problems of fast capacity fading and poor rate capability of the existing battery are also solved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of organic electrode materials, and in particular to a bipolar organic material, a preparation method, an application, a positive electrode sheet and a sodium ion battery. Background Art

[0002] With the rapid expansion of the electronic products, electric vehicles and energy storage power station markets, the demand for batteries has exploded. Gradually developed lithium-ion batteries such as lithium cobalt oxide, lithium manganese oxide, nickel cobalt manganese oxide, nickel cobalt aluminum oxide, lithium iron phosphate and lithium titanate have high energy density and excellent performance, but are limited by the scarcity and high prices of key raw materials such as nickel salts, cobalt salts, manganese salts and lithium salts, making the preparation cost of lithium-ion batteries high, which has become a bottleneck restricting its further development.

[0003] Compared with lithium-ion batteries, sodium-ion batteries (SIBs) have gradually attracted widespread attention in the industry due to their advantages of abundant reserves and low prices of sodium salt raw materials. As a potential substitute and supplement for lithium-ion batteries, sodium-ion batteries show great application potential in the field of large-scale energy storage. However, as one of the key factors affecting the energy density, specific capacity, rate performance and cycle performance of sodium-ion batteries, the performance of the cathode material directly determines the overall performance of the battery.

[0004] At present, the positive electrode materials of sodium ion batteries mainly include inorganic electrode materials such as transition metal layered oxides and polyanion compounds. For example, the layered oxide positive electrode material and its preparation method, positive electrode sheet and sodium ion secondary battery disclosed in CN117317213 A, the chemical composition of the layered oxide positive electrode material is Na x Ni a Mn b M1 c M2 d O2. The preparation method of the layered oxide positive electrode material is: weighing a nickel source, a manganese source, and an M2 source to prepare a hydroxide precursor; taking at least one raw material in the M1 source or taking at least one raw material in the M1 source and at least one raw material in the M2 source, and then mixing with a sodium source raw material and a hydroxide precursor and sintering to obtain a layered oxide positive electrode material. However, these inorganic electrode materials have the following problems: first, the presence of transition metals in inorganic motor materials leads to high costs; second, large-radius sodium ion deintercalation can easily cause poor structural stability; third, there are potential environmental and health risks, which limits their promotion in practical applications.

[0005] In contrast, organic materials have shown great potential in the field of positive electrode materials for sodium-ion batteries with their unique advantages. However, there are also some challenges when organic materials are used as positive electrode materials for sodium-ion batteries. For example, organic electrode materials are easily soluble in organic electrolytes, resulting in rapid capacity decay; at the same time, the electronic conductivity of organic matter is low, resulting in poor rate performance of the material. Therefore, in order to solve the problems of the above-mentioned organic materials as positive electrode materials for sodium-ion batteries, the development of a new type of organic small molecule electrode material with high specific capacity and good stable cyclability is of great significance to promoting the commercialization of sodium-ion batteries. Summary of the invention

[0006] In view of the shortcomings of the prior art, one of the objects of the present invention is to provide a bipolar organic material, a preparation method and an application to solve the problems of poor structural stability, high cost and potential environmental and health risks of existing inorganic electrode materials. The second object of the present invention is to provide a positive electrode plate and a sodium ion battery to solve the problems of fast capacity decay and poor rate performance of existing sodium ion batteries.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A bipolar organic material, the structure of which is shown in Formula I:

[0009]

[0010] It has been determined that the chemical structure of the bipolar organic material contains both electrochemically active hydroxyl units and furan ring units, which reflects the bipolar characteristics. When used as an electrode material, it has excellent discharge capacity and cycle stability. The bipolar organic material has a large molecular distance, which can adapt to the insertion and extraction of ions of various sizes, and has a fluffy structure, so that when it is used as an electrode material, it not only has a small structural change, but also is conducive to the transmission of ions, and has the advantage of high structural stability, which solves the problem of poor structural stability of existing inorganic electrode materials. The bipolar organic material is composed of abundant carbon, hydrogen and oxygen elements, with a wide source, low price, and environmentally friendly, which solves the potential environmental and health risks and high cost of existing inorganic electrode materials. Thus, it provides a new choice in the field of electrode materials.

[0011] The present invention also provides a method for preparing a bipolar organic material, comprising the following steps:

[0012] S1. Mix 2,5-dimethoxyphenylboronic acid, cesium carbonate and tetrakis(triphenylphosphine)palladium, place in an inert atmosphere, add 2,5-dibromofuran, tetrahydrofuran and water, heat to reflux, and cool to obtain an intermediate;

[0013] S2. Add acetonitrile to the intermediate, add cerium ammonium nitrate solution after cooling, heat to react, separate to obtain a precipitate, and recrystallize the precipitate to obtain a bipolar organic material.

[0014] The preparation method of the bipolar organic material is to mix 2,5-dimethoxyphenylboronic acid, cesium carbonate and tetrakis(triphenylphosphine)palladium, then add 2,5-dibromofuran, tetrahydrofuran and water, and heat and reflux to obtain an intermediate with high reaction activity, which is fully prepared for the successful preparation of the subsequent bipolar organic material; by using ammonium cerium nitrate as an oxidant and acetonitrile as a reaction medium, the bipolar organic material can be successfully prepared. Among them, the reaction in an inert atmosphere (such as nitrogen or argon) can prevent the influence of oxygen, moisture, etc. on the reaction, ensure the purity and efficiency of the reaction, and reduce the generation of by-products. Heating and reflux can promote the reaction and improve the yield and purity of the product. The heating reaction promotes the second step reaction and improves the yield and purity of the product. Recrystallization further improves the purity of the bipolar organic material. The preparation method has the advantages of low cost, simple operation, mild and easy-to-control process conditions, high efficiency and high purity, and is suitable for industrial large-scale production.

[0015] Preferably, the tetrakis(triphenylphosphine)palladium can be replaced by palladium acetate.

[0016] Among them, experiments have proved that the intermediate can also be successfully prepared by replacing tetrakis(triphenylphosphine)palladium with palladium acetate.

[0017] Preferably, the heating reflux temperature is 70°C to 80°C.

[0018] Preferably, the heating reflux temperature is 70°C.

[0019] Preferably, the heating reflux time is 72h to 96h.

[0020] Preferably, the heating reflux time is 72h.

[0021] Preferably, the molar ratio of the 2,5-dibromofuran, 2,5-dimethoxyphenylboric acid, tetrakis(triphenylphosphine)palladium and cesium carbonate is 1:2.1-2.4:0.03-0.05:3.3-3.5.

[0022] Preferably, the molar ratio of the 2,5-dibromofuran, 2,5-dimethoxyphenylboric acid, palladium acetate and cesium carbonate is 1:2.1-2.4:0.03-0.05:3.3-3.5.

[0023] Preferably, the inert atmosphere is selected from argon atmosphere.

[0024] Preferably, the temperature of the heating reaction is 30°C to 40°C.

[0025] Preferably, the temperature of the heating reaction is 35°C.

[0026] Preferably, the heating reaction time is 3 to 5 days.

[0027] Preferably, the heating reaction time is 3 days.

[0028] Preferably, the molar ratio of the intermediate to ammonium cerium nitrate is 1:6-8.

[0029] Preferably, in S1, after cooling to room temperature, the process further comprises: adding saturated brine to the cooled liquid, extracting with ethyl acetate or dichloromethane to obtain an organic phase, then drying the organic phase with anhydrous magnesium sulfate or anhydrous calcium sulfate, and separating and purifying the organic phase with a chromatographic column to obtain the intermediate.

[0030] Wherein, the chromatographic column is selected from a silica gel chromatographic column.

[0031] Preferably, S2 specifically includes: under inert atmosphere conditions, adding acetonitrile to the intermediate, mixing and cooling to 0°C, adding cerium ammonium nitrate solution, then heating to 35°C and stirring for reaction for 3 days, then adding water for ultrasonic treatment, separating and obtaining a precipitate; i washing the precipitate with dichloromethane and water at a temperature of 35°C to 45°C in sequence, and drying to obtain a crude product; and recrystallizing the crude product with 1,1,2,2-tetrachloroethane to obtain the bipolar organic material.

[0032] The present invention also provides an application of the bipolar organic material prepared by the preparation method of the present invention as an electrode active material of a battery.

[0033] Preferably, the bipolar organic material is used as a positive electrode active material of a battery.

[0034] Since the chemical structure of the bipolar organic material prepared by the present invention contains both electrochemically active hydroxyl units and furan ring units, when it is used as a positive electrode active material, the carbonyl unit can react with Na + For reversible storage, the furan ring unit can - The anions are reversibly stored, which effectively improves the battery's discharge capacity, rate performance and cycle stability. Especially for sodium ion batteries, the application effect is very significant.

[0035] Among them, the reaction equation of the energy storage mechanism of the bipolar organic material as the positive electrode active material is as follows:

[0036]

[0037] From the above reaction analysis, it can be seen that the carbonyl unit C=O functional group can reversibly deintercalate Na+, and the O atom near the furan unit can reversibly deintercalate A+. - (A- The reversible deintercalation of anions such as perchlorate, hexafluorophosphate or bis(trifluoromethanesulfonyl)imide is shown as follows: during discharge, the -1 The C=O characteristic peak disappears, and the double bond is reduced while storing a sodium ion to become CO-Na + During charging, CO weakens and the C=O peak reappears. At the same time, when charged to above 3.5V, a peak at 860cm -1 PF6 - The characteristic peak appears, but weakens in the subsequent discharge process. This is because the furan ring has electron-rich properties, storing an anion during charging and releasing it during discharge. This proves that the bipolar organic material of the present invention can simultaneously store sodium ions and anions to provide capacity during the cycle.

[0038] The present invention also provides a positive electrode plate, wherein the positive electrode active material in the positive electrode plate is selected from the bipolar organic material prepared by the preparation method of the present invention.

[0039] The present invention also provides a sodium ion battery using the positive electrode sheet of the present invention as a positive electrode.

[0040] Beneficial effects of the present invention:

[0041] The bipolar organic material of the present invention has a chemical structure in which both an electrochemically active hydroxyl unit and a furan ring unit exist, which reflects the bipolar characteristics. When used as an electrode material, it has excellent discharge capacity and cycle stability. The bipolar organic material has a large molecular distance, can adapt to the embedding and extraction of ions of various sizes, and has a fluffy structure, so that when it is used as an electrode material, not only the structural change is small, but also it is conducive to the transmission of ions, and has the advantage of high structural stability, which solves the problem of poor structural stability of existing inorganic electrode materials. The bipolar organic material is composed of abundant carbon elements, hydrogen elements and oxygen elements, has a wide source, low price, and is environmentally friendly, which solves the potential environmental and health risks of existing inorganic electrode materials, as well as the high cost problem. Thus, a new choice is provided in the field of electrode materials.

[0042] The preparation method of the bipolar organic material of the present invention can successfully prepare the bipolar organic material by heating reflux and heating reaction with 2,5-dimethoxyphenylboric acid, cesium carbonate, tetrakis(triphenylphosphine)palladium, 2,5-dibromofuran, tetrahydrofuran and ammonium cerium nitrate, and has the advantages of low cost, simple operation, mild and easy-to-control process conditions, high efficiency and high purity, and is suitable for industrial large-scale production.

[0043] The chemical structure of the bipolar organic material prepared by the present invention contains both hydroxyl units and furan ring units. When the bipolar organic material is used as a positive electrode active material, the carbonyl unit can react with Na+ For reversible storage, the furan ring unit can - The anions are reversibly stored, thereby effectively improving the battery's discharge capacity, rate performance and cycle stability, and has promotion and application value in the field of sodium ion battery technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 Schematic diagram of the structure of the H NMR spectrum of the intermediate prepared in Example 1;

[0045] Figure 2 is the infrared spectrum of the bipolar organic material prepared in Example 1;

[0046] Figure 3 This is an ex-situ infrared spectrum of the sodium ion battery prepared in Example 2;

[0047] Figure 4 This is a non-in-situ infrared spectrum of the sodium ion battery prepared in Control Example 2;

[0048] Figure 5 1 is a cyclic voltammetry result diagram of the sodium ion button cell prepared in Example 2;

[0049] Figure 6 Graph showing the cycle performance results of the sodium ion button batteries prepared in Example 2 and Control Example 2. DETAILED DESCRIPTION

[0050] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.

[0051] It should be noted that the illustrations provided in the following embodiments are only schematic illustrations of the basic concept of the present invention, and thus the drawings only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.

[0052] In the following description, numerous details are discussed to provide a more thorough explanation of the embodiments of the present application. However, it is obvious to those skilled in the art that the embodiments of the present application can be implemented without these specific details.

[0053] The present invention intends to disclose a bipolar organic material, a preparation method and an application to solve the problems of poor structural stability, high cost and potential environmental and health risks of existing inorganic electrode materials, and to disclose a positive electrode plate and a sodium ion battery to solve the problems of fast capacity decay and poor rate performance of existing sodium ion batteries.

[0054] The structure of the bipolar organic material is shown in Formula I:

[0055]

[0056] The chemical structure of the bipolar organic material contains both electrochemically active hydroxyl units and furan ring units, which reflects the bipolar characteristics. When used as an electrode material, it has excellent discharge capacity and cycle stability. The bipolar organic material has a large molecular distance, can adapt to the embedding and extraction of ions of various sizes, and has a fluffy structure, so that when it is used as an electrode material, not only the structure changes little, but also it is conducive to the transmission of ions, and has the advantage of high structural stability, which solves the problem of poor structural stability of existing inorganic electrode materials. The bipolar organic material is composed of abundant carbon, hydrogen and oxygen elements, has a wide source, is low in price, and is environmentally friendly, which solves the potential environmental and health risks and high cost of existing inorganic electrode materials.

[0057] In some embodiments, a method for preparing a bipolar organic material is provided, comprising the following steps:

[0058] S1. Mix 2,5-dimethoxyphenylboronic acid, cesium carbonate and tetrakis(triphenylphosphine)palladium, place in an inert atmosphere, add 2,5-dibromofuran, tetrahydrofuran and water, heat to reflux, and cool to obtain an intermediate;

[0059] S2. Add acetonitrile to the intermediate, add cerium ammonium nitrate solution after cooling, heat to react, separate to obtain a precipitate, and recrystallize the precipitate to obtain a bipolar organic material.

[0060] In some embodiments, tetrakis(triphenylphosphine)palladium can be replaced by palladium acetate.

[0061] In some embodiments, the temperature of heating to reflux is 70°C to 80°C.

[0062] Exemplarily, the temperature of heating to reflux is 70°C.

[0063] In some embodiments, the heating reflux time is 72 h to 96 h.

[0064] Exemplarily, the heating reflux time is 72 h.

[0065] In some embodiments, the molar ratio of 2,5-dibromofuran, 2,5-dimethoxyphenylboric acid, tetrakis(triphenylphosphine)palladium, and cesium carbonate is 1:2.1-2.4:0.03-0.05:3.3-3.5.

[0066] In some embodiments, the molar ratio of 2,5-dibromofuran, 2,5-dimethoxyphenylboronic acid, palladium acetate, and cesium carbonate is 1:2.1-2.4:0.03-0.05:3.3-3.5.

[0067] In some embodiments, the inert atmosphere is selected from an argon atmosphere.

[0068] In some embodiments, the temperature of the heating reaction is 30°C to 40°C.

[0069] Exemplarily, the temperature of the heating reaction is 35°C.

[0070] In some embodiments, the heating reaction time is 3 to 5 days.

[0071] Exemplarily, the heating reaction time is 3 days.

[0072] In some embodiments, the molar ratio of the intermediate to ammonium cerium nitrate is 1:6-8.

[0073] In some embodiments, in S1, after cooling to room temperature, it also includes: adding saturated brine to the cooled liquid, extracting with ethyl acetate or dichloromethane to obtain an organic phase, then drying the organic phase with anhydrous magnesium sulfate or anhydrous calcium sulfate, and separating and purifying the organic phase with a chromatographic column to obtain the intermediate.

[0074] Wherein, the chromatographic column is selected from a silica gel chromatographic column.

[0075] Exemplarily, S1 specifically includes: in a glove box, adding 2,5-dimethoxyphenylboronic acid and cesium carbonate to a Schlenk bottle, and then adding tetrakis(triphenylphosphine)palladium; in an argon atmosphere, adding 2,5-dibromofuran, tetrahydrofuran and water to the Schlenk bottle through a syringe, wherein tetrahydrofuran and water are used as solvents; then heating to 70°C, stirring and reflux for 72 hours; after the reaction is completed, after the Schlenk tube is cooled to room temperature, saturated brine is added, extracted three times with ethyl acetate, and the organic phase is dried with anhydrous magnesium sulfate, and then further separated and purified with a silica gel column to obtain a light green intermediate powder.

[0076] In some embodiments, S2 specifically includes: under inert atmosphere conditions, adding acetonitrile to the intermediate, mixing and cooling to 0°C, adding cerium ammonium nitrate solution, then heating to 35°C and stirring for reaction for 3 days, then adding water for ultrasonic treatment, separating and obtaining a precipitate; washing the precipitate with dichloromethane and water at a temperature of 35°C to 45°C, and drying to obtain a crude product; and recrystallizing the crude product with 1,1,2,2-tetrachloroethane to obtain the bipolar organic material.

[0077] Exemplarily, S2 specifically includes: under argon atmosphere, adding acetonitrile (MeCN) solution to a round-bottom flask, adding the intermediate obtained in S1, stirring to obtain a mixed solution, and cooling the mixed solution to 0°C; dissolving ammonium cerium nitrate in water to obtain an ammonium cerium nitrate solution, and adding it dropwise to the round-bottom flask within 20 minutes, then heating to 35°C and stirring for 3 days, during which the solution becomes darker and a yellow solid appears; after stopping the reaction, adding deionized water to the round-bottom flask and ultrasonically treating it for 30 minutes; separating by vacuum filtration to obtain a precipitate; washing the precipitate with dichloromethane and warm deionized water and drying it to obtain a crude product in the form of a yellow powder; adding the crude product to 1,1,2,2-tetrachloroethane for recrystallization to obtain the final product, i.e., a bipolar organic material.

[0078] In some embodiments, a use of a bipolar organic material as an electrode active material of a battery is also provided.

[0079] In some embodiments, the bipolar organic material is used as a positive active material in a battery.

[0080] Among them, the reaction equation of the energy storage mechanism of the bipolar organic material as the positive electrode active material is as follows:

[0081]

[0082] From the above reaction analysis, it can be seen that the carbonyl unit C=O functional group can reversibly deintercalate Na+, and the O atom near the furan unit can reversibly deintercalate A+. - (A - The reversible deintercalation of anions such as perchlorate, hexafluorophosphate or bis(trifluoromethanesulfonyl)imide is shown as follows: during discharge, the -1 The C=O characteristic peak disappears, and the double bond is reduced while storing a sodium ion to become CO-Na + During charging, CO weakens and the C=O peak reappears. At the same time, when charged to above 3.5V, a peak at 860cm -1 PF6 -The characteristic peak appears, but weakens in the subsequent discharge process. This is because the furan ring has electron-rich properties, storing an anion during charging and releasing it during discharge. This proves that the bipolar organic material of the present invention can simultaneously store sodium ions and anions to provide capacity during the cycle.

[0083] In some embodiments, a positive electrode plate is also provided, and the positive electrode active material in the positive electrode plate is selected from the bipolar organic material prepared by any of the above preparation methods.

[0084] In some embodiments, a sodium ion battery is provided that uses the positive electrode plate in any of the above embodiments as a positive electrode.

[0085] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the preparation method of the bipolar organic material and the sodium ion battery of the present invention will be further described in detail in combination with specific embodiments and drawings. Obviously, the specific embodiments described are only part of the embodiments of the present application, not all of them. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the present application and its application. Based on the specific embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of this application.

[0086] If no specific techniques or conditions are specified in the specific embodiments, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0087] Example 1

[0088] A method for preparing a bipolar organic material comprises the following steps:

[0089] S1. In a glove box, 1.72 g of 2,5-dimethoxyphenylboric acid, 0.28 g of tetrakis(triphenylphosphine)palladium, 4.89 g of cesium carbonate and 0.05 mL of 2,5-dibromofuran were added to a 200 mL dry Schlenk bottle in a molar ratio of 2.2:0.05:3.5. After mixing evenly, 70 mL of tetrahydrofuran and 9 mL of water were added to the Schlenk bottle by a syringe under argon (Ar) atmosphere, wherein water was used as a solvent; then the temperature was raised to 70° C., stirred and refluxed for 3 days, and after the reaction was completed, the Schlenk tube was cooled to room temperature, saturated brine was added, extracted three times with ethyl acetate, and the organic phase was dried with anhydrous magnesium sulfate, and then further separated and purified with a silica gel column to obtain a light green intermediate powder;

[0090] S2. Under argon atmosphere, 5 mL of acetonitrile (MeCN) solution was added to a round-bottom flask, and 0.20 g of the intermediate obtained in S1 was added and stirred to obtain a mixed solution, and the mixed solution was cooled to 0°C; 1.93 g of ammonium cerium nitrate was dissolved in 2 mL of water to obtain an ammonium cerium nitrate solution, and the solution was added dropwise to the round-bottom flask within 20 minutes, and then the temperature was raised to 35°C and stirred for 3 days. During this process, the solution became darker and a yellow solid appeared; after stopping the reaction, deionized water was added to the round-bottom flask and ultrasonically treated for 30 minutes; a precipitate was obtained by separation by vacuum filtration; the precipitate was washed with dichloromethane and warm deionized water and then dried to obtain a crude product in the form of a yellow powder; the crude product was added to 1,1,2,2-tetrachloroethane for recrystallization to obtain the final product 2,5-di-p-benzoquinonefuran (QFQ), i.e., a bipolar organic material.

[0091] Comparative Example 1

[0092] A method for preparing a bipolar organic material comprises the following steps:

[0093] S1. In a glove box, 1.72 g of 2,5-dimethoxyphenylboric acid, 0.3 g of palladium acetate, 4.89 g of cesium carbonate and 1,4-dibromobenzene were added to a 200 mL dry Schlenk bottle in a molar ratio of 2.4:0.05:3.5:1. After mixing evenly, 70 mL of tetrahydrofuran and 9 mL of water were added to the Schlenk bottle by a syringe under argon (Ar) atmosphere, wherein water was used as a solvent; then the temperature was raised to 70° C., stirred and refluxed for 5 days, and after the reaction was completed, the Schlenk tube was cooled to room temperature, saturated brine was added, extracted three times with dichloromethane, and the organic phase was dried with anhydrous magnesium sulfate, and then further separated and purified with a silica gel column to obtain a light green intermediate powder;

[0094] S2. Under argon atmosphere, 4 mL of acetonitrile (MeCN) solution was added to a round-bottom flask, and 0.20 g of the intermediate obtained in S1 was added and stirred to obtain a mixed solution, and the mixed solution was cooled to 0°C; 1.93 g of ammonium cerium nitrate was dissolved in 2.5 mL of water to obtain an ammonium cerium nitrate solution, and the solution was added dropwise to the round-bottom flask within 20 minutes, and then the temperature was raised to 35°C and stirred for 3 days. During this process, the solution became darker and a yellow solid appeared; after stopping the reaction, deionized water was added to the round-bottom flask and ultrasonically treated for 30 minutes; a precipitate was separated by vacuum filtration; the precipitate was washed with dichloromethane and warm deionized water and then dried to obtain a crude product in the form of a white powder; the crude product was added to 1,1,2,2-tetrachloroethane for recrystallization to obtain the final product 2,5-di-p-benzoquinonebenzene (BBQB), i.e., a bipolar organic material.

[0095] Example 2

[0096] A method for preparing a sodium ion battery comprises the following steps:

[0097] The 2,5-di-p-benzoquinone furan (QFQ) prepared in Example 1 was used as the positive electrode active material, and metallic sodium was used as the negative electrode;

[0098] Preparation of positive electrode sheet: 2,5-di-p-benzoquinone furan (QFQ), conductive carbon black and binder polyvinylidene fluoride (PVDF) in Example 1 were weighed in a mass ratio of 7:2:1, and then placed in a mortar, ground evenly, and then N-methylpyrrolidone was added to continue grinding to form a slurry, and the slurry was coated on a carbon-coated aluminum foil with a scraper, and dried overnight in a vacuum drying oven at a temperature of 60° C. to obtain a positive electrode sheet;

[0099] Preparation of button battery: In a glove box filled with argon, the positive electrode sheet, separator, 1 mol / L sodium hexafluorophosphate electrolyte (wherein the solvent is ethylene glycol dimethyl ether), sodium sheet, gasket, spring and negative electrode shell are placed on the positive electrode shell in sequence to assemble into a CR2032 button battery.

[0100] Comparative Example 2

[0101] A method for preparing a sodium ion battery comprises the following steps:

[0102] The 2,5-di-p-benzoquinonebenzene (BBQB) prepared in Comparative Example 1 was used as the positive electrode active material, and metallic sodium was used as the negative electrode;

[0103] Preparation of positive electrode sheet: 2,5-di-p-benzoquinonebenzene (BBQB), conductive carbon black and binder polyvinylidene fluoride (PVDF) in comparative example 1 were weighed in a mass ratio of 7:2:1, and then placed in a mortar, ground evenly, and then N-methylpyrrolidone was added to continue grinding to form a slurry, the slurry was coated on a carbon-coated aluminum foil by a scraper, and dried overnight in a vacuum drying oven at a temperature of 60°C to obtain a positive electrode sheet;

[0104] Preparation of button battery: In a glove box filled with argon, the positive electrode sheet, separator, 1 mol / L sodium hexafluorophosphate electrolyte (wherein the solvent is ethylene glycol dimethyl ether), sodium sheet, gasket, spring and negative electrode shell are placed on the positive electrode shell in sequence to assemble into a CR2032 button battery.

[0105] Detection and analysis

[0106] 1) H NMR spectroscopy characterization

[0107] The intermediate prepared in Example 1 was characterized by H NMR spectroscopy. Figure 1 shown.

[0108] from Figure 1It can be seen that the intermediate was successfully prepared in S1 of Example 1.

[0109] 2) Infrared spectroscopy analysis

[0110] The bipolar organic material 2,5-di-p-benzoquinonylfuran (QFQ) prepared in Example 1 was subjected to infrared spectroscopy analysis.

[0111] The results are as follows Figure 2 shown.

[0112] from Figure 2 The analysis shows that the -1 and 1025cm -1 The characteristic peak of COC is completely disappeared in 2,5-diphenylquinonylfuran (QFQ). -1 The carbonyl vibration peak appears at , indicating that the intermediate has been completely converted into the bipolar organic material 2,5-diphenylquinonylfuran (QFQ).

[0113] 3) Infrared spectroscopy analysis of sodium ion batteries

[0114] The sodium ion battery assembled with the bipolar organic material 2,5-diphenylquinonylfuran (QFQ) prepared in Example 2 was subjected to an ex situ infrared spectroscopy analysis. The results are as follows: Figure 3 shown.

[0115] from Figure 3 From the analysis, we can see that the 1620cm -1 The carbonyl vibration peak weakens during discharge and recovers during charge. Located at 840cm -1 PF6 - The characteristic peak appears during the charging process and weakens during the discharging process. This proves that the sodium ion battery assembled with the bipolar organic material 2,5-diphenylquinone furan (QFQ) of the present invention releases sodium ions and stores PF6 during charging. - PF6 is released during discharge - And store sodium ions, having bipolar characteristics, further proving that the bipolar organic material of the present invention has bipolar characteristics.

[0116] The sodium ion battery assembled with the bipolar organic material 2,5-di-p-benzoquinonebenzene (BBQB) prepared in Control Example 2 was subjected to an ex situ infrared spectroscopy analysis. The results are as follows: Figure 4 shown.

[0117] from Figure 4 From the analysis, we can see that the 1635cm -1 The carbonyl vibration peak weakens during discharge and recovers during charge. -1 No PF6 observed nearby -The change of vibration peaks indicates that the sodium-ion battery assembled by BBQB only stores sodium ions to provide capacity during the charge and discharge process.

[0118] 4) Cyclic voltammetry test

[0119] The sodium ion button cell prepared in Example 2 was tested by cyclic voltammetry (scan rate of 0.1 mv / s). The experimental results are as follows: Figure 5 shown.

[0120] from Figure 5 From the analysis, it can be seen that in the voltage window of 1.0-3.9V, there are two oxidation peaks (2.7V and 3.7V) and one reduction peak (1.85V), 2.7V and 3.7V represent the reversible storage of sodium ions and anions by the carbonyl group and the furan ring respectively, thus proving that the bipolar organic material of the present invention can be used as both n-type and p-type materials at the same time and has bipolar characteristics.

[0121] 5) Cycle performance test

[0122] The sodium ion button cells prepared in Example 2 and Comparative Example 2 were subjected to a cycle performance test at a current density of 100 mA / g. The experimental results are shown in FIG. Figure 6 shown.

[0123] from Figure 6 It can be seen from the analysis that at a current density of 100 mA / g, the initial discharge capacity of the sodium ion button cell prepared in Example 2 can reach 227 mAh / g, and the capacity retention rate is 97% after 300 cycles. This proves that the bipolar organic material of the present invention has a high discharge capacity and good cycle stability.

[0124] In summary, the bipolar organic material of the present invention, through the results of non-in-situ infrared spectroscopy test, shows that the chemical structure of the bipolar organic material contains both electrochemically active hydroxyl units and furan ring units, which reflects the bipolar characteristics. When used as an electrode material, it has excellent discharge capacity and cycle stability. The bipolar organic material is composed of C, H and O elements, has a wide source, is low in price, and is environmentally friendly. The bipolar organic material has a large molecular spacing and can adapt to various ions of different sizes (including Li + 、Na + Mg 2+and anion, etc.); the bipolar organic material has a fluffy structure, so when it is used as an electrode material, not only the structural change is small, but also it is conducive to the transmission of ions, and has the advantage of high structural stability. The bipolar organic material has a single molecule storage capacity and a high theoretical specific capacity. For example, the theoretical specific capacity of p-benzoquinone is as high as 496mAh / g. It solves the problem of poor structural stability of existing inorganic electrode materials, and also solves the problem of potential environmental and health risks and high cost of existing inorganic electrode materials.

[0125] The preparation method of the bipolar organic material of the present invention can successfully prepare the bipolar organic material by heating reflux and heating reaction with 2,5-dimethoxyphenylboric acid, cesium carbonate, tetrakis(triphenylphosphine)palladium, 2,5-dibromofuran, tetrahydrofuran and ammonium cerium nitrate, and has the advantages of low cost, simple operation, mild and easy-to-control process conditions, high efficiency and high purity, and is suitable for industrial large-scale production.

[0126] The chemical structure of the bipolar organic material prepared by the present invention contains both hydroxyl units and furan ring units. When the bipolar organic material is used as a positive electrode active material, the carbonyl unit can react with Na + For reversible storage, the furan ring unit can - The anions are reversibly stored, which effectively improves the battery's discharge capacity, rate performance and cycle stability, demonstrating excellent electrochemical properties. It has promotion and application value in the field of sodium ion battery technology.

[0127] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present application. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present application. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed in the present application shall still be covered by the claims of the present application.

Claims

1. A bipolar organic material, characterized in that: The structure of the bipolar organic material is shown in Formula I:

2. A method for preparing a bipolar organic material as claimed in claim 1, characterized in that: The following steps are involved: S1. Mix 2,5-dimethoxyphenylboronic acid, cesium carbonate and tetrakis(triphenylphosphine)palladium, place in an inert atmosphere, add 2,5-dibromofuran, tetrahydrofuran and water, heat to reflux, and cool to obtain an intermediate; S2. Add acetonitrile to the intermediate, add cerium ammonium nitrate solution after cooling, heat to react, separate to obtain a precipitate, and recrystallize the precipitate to obtain a bipolar organic material.

3. The method for preparing a bipolar organic material according to claim 2, characterized in that: The tetrakis(triphenylphosphine)palladium can be replaced by palladium acetate; And / or, the heating reflux temperature is 70°C to 80°C; And / or, the heating reflux time is 72h to 96h; and / or, the molar ratio of the 2,5-dibromofuran, 2,5-dimethoxyphenylboric acid, tetrakis(triphenylphosphine)palladium and cesium carbonate is 1:2.1-2.4:0.03-0.05:3.3-3.5; and / or, the molar ratio of the 2,5-dibromofuran, 2,5-dimethoxyphenylboric acid, palladium acetate and cesium carbonate is 1:2.1-2.4:0.03-0.05:3.3-3.5; And / or, the inert atmosphere is selected from argon atmosphere.

4. The method for preparing a bipolar organic material according to claim 2, characterized in that: The temperature of the heating reaction is 30°C to 40°C; And / or, the heating reaction time is 3 to 5 days; And / or, the molar ratio of the intermediate to ammonium cerium nitrate is 1:6-8.

5. The method for preparing a bipolar organic material according to claim 2, characterized in that: In the S1, after cooling to room temperature, it also includes: adding saturated brine to the cooled liquid, extracting with ethyl acetate or dichloromethane to obtain an organic phase, then drying the organic phase with anhydrous magnesium sulfate or anhydrous calcium sulfate, and separating and purifying the organic phase with a chromatographic column to obtain the intermediate.

6. The method for preparing a bipolar organic material according to claim 2, characterized in that: The S2 specifically includes: under inert atmosphere conditions, adding acetonitrile to the intermediate, mixing and cooling to 0°C, adding cerium ammonium nitrate solution, then heating to 35°C and stirring for reaction for 3 days, then adding water for ultrasonic treatment, separating and obtaining a precipitate; washing the precipitate with dichloromethane and water at a temperature of 35°C to 45°C in turn, and drying to obtain a crude product; and recrystallizing the crude product with 1,1,2,2-tetrachloroethane to obtain the bipolar organic material.

7. An application of a bipolar organic material obtained by the preparation method according to any one of claims 2 to 6, characterized in that: The bipolar organic material is used as an electrode active material of a battery.

8. The use according to claim 7, characterized in that: The bipolar organic material is used as a positive electrode active material of a battery.

9. A positive electrode sheet, characterized in that: The positive electrode active material in the positive electrode plate is selected from the bipolar organic material prepared by the preparation method according to any one of claims 2 to 6.

10. A sodium ion battery, characterized in that: The positive electrode sheet as claimed in claim 9 is used as the positive electrode of the sodium ion battery.

Citation Information

Patent Citations

  • Compound for positive electrode material of lithium ion battery, and preparation method and application

    CN111211327A

  • Organic electrode material and preparation method and application thereof

    CN112279806A

  • Bipolar organic material, preparation method thereof and application of bipolar organic material in sodium-ion battery

    CN116589416A

  • Power storage material, electrode for power storage device, and power storage device

    JP2016091751A

  • Power storage material, electrode for power storage device, and power storage device

    JP2016115454A