Polyethylene modified foamed cotton as well as preparation method and application thereof

By using sol-gel reaction in polyethylene modified foam to prepare Al2O3/TiO2 composite microspheres and coat wrinkled graphene oxide and carbon fibers, the radiation crosslinked polyethylene foam cannot achieve electromagnetic shielding and The problem of wave absorption improves the mechanical and electromagnetic shielding performance of the material, simplifies the process and reduces environmental pollution and production costs.

CN119081210APending Publication Date: 2024-12-06ZHIHUIMAO (DONGYING) INTELLIGENT TECH CO LTD

Patent Information

Application Number
CN202411431217.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing radiation crosslinked polyethylene foam products cannot achieve electromagnetic shielding and wave absorption functions. At the same time, the process is complex, the environmental pollution is large, the production efficiency is low, and the cost is high. The electromagnetic shielding and wave absorption performance need to be improved.

Method used

Al2O3/TiO2 composite microspheres were prepared by sol-gel reaction, and wrinkled graphene oxide and carbon fiber were coated on their surface. Modified using a silane coupling agent, and added low-density polyethylene and foaming agent for cross-linking. The preparation was performed. Polyethylene modified foam with good mechanical properties and electromagnetic shielding properties.

Benefits of technology

The preparation of polyethylene modified foam has been realized, with good mechanical properties, heat resistance, antibacterial and flame retardant properties, excellent electromagnetic shielding performance, suitable for electronic products, simplified process flow, reduced environmental pollution and production costs .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides polyethylene modified foamed cotton as well as a preparation method and application thereof, and belongs to the technical field of polyethylene. The preparation method comprises the following steps: preparing Al2O3 / TiO2 composite microspheres through a sol-gel reaction, coating the surfaces of the Al2O3 / TiO2 composite microspheres with wrinkled graphene oxide, carrying out coupling and reduction with p-phenylenediamine and carbon fibers, carrying out modification through a silane coupling agent, adding low-density polyethylene, an ethylene-vinyl acetate copolymer, a sensitizer, polyethylene wax and the modified microspheres, carrying out open milling, adding a foaming agent and a cross-linking agent, carrying out heating cross-linking, carrying out foaming, and carrying out cooling. The polyethylene modified foamed cotton is prepared. The polyethylene modified foamed cotton prepared by the invention is simple in method, wide in raw material source, relatively good in mechanical property, good in rebound resilience, heat-resistant, antibacterial and flame-retardant properties and good in electromagnetic shielding property, can be widely applied to electronic products, and is high in reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyethylene, and in particular to a polyethylene modified foam cotton and a preparation method and application thereof. Background Art

[0002] Cross-linked polyethylene foam material is a new type of foamed plastic with a closed-cell structure between soft (polyurethane) and hard (polystyrene) foam materials. It has a series of characteristics such as superior toughness, elasticity, flexibility, wear resistance, chemical corrosion resistance, low temperature resistance and good insulation. It can be used as a good insulation, heat insulation, shockproof and buoyancy material. High-strength polyethylene foam products are widely used in mechanical shock absorption, floor mats, automotive interiors, electronic equipment and other fields. With the upgrading of products, higher requirements are put forward for product strength.

[0003] Radiation cross-linked polyethylene foam (IXPE) material is a high-molecular foam material made of low-density polyethylene (LDPE) as the main raw material, azodicarbonamide (AC) and other chemical raw materials as the foaming agent, through mixing and granulation, extrusion processing, radiation cross-linking, and foaming molding. It has a smooth surface, closed, fine and uniform pores, does not absorb water, is environmentally friendly, light in weight, and has low cost. It also has excellent sealing and cushioning properties, high shape recovery ability, and high cushioning and shock absorption ability. However, existing radiation cross-linked polyethylene foam products cannot eliminate electromagnetic waves, and the existing radiation cross-linked polyethylene foam is a closed-cell material and does not have the function of absorbing waves.

[0004] With the development of science and technology, its uses have also diversified, and it is necessary to innovate and improve the development of radiation cross-linked polyethylene foam products, which are not only light in weight, low in cost, and have high cushioning and shock absorbing capabilities, but also have good electromagnetic shielding properties and wave absorbing functions.

[0005] In order to solve the above problems, CN107540959A discloses a multifunctional foam sheet and a preparation method thereof, which comprises the following steps: S1: granulating the raw materials to obtain formulated particles, S2: extruding the formulated particles into sheets, and at the same time, performing certain longitudinal stretching and transverse stretching, the longitudinal stretching ratio is 1.0-4.0, and the transverse stretching ratio is 1.0-3.0, S3: adopting electron beam radiation crosslinking, and the electron energy of radiation crosslinking is 0.5MeV-2.5MeV, S4: performing free-style foaming, and the foaming temperature is 160℃-400℃, S5: adopting continuous precision cutting to cut the thickness of the substrate into a size smaller than its average pore size, the thickness of the foam sheet is less than 0.3mm, and it is in the shape of a honeycomb plate in the thickness direction, and its structure has through holes along the thickness direction, and its through-porosity is 20%-60%, S6: adopting one or more of chemical plating, magnetron sputtering or electroplating to attach the coating material to the surface of the foam sheet to form a multifunctional coating. Its thickness is less than 0.3 mm, its weight is light, its sealing and cushioning performance is excellent, it has high shape recovery ability, high cushioning and shock absorption ability, it can conduct heat and electricity, and it has good electromagnetic shielding effect. It can meet the increasingly high requirements of electronic products for auxiliary materials. However, the above technology has at least the following technical problems: (1) It has relatively large environmental pollution, complex process, low production efficiency, high process cost, and high foaming density of the foam; (2) The electromagnetic shielding performance and wave absorbing performance of the foam need to be improved. Summary of the invention

[0006] The purpose of the present invention is to provide a polyethylene modified foam cotton and a preparation method and application thereof. The preparation method is simple, the raw material source is wide, the foam cotton has good mechanical properties, good resilience, good heat resistance, antibacterial and flame retardant properties, good electromagnetic shielding performance, can be widely used in electronic products, and has high reliability.

[0007] The technical scheme of the present invention is achieved as follows: the present invention provides a preparation method of polyethylene modified foam cotton, wherein Al2O3 / TiO2 composite microspheres are prepared by sol-gel reaction, the surface of which is coated with wrinkled graphene oxide and coupled with p-phenylenediamine and carbon fiber, reduced, modified by a silane coupling agent, low-density polyethylene, ethylene-vinyl acetate copolymer, sensitizer, polyethylene wax and modified microspheres are added for refining, and then a foaming agent and a cross-linking agent are added, heated for cross-linking, foamed, and cooled to obtain polyethylene modified foam cotton.

[0008] As a further improvement of the present invention, the following steps are included: S1. Preparation of Al2O3 / TiO2 composite microspheres: dissolving aluminum isopropoxide and tetrabutyl titanate in ethyl acetate, dropping into ammonia water, adding an emulsifier for emulsification, centrifuging, washing, drying, and calcining to obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: adding graphene oxide to water, adding Al2O3 / TiO2 composite microspheres, p-phenylenediamine and ammonia water, stirring and mixing to react, spray drying, and obtaining p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite coated microspheres: adding carbon fiber to nitric acid, stirring, centrifuging, washing, drying, adding the product to water, adding p-phenylenediamine modified wrinkled graphene oxide coated microspheres and sodium nitrite, dropping hydrochloric acid, heating and refluxing, centrifuging, washing, drying, and obtaining wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites; S4. Preparation of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres: reducing the wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite with hydrazine hydrate vapor to obtain wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres; S5. Modification: adding wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres to ethanol, adding silane coupling agent, heating and stirring, centrifuging, washing, drying, and obtaining modified microspheres; S6. Preparation of polyethylene modified foam cotton: melt low-density polyethylene, add ethylene-vinyl acetate copolymer, stir and mix evenly, add sensitizer, polyethylene wax and modified microspheres, and then add foaming agent and cross-linking agent, heat and cross-link, foam, and cool to obtain polyethylene modified foam cotton.

[0009] As a further improvement of the present invention, the mass ratio of aluminum isopropoxide, tetrabutyl titanate and emulsifier in step S1 is 12-15:7-10:0.5-1, the concentration of ammonia water is 10-15wt%, the calcination temperature is 400-600°C, the time is 1-3h, and the emulsifier is selected from at least one of Tween-20, Tween-40, Tween-60, Tween-80 and Tween-85.

[0010] As a further improvement of the present invention, the mass ratio of graphene oxide, Al2O3 / TiO2 composite microspheres, p-phenylenediamine and ammonia water in step S2 is 3-5:10:4-6:7-10, the temperature of the stirring and mixing reaction is 90-100°C, and the time is 6-8h.

[0011] As a further improvement of the present invention, the mass ratio of the carbon fiber, p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres, sodium nitrite, and hydrochloric acid in step S3 is 2-3:10:0.5-1:2-4, the concentration of the hydrochloric acid is 1-3 mol / L, the concentration of the nitric acid is 20-30wt%, and the heating reflux reaction time is 2-3h.

[0012] As a further improvement of the present invention, the reduction time in step S4 is 7-10 hours.

[0013] As a further improvement of the present invention, the mass ratio of the wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres and the silane coupling agent in step S5 is 10:2-3, the silane coupling agent is at least one of KH570, A151, and A171, and the heating and stirring reaction time is 35-45°C for 1-2h.

[0014] As a further improvement of the present invention, the mass ratio of the low-density polyethylene, ethylene-vinyl acetate copolymer, sensitizer, polyethylene wax, modified microspheres, foaming agent and cross-linking agent in step S6 is 90-100:8-10:1-2:1-2:10-12:3-4:0.5-1, the heating cross-linking temperature is 130-140°C, the time is 1-3h, the foaming condition is 180-190°C for 7-10min, the foaming agent is 4,4-oxybisbenzenesulfonylhydrazide, and the cross-linking agent is diisopropylbenzene peroxide.

[0015] The present invention further protects a polyethylene modified foamed cotton prepared by the above preparation method.

[0016] The present invention further protects an application of the polyethylene modified foam cotton in the field of electronic product materials.

[0017] The present invention has the following beneficial effects: the present invention prepares a composite nano-microsphere of aluminum oxide and titanium oxide through a sol-gel reaction, and adds the composite nano-microsphere to polyethylene modified foam cotton, which greatly improves the heat resistance, flame retardancy, electromagnetic shielding and antibacterial properties of the foam cotton, and as an electronic product material, greatly improves the reliability of the product. However, when the composite nano-microsphere is directly added to polyethylene modified foam cotton, the surface effect of the nano-microsphere often causes the nano-microsphere to easily agglomerate, and the distribution in the substrate is uneven, which greatly affects the mechanical properties of the material, limits the application area, and the electromagnetic shielding performance of the oxide material is limited.

[0018] Therefore, the present invention coats a layer of wrinkled graphene oxide on the surface of the prepared Al2O3 / TiO2 composite microspheres by spray drying, and the wrinkled structure destroys the ordered structure of graphene, greatly improving its dispersibility and compatibility in the substrate and improving the mechanical properties. However, its electromagnetic shielding performance is still not good due to the influence of the oxidation structure.

[0019] Therefore, the inventors connected graphene oxide and carbon fiber to form a composite through the connecting effect of p-phenylenediamine. The grafted structure is conducive to the dispersion of carbon fiber and graphene, and the support effect also prevents the restacking of graphene oxide sheets, increases conductivity, and improves electromagnetic shielding performance. Subsequently, under the reduction effect of hydrazine hydrate vapor, wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres with better conductivity are prepared. However, after the microspheres are added to the substrate, they still have a small negative impact on the mechanical properties of the material.

[0020] Therefore, the inventors modified the wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres and modified the microspheres with a silane coupling agent with double bonds, so that the microspheres have double bonds. Under the action of the subsequent cross-linking agent, the double bonds can copolymerize with polyethylene, and the cross-linking agent can also polymerize p-phenylenediamine to form poly-p-phenylenediamine, so that the prepared polyethylene modified foam cotton forms a complex cross-linked network structure with dense and uniform pores, and therefore its mechanical properties are significantly improved.

[0021] The polyethylene modified foamed cotton prepared by the invention has a simple preparation method, a wide source of raw materials, good mechanical properties, good resilience, good heat resistance, antibacterial and flame retardant properties, good electromagnetic shielding performance, can be widely used in electronic products, and has high reliability. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Low density polyethylene, 2426H, Shenhua Yulin Energy Chemical Co., Ltd.

[0024] Example 1: This example provides a method for preparing polyethylene modified foamed cotton, comprising the following steps: S1. Preparation of Al2O3 / TiO2 composite microspheres: 12g aluminum isopropoxide and 7g tetrabutyl titanate are dissolved in 500mL ethyl acetate, dropped into 1L 10wt% ammonia water, 0.5g Tween-20 is added, emulsified at 7000r / min for 10min, centrifuged, washed, dried, and calcined at 400℃ for 1h to obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: 3g graphene oxide is added to 500mL water, 10g Al2O3 / TiO2 composite microspheres, 4g p-phenylenediamine and 7g ammonia water are added, stirred and mixed at 90℃ for 6h, and spray dried to obtain p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite coated microspheres: add 2g carbon fiber into 50mL 20wt% nitric acid, stir for 0.5h, centrifuge, wash, dry, add the product into 200mL water, add 10g p-phenylenediamine modified wrinkled graphene oxide coated microspheres and 0.5g sodium nitrite, add 2g 1mol / L hydrochloric acid dropwise, heat and reflux for 2h, centrifuge, wash, dry, and obtain wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite; S4. Preparation of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres: reduce the wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite with hydrazine hydrate vapor for 7h to obtain wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres; S5. Modification: Add 10g of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres to ethanol, add 2g of silane coupling agent KH570, heat to 35°C, stir to react for 1h, centrifuge, wash, and dry to obtain modified microspheres; S6. Preparation of polyethylene modified foam cotton: melt 90g of low-density polyethylene, add 8g of ethylene-vinyl acetate copolymer, stir and mix for 20min, add 1g of zinc stearate, 1g of polyethylene wax and 10g of modified microspheres, pressurize to 12MPa on a flat vulcanizer at 110°C for 4min, then add 3g of 4,4-oxybisbenzenesulfonylhydrazine and 0.5g of diisopropylbenzene peroxide, heat to 130°C, crosslink for 1h, foam at 180°C for 7min, cool, and obtain polyethylene modified foam cotton.

[0025] Example 2: This example provides a method for preparing polyethylene modified foamed cotton, comprising the following steps: S1. Preparation of Al2O3 / TiO2 composite microspheres: 15g of aluminum isopropoxide and 10g of tetrabutyl titanate were dissolved in 500mL of ethyl acetate, and then dropped into 1L of 15wt% ammonia water, 1g of Tween-40 was added, and the mixture was emulsified at 7000r / min for 10min, centrifuged, washed, dried, and calcined at 600℃ for 3h to obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: 5g of graphene oxide was added to 500mL of water, and then 10g of Al2O3 / TiO2 composite microspheres, 6g of p-phenylenediamine and 10g of ammonia water were added, and the mixture was stirred and mixed at 100℃ for 8h, and then spray-dried to obtain p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite coated microspheres: 3g carbon fiber was added to 50mL 30wt% nitric acid, stirred for 1h, centrifuged, washed, dried, the product was added to 200mL water, 10g p-phenylenediamine modified wrinkled graphene oxide coated microspheres and 1g sodium nitrite were added, 4g 3mol / L hydrochloric acid was added dropwise, heated to reflux reaction for 3h, centrifuged, washed, dried, and wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites were obtained; S4. Preparation of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres: wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites were reduced with hydrazine hydrate vapor for 10h to obtain wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres; S5. Modification: Add 10g of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres to ethanol, add 3g of silane coupling agent A151, heat to 45°C, stir to react for 2h, centrifuge, wash, and dry to obtain modified microspheres; S6. Preparation of polyethylene modified foam cotton: melt 100g of low-density polyethylene, add 10g of ethylene-vinyl acetate copolymer, stir and mix for 20min, add 2g of zinc stearate, 2g of polyethylene wax and 12g of modified microspheres, pressurize to 14MPa on a 120°C flat vulcanizer for melting treatment for 6min, then add 4g of 4,4-oxybisbenzenesulfonylhydrazine and 1g of diisopropylbenzene peroxide, heat to 140°C, crosslink for 2h, foam at 190°C for 10min, cool, and obtain polyethylene modified foam cotton.

[0026] Example 3: This example provides a method for preparing polyethylene modified foamed cotton, comprising the following steps: S1. Preparation of Al2O3 / TiO2 composite microspheres: 13g of aluminum isopropoxide and 8g of tetrabutyl titanate were dissolved in 500mL of ethyl acetate, and then dropped into 1L of 12wt% ammonia water, and 0.7g of Tween-85 was added, and emulsified at 7000r / min for 10min, centrifuged, washed, dried, and calcined at 500℃ for 2h to obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: 4g of graphene oxide was added to 500mL of water, and then 10g of Al2O3 / TiO2 composite microspheres, 5g of p-phenylenediamine and 8g of ammonia water were added, and the mixture was stirred and reacted at 95℃ for 7h, and then spray-dried to obtain p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite coated microspheres: 2.5g carbon fiber was added to 50mL 25wt% nitric acid, stirred for 1h, centrifuged, washed, dried, the product was added to 200mL water, 10g p-phenylenediamine modified wrinkled graphene oxide coated microspheres and 0.7g sodium nitrite were added, 3g 2mol / L hydrochloric acid was added dropwise, heated to reflux reaction for 2.5h, centrifuged, washed, dried, and wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites were obtained; S4. Preparation of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres: wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites were reduced with hydrazine hydrate vapor for 8h to obtain wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres; S5. Modification: Add 10g of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres to ethanol, add 2.5g of silane coupling agent KH570, heat to 40℃, stir to react for 1.5h, centrifuge, wash, and dry to obtain modified microspheres; S6. Preparation of polyethylene modified foam cotton: Melt 95g of low-density polyethylene, add 9g of ethylene-vinyl acetate copolymer, stir and mix for 20min, add 1.5g of zinc stearate, 1.5g of polyethylene wax and 11g of modified microspheres, pressurize to 13MPa on a flat vulcanizer at 115℃ for melting for 5min, then add 3.5g of 4,4-oxybisbenzenesulfonylhydrazine and 0.7g of diisopropyl peroxide, heat to 135℃, crosslink for 1.5h, foam at 185℃ for 8min, cool, and obtain polyethylene modified foam cotton.

[0027] Comparative Example 1 Compared with Example 3, the difference is that aluminum isopropoxide is not added in step S1.

[0028] The details are as follows: S1. Preparation of TiO2 composite microspheres: 21g of tetrabutyl titanate was dissolved in 500mL of ethyl acetate, dropped into 1L of 12wt% ammonia water, added with 0.7g of Tween-85, emulsified at 7000r / min for 10min, centrifuged, washed, dried, and calcined at 500℃ for 2h to obtain TiO2 microspheres.

[0029] Comparative Example 2 Compared with Example 3, the difference is that the spray drying in step S2 is replaced by room temperature drying.

[0030] The details are as follows: S2. Preparation of p-phenylenediamine-modified wrinkled graphene oxide coated microspheres: Add 4 g of graphene oxide into 500 mL of water, add 10 g of Al2O3 / TiO2 composite microspheres, 5 g of p-phenylenediamine and 8 g of ammonia water, stir and react at 95°C for 7 hours, and dry at room temperature to obtain p-phenylenediamine-modified wrinkled graphene oxide coated microspheres.

[0031] Comparative Example 3 Compared with Example 3, the difference is that step S3 is not performed.

[0032] The details are as follows: S1. Preparation of Al2O3 / TiO2 composite microspheres: 13g aluminum isopropoxide and 8g tetrabutyl titanate were dissolved in 500mL ethyl acetate, dropped into 1L 12wt% ammonia water, added 0.7g Tween-85, emulsified at 7000r / min for 10min, centrifuged, washed, dried, and calcined at 500℃ for 2h to obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: 4g graphene oxide was added to 500mL water, 10g Al2O3 / TiO2 composite microspheres, 5g p-phenylenediamine and 8g ammonia water were added, stirred and reacted at 95℃ for 7h, and spray dried to obtain p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene-coated microspheres: The p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres were subjected to hydrazine hydrate vapor reduction for 8 hours to obtain wrinkled graphene-coated microspheres; S4. Modification: 10g of wrinkled graphene-coated microspheres were added to ethanol, 2.5g of silane coupling agent KH570 was added, heated to 40°C, stirred for reaction for 1.5h, centrifuged, washed, and dried to obtain modified microspheres; S5. Preparation of polyethylene-modified foamed cotton: 95g of low-density polyethylene was melted, 9g of ethylene-vinyl acetate copolymer was added, stirred and mixed for 20min, 1.5g of zinc stearate, 1.5g of polyethylene wax and 11g of modified microspheres were added, and melted on a flat vulcanizer at 115°C under pressure to 13MPa for 5min, and then 3.5g of 4,4-Oxybisbenzenesulfonyl hydrazide and 0.7g diisopropylbenzene peroxide were heated to 135°C, cross-linked for 1.5h, foamed at 185°C for 8min, and cooled to obtain polyethylene modified foam.

[0033] Comparative Example 4 Compared with Example 3, the difference is that step S4 is not performed.

[0034] The details are as follows: S1. Preparation of Al2O3 / TiO2 composite microspheres: 13g aluminum isopropoxide and 8g tetrabutyl titanate were dissolved in 500mL ethyl acetate, dropped into 1L 12wt% ammonia water, added 0.7g Tween-85, emulsified at 7000r / min for 10min, centrifuged, washed, dried, and calcined at 500℃ for 2h to obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: 4g graphene oxide was added to 500mL water, 10g Al2O3 / TiO2 composite microspheres, 5g p-phenylenediamine and 8g ammonia water were added, stirred and reacted at 95℃ for 7h, and spray dried to obtain p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite coated microspheres: 2.5g carbon fiber was added to 50mL 25wt% nitric acid, stirred for 1h, centrifuged, washed, dried, the product was added to 200mL water, 10g p-phenylenediamine modified wrinkled graphene oxide coated microspheres and 0.7g sodium nitrite were added, 3g 2mol / L hydrochloric acid was added dropwise, heated to reflux for 2.5h, centrifuged, washed, dried, and wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites were obtained; S4. Modification: 10g wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite was added to ethanol, 2.5g silane coupling agent KH570 was added, heated to 40℃, stirred for 1.5h, centrifuged, washed, dried, and modified microspheres were obtained; S5. Preparation of polyethylene modified foam cotton: melt 95g low-density polyethylene, add 9g ethylene-vinyl acetate copolymer, stir and mix for 20min, add 1.5g zinc stearate, 1.5g polyethylene wax and 11g modified microspheres, pressurize to 13MPa on a 115℃ flat vulcanizer for melting for 5min, then add 3.5g 4,4-oxybisbenzenesulfonyl hydrazide and 0.7g diisopropyl peroxide, heat to 135℃, crosslink for 1.5h, foam at 185℃ for 8min, cool, and obtain polyethylene modified foam cotton.

[0035] Comparative Example 5 Compared with Embodiment 3, the difference is that step S5 is not performed.

[0036] The details are as follows: S1. Preparation of Al2O3 / TiO2 composite microspheres: 13g aluminum isopropoxide and 8g tetrabutyl titanate were dissolved in 500mL ethyl acetate, dropped into 1L 12wt% ammonia water, added 0.7g Tween-85, emulsified at 7000r / min for 10min, centrifuged, washed, dried, and calcined at 500℃ for 2h to obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: 4g graphene oxide was added to 500mL water, 10g Al2O3 / TiO2 composite microspheres, 5g p-phenylenediamine and 8g ammonia water were added, stirred and reacted at 95℃ for 7h, and spray dried to obtain p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite coated microspheres: 2.5g carbon fiber was added to 50mL 25wt% nitric acid, stirred for 1h, centrifuged, washed, dried, the product was added to 200mL water, 10g p-phenylenediamine modified wrinkled graphene oxide coated microspheres and 0.7g sodium nitrite were added, 3g 2mol / L hydrochloric acid was added dropwise, heated to reflux reaction for 2.5h, centrifuged, washed, dried, and wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites were obtained; S4. Preparation of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres: wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites were reduced with hydrazine hydrate vapor for 8h to obtain wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres; S5. Preparation of polyethylene modified foam cotton: 95g low-density polyethylene was melted in an open mill, 9g ethylene-vinyl acetate copolymer was added, and the mixture was stirred for 20min. 1.5g zinc stearate, 1.5g polyethylene wax and 11g wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres were added, and the mixture was melted on a flat vulcanizer at 115°C under pressure to 13MPa for 5min. Then 3.5g 4,4-oxybisbenzenesulfonylhydrazine and 0.7g diisopropyl peroxide were added, and the mixture was heated to 135°C, cross-linked for 1.5h, foamed at 185°C for 8min, and cooled to obtain polyethylene modified foam cotton.

[0037] Test Example 1 The polyethylene modified foamed cottons prepared in Examples 1-3 of the present invention and Comparative Examples 1-5 were subjected to performance tests.

[0038] Mechanical properties: Tested in accordance with GB / T 6669-2008 "Determination of permanent compression set of flexible foam", GB / T 10807-2006 "Determination of hardness of flexible polymeric foam materials (indentation method)" and GB / T 6344-2008 "Determination of tensile strength and elongation at break of flexible foam".

[0039] Limiting oxygen index (LOI): Tested in accordance with GB / T2406.2-2009 "Determination of combustion behavior of plastics by oxygen index method Part 2: Room temperature test".

[0040] Electromagnetic shielding performance: tested in accordance with GB / T32596-2016 "General Specification for Electromagnetic Shielding Absorbers".

[0041] The results are shown in Table 1.

[0042]

[0043] It can be seen from the above table that the polyethylene modified foamed cotton prepared in Examples 1-3 of the present invention has good mechanical properties, flame retardant properties and electromagnetic shielding properties.

[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing polyethylene modified foamed cotton, characterized in that: Al2O3 / TiO2 composite microspheres are prepared by sol-gel reaction, and the surface is coated with wrinkled graphene oxide and coupled with p-phenylenediamine and carbon fiber, reduced, modified by silane coupling agent, low-density polyethylene, ethylene-vinyl acetate copolymer, sensitizer, polyethylene wax and modified microspheres are added for refining, and then foaming agent and cross-linking agent are added, heated for cross-linking, foaming, and cooling to obtain polyethylene modified foam cotton.

2. The preparation method according to claim 1, characterized in that The following steps are involved: S1. Preparation of Al2O3 / TiO2 composite microspheres: dissolve aluminum isopropoxide and tetrabutyl titanate in ethyl acetate, drop into ammonia water, add emulsifier for emulsification, centrifuge, wash, dry, calcine, and obtain Al2O3 / TiO2 composite microspheres; S2. Preparation of p-phenylenediamine-modified p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres: add graphene oxide to water, add Al2O3 / TiO2 composite microspheres, p-phenylenediamine and ammonia water, stir and mix to react, spray dry, and obtain p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres; S3. Preparation of wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite coated microspheres: adding carbon fiber to nitric acid, stirring, centrifuging, washing, drying, adding the product to water, adding p-phenylenediamine modified wrinkled graphene oxide coated microspheres and sodium nitrite, adding hydrochloric acid dropwise, heating under reflux reaction, centrifuging, washing, drying, and obtaining wrinkled graphene oxide-p-phenylenediamine-carbon fiber composites; S4. Preparation of wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres: reducing the wrinkled graphene oxide-p-phenylenediamine-carbon fiber composite with hydrazine hydrate vapor to obtain wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres; S5. Modification: Add wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres into ethanol, add silane coupling agent, heat and stir to react, centrifuge, wash, and dry to obtain modified microspheres; S6. Preparation of polyethylene modified foam cotton: melt low-density polyethylene, add ethylene-vinyl acetate copolymer, stir and mix evenly, add sensitizer, polyethylene wax and modified microspheres, and then add foaming agent and cross-linking agent, heat and cross-link, foam, and cool to obtain polyethylene modified foam cotton.

3. The preparation method according to claim 2, characterized in that: In step S1, the mass ratio of aluminum isopropoxide, tetrabutyl titanate and emulsifier is 12-15:7-10:0.5-1, the concentration of ammonia water is 10-15wt%, the calcination temperature is 400-600°C, the time is 1-3h, and the emulsifier is selected from at least one of Tween-20, Tween-40, Tween-60, Tween-80 and Tween-85.

4. The preparation method according to claim 2, characterized in that: In step S2, the mass ratio of graphene oxide, Al2O3 / TiO2 composite microspheres, p-phenylenediamine and ammonia water is 3-5:10:4-6:7-10, and the stirring and mixing reaction is carried out at a temperature of 90-100°C and for a time of 6-8h.

5. The preparation method according to claim 2, characterized in that: In step S3, the mass ratio of the carbon fiber, p-phenylenediamine-modified wrinkled graphene oxide-coated microspheres, sodium nitrite, and hydrochloric acid is 2-3:10:0.5-1:2-4, the concentration of the hydrochloric acid is 1-3 mol / L, the concentration of the nitric acid is 20-30wt%, and the heating reflux reaction time is 2-3h.

6. The preparation method according to claim 2, characterized in that: The reduction time in step S4 is 7-10 hours.

7. The preparation method according to claim 2, characterized in that: In step S5, the mass ratio of the wrinkled graphene-p-phenylenediamine-carbon fiber coated microspheres and the silane coupling agent is 10:2-3, the silane coupling agent is at least one of KH570, A151, and A171, and the heating and stirring reaction time is 35-45° C. for 1-2 hours.

8. The preparation method according to claim 2, characterized in that: The mass ratio of low-density polyethylene, ethylene-vinyl acetate copolymer, sensitizer, polyethylene wax, modified microspheres, foaming agent and cross-linking agent in step S6 is 90-100:8-10:1-2:1-2:10-12:3-4:0.5-1, the heating cross-linking temperature is 130-140°C, the time is 1-3h, the foaming condition is 180-190°C for 7-10min, the foaming agent is 4,4-oxybisbenzenesulfonylhydrazide, and the cross-linking agent is diisopropylbenzene peroxide.

9. A polyethylene modified foam obtained by the preparation method according to any one of claims 1 to 8.

10. Use of the polyethylene modified foam as claimed in claim 9 in the field of electronic product materials.

Citation Information

Patent Citations

  • Multifunctional foam sheet and preparation method thereof

    CN107540959A

Cited By

  • Composite filler containing silicon oxide micropowder and preparation method thereof

    CN120988366A

  • Composite filler containing silicon oxide fine powder and method for producing the same

    CN120988366B