Organic phosphorus flame retardant as well as preparation method and application thereof
By preparing a high-phosphorus aryl phosphate flame retardant (oxo-5-phosphoric trimethyl)tri(methylene)tri(diphenyl phosphine), the problems of low thermal stability and flame retardant efficiency of traditional organophosphorus flame retardants in polyester polymer materials were solved, achieving a balance between excellent flame retardant performance and mechanical properties.
Patent Information
- Application Number
- CN202411021438.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional organophosphorus flame retardants have poor thermal stability and low flame retardant efficiency in polyester polymers, which leads to easy decomposition and volatilization during processing, reducing mechanical properties.
(Oxo-5-phosphoric trimethyl)tri(methylene)tri(diphenyl phosphine) was used as an organophosphorus flame retardant. PO and PC groups were introduced through nucleophilic substitution reactions to prepare aryl phosphate flame retardants with high phosphorus content, thereby improving their compatibility and thermal stability with polyester polymers.
It achieves high-efficiency flame retardant properties while maintaining the mechanical and processing properties of the material, thus expanding the application scope of polyester polymer materials in emerging fields.
Smart Images

Figure CN118955558A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of phosphorus flame retardants, and in particular to an organic phosphorus flame retardant and a preparation method and application thereof. Background Art
[0002] There are many types of polyester polymer materials, and they have excellent comprehensive properties. They are widely used in electronic appliances, construction materials, automobile manufacturing and other fields. However, polyester polymer materials are generally flammable, and they produce a large amount of flammable droplets and toxic gases during the combustion process, which poses a great threat to human production and life safety. Therefore, in most of the applications of polyester polymer materials, they must be flame-retardant modified.
[0003] Compared with the inorganic flame retardants, nitrogen flame retardants and silicon flame retardants traditionally used for polyester polymers, organophosphorus flame retardants can decompose and produce phosphorus-containing free radicals in the gas phase, and can capture H·, O· and OH· produced by the cracking of polyester polymer materials in the gas phase, thereby effectively playing a gas phase capture role in the gas phase. In addition, organophosphorus flame retardants can produce phosphoric acid, metaphosphoric acid and polyphosphoric acid in the condensed phase, which promotes the degradation and carbonization of polyester polymer materials in advance, forming a protective carbon layer, and playing a shielding role in the condensed phase. Therefore, organophosphorus flame retardants have been widely used in polyester materials. However, traditional organophosphorus flame retardants in polyester materials often have poor thermal stability and low flame retardant efficiency, and are easy to decompose and volatilize during material processing, which significantly reduces the mechanical properties of polyester materials and limits their wide application in polyester materials. With the continuous development of miniaturization and miniaturization of electronic appliances, higher requirements are placed on the comprehensive properties of polyester materials such as flame retardancy and mechanics. Therefore, it is imperative to develop high-performance flame-retardant polyester polymer materials. Summary of the invention
[0004] The present invention aims to solve the problems of poor thermal stability and low flame retardant efficiency of existing organophosphorus flame retardants, and provides an organophosphorus flame retardant and a preparation method and application thereof.
[0005] The organic phosphorus flame retardant of the present invention is (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphinate), and its chemical structure is as follows:
[0006]
[0007] The preparation method of the above-mentioned organophosphorus flame retardant comprises the following steps:
[0008] 1. Add trimethylolphosphine oxide and dioxane to a reaction device to obtain a mixed solution, heat the mixed solution to 70-80° C., and stir until dissolved;
[0009] 2. Then, diphenylphosphinoyl chloride is placed in a constant pressure dropping funnel and added dropwise to the reaction device, the dropping speed is controlled, and the reaction temperature is maintained at 70-80°C during the dropping process;
[0010] 3. After the dropwise addition is completed, the reaction temperature is raised to the reflux temperature, and the reaction is continued under reflux for 3 to 6 hours. After the reaction is completed, it is cooled to room temperature and allowed to stand for 4 to 8 hours. The product is filtered and washed, and then the product is vacuum dried to obtain the organophosphorus flame retardant (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphite) (OPMP).
[0011] Furthermore, in step 1, the molar ratio of trishydroxymethylphosphine oxide to dioxane is 1:(1-2).
[0012] Furthermore, in step 2, the molar ratio of trihydroxymethylphosphine oxide to diphenylphosphinoyl chloride is 1:3.
[0013] Furthermore, in step 2, the dripping speed is 1 drop every 3 seconds.
[0014] Furthermore, in step three, the reflux temperature is 101°C.
[0015] Furthermore, the vacuum drying conditions in step three are: drying in a vacuum drying oven at 80-85° C. for 4-8 hours.
[0016] The organic phosphorus flame retardant of the invention is used for flame retardant polyester polymer materials.
[0017] Beneficial effects of the present invention:
[0018] The organophosphorus flame retardant OPMP of the present invention is a white powder with a yield of more than 90%. The melting point of the product is 187°C. Unlike traditional liquid organophosphate flame retardants, this product is easy to add due to its relatively high melting point and has excellent processing performance. Thermogravimetric analysis tests show that the initial decomposition temperature of the flame retardant is 306°C, indicating that the organophosphorus flame retardant OPMP has excellent thermal stability and meets the processing requirements of traditional polyester polymer materials.
[0019] The organophosphorus flame retardant OPMP of the present invention introduces a large number of non-polar benzene ring structures and phosphate structures into its structure, and contains PO and PC groups and high phosphorus content aromatic phosphate flame retardants, thereby increasing its compatibility with polyester polymer materials.
[0020] The organophosphorus flame retardant OPMP of the present invention has a high phosphorus content of 16.73%, and has a high flame retardant efficiency in polyester materials. Compared with DOPO-based reactive flame retardants and traditional phosphorus flame retardants containing PC and PO, the melting point of OPMP is better matched with the processing temperature of most polyester materials, and due to the conjugated stacking effect and excellent compatibility between OPMP and the aromatic ring of the material matrix, it is not easy to migrate and precipitate.
[0021] OPMP was added to polyester polymer thermoplastic polyurethane (TPU) materials. When the OPMP addition amount was only 5wt%, the flame retardant TPU composite material passed the vertical combustion UL-94V-0 level, and the limiting oxygen index was increased from 19.0% of the pure TPU material to 29.7%. Then, OPMP was added to polycarbonate (PC) materials. When the OPMP addition amount was only 7wt%, the flame retardant PC composite material passed the vertical combustion UL-94V-0 level, and the limiting oxygen index was increased from 25.3% of the pure PC material to 37.8%. The flame retardant exhibits excellent flame retardant properties in polyester polymer materials such as TPU and PC. Since the addition amount of the flame retardant OPMP is low and it has good compatibility with polyester polymers, the introduction of the flame retardant OPMP has little effect on the mechanical, processing and other properties of polyester polymer materials, thereby obtaining a flame retardant polyester polymer material with excellent comprehensive performance.
[0022] The synthesis method of the organophosphorus flame retardant of the present invention is simple, does not require a catalyst, has a high yield, and is easy to industrialize. The solvent in the synthesis process can be recycled and reused, saving costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is the thermogravimetric analysis curve of the product OPMP prepared in Example 1;
[0024] Figure 2 The FTIR spectra of the raw materials trimethylolphosphine oxide, diphenylphosphinoyl chloride and the product OPMP;
[0025] Figure 3 The product OPMP prepared in Example 1 1 H NMR spectrum;
[0026] Figure 4 The product OPMP prepared in Example 1 31 P NMR spectrum. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.
[0028] Specific implementation method 1: The organic phosphorus flame retardant in this implementation method is (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphinate), and its chemical structure is as follows:
[0029]
[0030] The present invention uses trihydroxymethylphosphine oxide and diphenylphosphinoyl chloride as starting materials, and introduces PO and PC groups into the same molecular structure through nucleophilic substitution reaction, thereby preparing an aromatic phosphate flame retardant with a high phosphorus content. The flame retardant is a polyaryl structure and has good compatibility with aromatic polyester polymer materials. The present invention solves the problems of low flame retardant efficiency, poor compatibility with material matrix, low thermal stability, and reduced material mechanics of the traditional organic phosphorus flame retardant used for flame retardant of aromatic polyester polymers such as thermoplastic polyurethane and polycarbonate. While giving flame retardant polyester polymer materials excellent flame retardant properties, the mechanical properties remain unchanged, making them have excellent comprehensive properties, and expanding the application scope of flame retardant polyester polymer materials in current emerging fields.
[0031] Specific embodiment 2: The preparation method of the organophosphorus flame retardant in this embodiment comprises the following steps:
[0032] 1. Add trimethylolphosphine oxide and dioxane to a reaction device to obtain a mixed solution, heat the mixed solution to 70-80° C., and stir until dissolved;
[0033] 2. Then, diphenylphosphinoyl chloride is placed in a constant pressure dropping funnel and added dropwise to the reaction device, the dropping speed is controlled, and the reaction temperature is maintained at 70-80°C during the dropping process;
[0034] 3. After the dropwise addition is completed, the reaction temperature is raised to the reflux temperature, and the reaction is continued under reflux for 3 to 6 hours. After the reaction is completed, it is cooled to room temperature and allowed to stand for 4 to 8 hours. The product is filtered and washed, and then the product is vacuum dried to obtain the organophosphorus flame retardant (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphite) (OPMP).
[0035] Specific embodiment 3: This embodiment differs from specific embodiment 2 in that the molar ratio of tris(hydroxymethyl)phosphine oxide to dioxane in step 1 is 1:(1-2). Other aspects are the same as those of specific embodiment 2.
[0036] Specific embodiment 4: This embodiment is different from specific embodiment 2 or 3 in that the molar ratio of trimethylolphosphine oxide to diphenylphosphinyl chloride is 1:3. Other aspects are the same as specific embodiment 2 or 3.
[0037] Specific implementation mode 5: This implementation mode is different from the first one of the second to fourth implementation modes in that the dripping speed in step 2 is 1 drop every 3 seconds. The rest is the same as the first one of the second to fourth implementation modes.
[0038] Specific embodiment 6: This embodiment is different from specific embodiments 2 to 5 in that the reflux temperature in step 3 is 101° C. The rest is the same as specific embodiments 2 to 5.
[0039] Specific embodiment 7: This embodiment differs from specific embodiments 2 to 6 in that the vacuum drying condition in step 3 is: drying in a vacuum drying oven at 80 to 85° C. for 4 to 8 hours. The rest is the same as specific embodiments 2 to 6.
[0040] Specific implementation method 8: In this implementation method, the organic phosphorus flame retardant is used to flame retard polyester polymer materials.
[0041] The embodiments of the present invention are described in detail below. The following embodiments are implemented on the premise of the technical solution of the present invention, and detailed implementation schemes and specific operation processes are given, but the protection scope of the present invention is not limited to the following embodiments.
[0042] Embodiment 1:
[0043] The preparation method of the organophosphorus flame retardant OPMP in this embodiment comprises the following steps:
[0044] A stirrer, a thermometer, a spherical condenser, a nitrogen protection and a constant pressure dropping funnel were installed on a 500 mL dry five-necked flask, and the flask was purged repeatedly with dry nitrogen several times to ensure that there was no water and no oxygen in the reactor.
[0045] Add 14.21g of trimethylolphosphine oxide and 100g of dioxane to a five-necked flask, heat to 75°C with a heating device, stir thoroughly until all dissolved and the solution is clear and transparent. Weigh 72.43g of diphenylphosphinoyl chloride in a constant pressure dropping funnel, control the drop rate to 1 drop every 3 seconds, and slowly drop it into the five-necked flask. As the reaction proceeds, white solid substances are obviously generated in the solution. During the dropwise addition, the temperature of the reaction system is controlled at 75°C. After the dropwise addition is completed, the temperature of the heating equipment is raised to 101°C, and the reaction is continued for 4h under reflux. After stopping the reaction, cool to room temperature and stand for 3h. After no more crystals are produced, separate the target product generated by the reaction by suction filtration and washing. Then place the obtained white crystals in a vacuum drying oven at 80°C and dry for 6h to obtain the target product (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphinate) (OPMP). The synthetic route is as follows:
[0046]
[0047] The thermogravimetric analysis curve of the organophosphorus flame retardant OPMP prepared in this example is as follows: Figure 1 As shown, from Figure 1 It can be seen that the initial thermal decomposition temperature of the product OPMP is 306°C, indicating that OPMP has excellent thermal stability and can meet the processing temperature requirements of most polyester polymer materials. Pure OPMP is a white solid powder at room temperature, and the flame retardant OPMP has a clear melting point of 187°C, which shows that the flame retardant is easy to add during the processing, and because it has a corresponding melting point, it has good dispersibility and compatibility in the material matrix during the TPU material processing.
[0048] (I) Characterization of the product (oxy-5-phosphotriyl) tris(methylene) tris(diphenylphosphinate) (OPMP)
[0049] The infrared spectra of the raw materials trishydroxymethylphosphine oxide (THPO), diphenylphosphinoyl chloride (DPPC) and the product (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphinoyl) (OPMP) are shown in Figure 2 As shown. According to the infrared spectrum analysis of raw material THPO, 3191cm -1 The absorption peak at 2850cm is the absorption peak of -OH. -1 The absorption peak at 3070cm is the stretching vibration peak of CH on trihydroxymethylphosphine oxide. -1 The absorption peak is the stretching vibration peak of CH on the benzene ring; 1437cm -1 The absorption peak at 1120cm is the stretching vibration peak of P-Ph; -1 The absorption peak at 960 cm is the characteristic peak of P=O. -1 At the same time, the characteristic peak of the newly generated PO in the product OPMP structure is 3191cm -1 、617cm -1 The characteristic peaks of -OH and P-Cl disappeared obviously, indicating that trihydroxymethylphosphine oxide and diphenylphosphinoyl chloride reacted completely and the flame retardant OPMP was successfully synthesized.
[0050] Product OPMP 1 H NMR spectrum Figure 3 As shown. From OPMP 1 It can be seen from the H NMR graph that the peak at 7.75 ppm is the chemical shift of H on the a benzene ring identified in the structure, the peak at 7.47 ppm is the chemical shift of H on the b benzene ring identified in the structure, and the peak at 3.56 ppm is the chemical shift of the c hydrogen atom on trishydroxymethylphosphine oxide.
[0051] Product OPMP 31P NMR spectrum Figure 4 As shown. From OPMP 31 It can be seen from the P NMR spectrum that there are two phosphorus peaks at 23.41ppm and 23.06ppm, which are respectively attributed to the P atoms at positions a and b on diphenylphosphinoyl chloride and trihydroxymethylphosphine oxide, and the peak area ratio of the two peaks is 3:1. This indicates that there are two phosphorus chemical environments in OPMP, and the number is 3:1, which is consistent with the theoretical value. This further proves that OPMP was successfully synthesized.
[0052] (II) Performance analysis of flame retardant polyester polymer materials
[0053] 1. Sample preparation
[0054] The synthetic product (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphite) (OPMP) and thermoplastic polyurethane (TPU) were melt blended in a torque rheometer at a certain mass ratio for 10 minutes, with the temperature of each heating zone at 187°C and the speed at 60r / min. After the flame-retardant TPU composite material was mixed evenly in the cavity, it was placed on a flat vulcanizer and hot-pressed at 187°C and 10MPa, and then cut into standard specimens for performance testing.
[0055] The synthetic product (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphite) (OPMP) and polycarbonate (PC) were melt blended in a torque rheometer at a certain mass ratio for 10 minutes, with the temperature of each heating zone at 235°C and the speed at 60r / min. After the flame-retardant PC composite material was mixed evenly in the cavity, it was placed on a flat vulcanizer and hot-pressed at 235°C and 10MPa, and then cut into standard specimens for performance testing.
[0056] 2. Flame retardant performance test of TPU composite materials
[0057] The flame retardant properties of TPU composites were characterized by vertical combustion (UL-94) and limiting oxygen index (LOI), and the test results are shown in Table 1. Pure TPU is very easy to burn in the air, accompanied by a large number of flaming droplets, and its LOI value is only 19.0%, with no vertical combustion grade. With the introduction of organophosphorus flame retardant OPMP, the flame retardant properties of TPU flame retardant composites are significantly improved. When the addition amount of OPMP reaches 3wt%, the TPU / 3wt%OPMP composite material passes the UL-94V-2 level, and the oxygen index is increased to 27.5%. When the addition amount of OPMP reaches 5wt%, the TPU / 5wt%OPMP composite material successfully passes the UL-94V-0 level, and the LOI value is as high as 29.7%. The test results show that OPMP has excellent flame retardant efficiency for thermoplastic polyurethane materials. At the same time, when the addition amount of OPMP reaches 5wt%, the mechanical properties of the material are basically the same as those of the raw materials, and the original transparency of TPU is maintained, which provides a good solution for the preparation of flame retardant TPU composite materials with excellent comprehensive performance.
[0058] Table 1 Vertical combustion and limiting oxygen index test data of TPU / OPMP composites
[0059]
[0060] 3. Flame retardant performance test of PC composite materials
[0061] The flame retardant properties of PC materials were characterized by vertical combustion (UL-94) and limiting oxygen index (LOI), and the test results are shown in Table 2. Pure PC releases a large amount of heat during combustion and produces droplets. The droplets quickly ignite the cotton wool, which can easily cause secondary disasters. With the introduction of the organophosphorus flame retardant OPMP, the flame retardant properties of PC flame retardant composites have been significantly improved. When the OPMP addition amount reaches 7wt%, the PC / 7wt% OPMP composite material successfully passes the UL-94V-0 level, and the LOI value is as high as 37.8%. The test results show that OPMP has excellent flame retardant efficiency for polycarbonate materials. At the same time, when the OPMP addition amount reaches 7wt%, the mechanical properties of the material are basically the same as those of the raw materials, and the original transparency of PC is maintained, which provides a new strategy for the preparation of transparent flame retardant PC composite materials.
[0062] Table 2 Vertical combustion and limiting oxygen index test data of PC / OPMP composites
[0063]
[0064] Compared with traditional flame retardants, the advantages of synthetic organophosphorus flame retardant OPMP in flame retardant polyester polymers are as follows: 1) The synthesis method of OPMP is simple, time-saving, high in yield and purity, which is conducive to its industrial production; 2) OPMP has excellent thermal stability, can well meet the processing requirements of various materials, and has a wide range of uses; 3) OPMP introduces PC and PO groups into the same molecular structure, and through the synergistic effect of gas phase and condensed phase, it shows excellent flame retardant efficiency in polyester polymers; 4) OPMP molecular structure contains a large amount of PC and P-Ph, which will produce phosphorus and benzene free radicals during combustion, which can effectively quench high-energy free radicals such as H, ·O, ·HO· generated during the combustion of polyester polymer materials in the gas phase, and has an excellent gas phase inhibition effect; 5) OPMP molecular structure contains a large number of PO groups, which will generate structures such as metaphosphoric acid, pyrophosphoric acid and polyphosphoric acid during combustion, promote the dehydration and carbonization of polyester polymer substrates, form a hard and dense carbon layer, and have an excellent condensed phase flame retardant effect. 6) OPMP has high flame retardant efficiency in polyester polymer materials and requires a small amount of addition. At the same time, it has a phosphate structure and has good compatibility with polyester polymer materials, so that it maintains the mechanical properties and transparency of the original material during the flame retardant polyester polymer process. In summary, the successful design of the organophosphorus flame retardant OPMP provides a new idea for the preparation of flame retardant polyester polymer materials with excellent comprehensive performance.
Claims
1. An organophosphorus flame retardant, characterized in that: The flame retardant is (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphinate), and its chemical structure is as follows:
2. The method for preparing an organophosphorus flame retardant according to claim 1, characterized in that: The method comprises the following steps:
1. Add trimethylolphosphine oxide and dioxane to a reaction device to obtain a mixed solution, heat the mixed solution to 70-80° C., and stir until dissolved; 2. Then, diphenylphosphinoyl chloride is placed in a constant pressure dropping funnel and added dropwise to the reaction device, the dropping speed is controlled, and the reaction temperature is maintained at 70-80°C during the dropping process; 3. After the dropwise addition is completed, the reaction temperature is raised to the reflux temperature, and the reaction is continued under reflux for 3 to 6 hours. After the reaction is completed, it is cooled to room temperature and allowed to stand for 4 to 8 hours. The product is filtered and washed, and then the product is vacuum dried to obtain the organophosphorus flame retardant (oxy-5-phosphorus triyl) tris(methylene) tris(diphenylphosphite).
3. The method for preparing an organophosphorus flame retardant according to claim 2, characterized in that: In step 1, the molar ratio of trimethylolphosphine oxide to dioxane is 1:(1-2).
4. The method for preparing an organophosphorus flame retardant according to claim 2 or 3, characterized in that: The molar ratio of trishydroxymethylphosphine oxide to diphenylphosphinyl chloride is 1:
3.
5. The method for preparing an organophosphorus flame retardant according to claim 4, characterized in that: The dripping speed in step 2 is 1 drop every 3 seconds.
6. The method for preparing an organophosphorus flame retardant according to claim 2, characterized in that: The reflux temperature in step 3 is 101°C.
7. The method for preparing an organophosphorus flame retardant according to claim 2, characterized in that: The vacuum drying conditions in step 3 are: drying in a vacuum drying oven at 80-85° C. for 4-8 hours.
8. The organic phosphorus flame retardant as claimed in claim 1 is used for flame retardant polyester polymer materials.
Citation Information
Patent Citations
Phosphorus-containing compound and preparation method thereof, and application of phosphorus-containing compound in preparation of anti-aging flame-retardant polyurethane
CN116854736A
Phosphorus-nitrogen type flame retardant with multiple phosphorus-containing groups as well as preparation method and application of phosphorus-nitrogen type flame retardant
CN117263980A
Cited By
A toluene-2,4-dicarbamate dimethyl methylphosphonate and a method for preparing the same
CN122978169A