Amino cross-linking agent, cross-linked biomass amino material prepared based on amino cross-linking agent and preparation method of cross-linked biomass amino material
By using polyphenol compounds and other components in biomass amino materials to prepare amino crosslinking agents to form stable chemical bonds, the problem of poor mechanical properties of traditional biomass amino materials is solved, cost reduction and performance improvement is achieved, and industrial applications are provided potential.
Patent Information
- Application Number
- CN202411004968.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
AI Technical Summary
Traditional biomass amino materials have poor mechanical properties and are difficult to meet the needs of industrial applications. The chemical modification method based on the structural characteristics of the amino materials themselves is costly and difficult to be used in industrial production.
The amino crosslinking agent is prepared by reacting components such as polyphenol compounds, paraformaldehyde, magnesium chloride, triethylamine and hydrochloric acid, and crosslinking it with the amino material to form stable chemical bonds and enhance the mechanical properties of the material.
It significantly improves the mechanical properties of amino materials, reduces production costs, and has a wide range of industrial application prospects.
Smart Images

Figure CN118955586A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomass amino materials, and in particular to an amino cross-linking agent, a cross-linked biomass amino material prepared based on the amino cross-linking agent, and a preparation method thereof. Background Art
[0002] There are abundant amino groups in the structure of amino materials, which have various functional effects. Among them, chitosan materials, gelatin protein materials and other biomass amino materials have received widespread attention. Chitosan is the product of chitin removing some acetyl groups. It is mostly prepared from the shells of crustaceans such as shrimps and crabs, animal bones and cell walls of fungi. Chitosan has good film-forming properties and degradability, and is widely used in the field of functional materials. Gelatin is a type of biodegradable protein structure macromolecule. It is a product prepared by hydrolyzing collagen in the skin, bones and other tissues of animals. It is one of the most studied biomass materials and is widely used in food, medicine, chemical and other industries. These amino materials have good biocompatibility, a wide range of raw material sources, and are cheap and easy to obtain. They are ideal choices for preparing new functional materials under the concept of sustainable development.
[0003] Traditional biomass amino materials generally have inherent defects of poor mechanical properties, which are difficult to meet the application requirements of production and life. To this end, the relevant field has proposed a method of chemical modification based on the structural characteristics of the amino materials themselves. However, the method of chemical modification based on the structural characteristics of the amino materials themselves has the problem of high cost and difficulty in industrial production. Summary of the invention
[0004] The present invention solves the technical problems that the method of chemical modification based on the structural characteristics of the amino material itself is high in cost and difficult to be used in industrial production by disclosing an amino crosslinking agent, a crosslinked biomass amino material prepared based on the amino crosslinking agent and a preparation method thereof.
[0005] In order to solve the above technical problems, the present invention provides an amino cross-linking agent in the first aspect. The amino cross-linking agent comprises the following component raw materials in parts by weight:
[0006] 0.5-2 parts of polyphenol compounds, 0.4-1 parts of paraformaldehyde, 0.5-2 parts of magnesium chloride, 1-4 parts of triethylamine, 20-40 parts of organic solvents, 40-60 parts of hydrochloric acid;
[0007] The mixture of the polyphenol compound, paraformaldehyde, magnesium chloride, triethylamine and organic solvent is reacted at a temperature of 55-80° C. for 6-12 hours, then heating is stopped, and the hydrochloric acid is added and stirred to obtain a reaction solution; the reaction solution is concentrated, separated and dried to obtain the amino cross-linking agent.
[0008] In some embodiments, concentrating, separating and drying the reaction solution comprises:
[0009] The reaction solution is concentrated under reduced pressure, separated by using a macroporous adsorption resin, eluted with a 50-70% by mass ethanol solution, the eluate is collected, and the eluate is concentrated and dried;
[0010] The macroporous resin is any one of HP-20, ADS-7, D101, AB-8, S-8, and HPD100.
[0011] In some embodiments, the following components are included in the following weight parts:
[0012] 1 part of polyphenol compound, 0.8 parts of paraformaldehyde, 1.5 parts of magnesium chloride, 3 parts of triethylamine, 30 parts of organic solvent, 50 parts of hydrochloric acid.
[0013] In some embodiments, the polyphenol compound is any one of tea polyphenols or tannic acid, preferably tannic acid;
[0014] And / or, the organic solvent is any one of tetrahydrofuran, acetone or acetonitrile, preferably acetone.
[0015] In a second aspect, the present invention provides a cross-linked biomass amino material, wherein the cross-linked biomass amino material comprises an amino material and an amino cross-linking agent.
[0016] In some embodiments, the weight ratio of the amino material to the amino cross-linking agent is 80-120:1.
[0017] It should be noted that the weight ratio of the amino material to the amino cross-linking agent can be 80:1, 90:1, 100:1, 110:1, 120:1 or 85:1, 95:1, 105:1, 115:1, etc., any one within the weight ratio range is acceptable, and the present application embodiment does not make any special limitation. The weight ratio of the amino material to the amino cross-linking agent is preferably 100:1.
[0018] In some embodiments, the amino material is any one of a gelatin solution or a chitosan solution, wherein the mass fraction of gelatin contained in the gelatin solution is 8-12%, and the mass fraction of chitosan contained in the chitosan solution is 8-12%; the mass fraction of gelatin contained in the gelatin solution is preferably 10%, and the mass fraction of chitosan contained in the chitosan solution is preferably 10%.
[0019] The present invention provides a method for preparing the cross-linked biomass amino material in a third aspect, comprising mixing the amino cross-linking agent with the amino material, standing and drying to obtain the cross-linked biomass amino material.
[0020] In some embodiments, the standing time is 8-16 hours;
[0021] And / or, the drying temperature is 45-55° C. and the drying time is 20-26 hours.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The amino cross-linking agent provided by the present invention is obtained by reacting a polyphenol compound, an organic solvent, magnesium chloride, triethylamine, polyformaldehyde and hydrochloric acid. Specifically, the polyphenol compound is firstly dissolved by an organic solvent, and then magnesium chloride is added, so that the polyphenol compound and the magnesium chloride generate a phenol magnesium salt intermediate; further, the phenol magnesium salt intermediate generates tautomerism under the action of triethylamine to generate a ketone magnesium salt intermediate; secondly, the ketone magnesium salt intermediate is converted into an oxone magnesium salt intermediate after complexation and rearrangement reaction under the action of polyformaldehyde; finally, the oxone magnesium salt intermediate undergoes ketone-enol tautomerism and elimination reaction under the acidic condition provided by hydrochloric acid to obtain a light yellow powder reaction product, and the light yellow powder reaction product is the amino cross-linking agent. On the one hand, on the basis of retaining the active phenolic hydroxyl groups in the structure of the polyphenolic compound, a functional aldehyde group is introduced to prepare an amino crosslinking agent; on the other hand, the aldehyde group in the amino crosslinking agent can form a stable chemical bond with the amino structure in the amino material by chemical crosslinking, and the amino crosslinking agent retains the original active phenolic hydroxyl groups, so that it can form a multi-point hydrogen bond crosslinking effect with the amino material. Under the joint action of the two crosslinkings, the mechanical properties of the amino material are significantly improved. The amino crosslinking agent is based on the structural modification of polyphenolic compounds, with green and safe raw materials, simple preparation method, strong crosslinking effect, reduced cost, and has broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 This is a comparison chart of the mechanical properties of the membrane material with added modified cross-linking agent, the membrane material with added unmodified cross-linking agent, and the membrane material without added cross-linking agent in Experimental Example 2.
[0026] Figure 2 This is a comparison chart of the mechanical properties of the membrane material with added modified cross-linking agent, the membrane material with added unmodified cross-linking agent, and the membrane material without added cross-linking agent in Experimental Example 3.
[0027] Figure 3This is a comparison chart of the mechanical properties of the membrane material with added modified cross-linking agent, the membrane material with added unmodified cross-linking agent, and the membrane material without added cross-linking agent in Test Example 4. DETAILED DESCRIPTION
[0028] The present invention is described in detail below in conjunction with the accompanying drawings and specific examples, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the following examples are conventional means well known to those skilled in the art, and the raw materials, components, etc. used in the following examples, unless otherwise specified, can be obtained from commercial sources.
[0029] The technical solution of the present invention will be described below in conjunction with specific embodiments.
[0030] Example 1
[0031] This embodiment provides an amino cross-linking agent, which includes the following raw material components in parts by weight:
[0032] 1 part of tannic acid, 30 parts of acetone, 1.5 parts of magnesium chloride, 3 parts of triethylamine, 0.8 parts of paraformaldehyde, 50 parts of hydrochloric acid; the concentration of the hydrochloric acid is 1 mol / L;
[0033] Place 1 part of tannic acid in a reaction bottle under an ice-water bath, then add 30 parts of acetone to dissolve it, then add 1.5 parts of magnesium chloride, 3 parts of triethylamine and 0.8 parts of paraformaldehyde, and stir to dissolve to obtain a mixture; react the mixture at a temperature of 60° C. for 10 hours, stop heating after the reaction, add 50 parts of 1 mol / L hydrochloric acid, and continue stirring for 30 minutes to obtain a reaction solution; concentrate the reaction solution under reduced pressure, separate it with HP-20 macroporous adsorption resin, elute it with 60% ethanol solution by mass, and collect the eluate; concentrate and dry the eluate to obtain an amino cross-linking agent.
[0034] Example 2
[0035] This embodiment provides an amino cross-linking agent, which includes the following raw material components in parts by weight:
[0036] 0.5 parts of tannic acid, 20 parts of acetone, 0.5 parts of magnesium chloride, 1 part of triethylamine, 0.4 parts of paraformaldehyde, 40 parts of hydrochloric acid; the concentration of the hydrochloric acid is 0.8 mol / L;
[0037] 0.5 parts of tannic acid are placed in a reaction bottle under an ice-water bath, and then 20 parts of acetone are added to dissolve it, and then 0.5 parts of magnesium chloride, 1 part of triethylamine and 0.4 parts of paraformaldehyde are added, and the mixture is stirred and dissolved to obtain a mixture; the mixture is reacted at a temperature of 65° C. for 12 hours, and after the reaction is completed, heating is stopped, 40 parts of hydrochloric acid with a concentration of 0.8 mol / L are added, and stirring is continued for 25 minutes to obtain a reaction solution; the reaction solution is concentrated under reduced pressure and separated by HP-20 macroporous adsorption resin, eluted with 50% by mass ethanol solution, and the eluate is collected; the eluate is concentrated and dried to obtain an amino cross-linking agent.
[0038] Example 3
[0039] This embodiment provides an amino cross-linking agent, which includes the following raw material components in parts by weight:
[0040] 2 parts of tannic acid, 40 parts of acetone, 2 parts of magnesium chloride, 4 parts of triethylamine, 1 part of paraformaldehyde, and 60 parts of hydrochloric acid; the concentration of the hydrochloric acid is 1.2 mol / L;
[0041] 2 parts of tannic acid are placed in a reaction bottle under an ice-water bath, and then 40 parts of acetone are added to dissolve it, and then 2 parts of magnesium chloride, 4 parts of triethylamine and 1 part of paraformaldehyde are added, and the mixture is obtained after stirring and dissolving; the mixture is reacted at a temperature of 55° C. for 8 hours, and after the reaction is completed, heating is stopped, 60 parts of hydrochloric acid with a concentration of 1.2 mol / L are added, and stirring is continued for 40 minutes to obtain a reaction solution; the reaction solution is concentrated under reduced pressure and separated by HP-20 macroporous adsorption resin, eluted with 70% by mass ethanol solution, and the eluate is collected; the eluate is concentrated and dried to obtain an amino cross-linking agent.
[0042] Example 4
[0043] This embodiment provides an amino cross-linking agent, which includes the following raw material components in parts by weight:
[0044] 1 part of tea polyphenols, 20 parts of tetrahydrofuran, 0.5 parts of magnesium chloride, 1 part of triethylamine, 0.4 parts of paraformaldehyde, and 30 parts of hydrochloric acid; the concentration of the hydrochloric acid is 1 mol / L;
[0045] Place 1 part of tea polyphenol in a reaction bottle under an ice water bath, then add 20 parts of tetrahydrofuran to dissolve it, then add 0.5 parts of magnesium chloride, 1 part of triethylamine and 0.4 parts of paraformaldehyde, and stir to dissolve to obtain a mixture; react the mixture at a temperature of 80°C for 6 hours, stop heating after the reaction, add 30 parts of 1 mol / L hydrochloric acid, and continue stirring for 30 minutes to obtain a reaction solution; concentrate the reaction solution under reduced pressure, separate it with ADS-7 macroporous adsorption resin, elute it with 60% ethanol solution by mass, and collect the eluate; concentrate and dry the eluate to obtain an amino cross-linking agent.
[0046] Example 5
[0047] This embodiment provides an amino cross-linking agent, which includes the following raw material components in parts by weight:
[0048] 1 part of tannic acid, 25 parts of acetonitrile, 1 part of magnesium chloride, 2 parts of triethylamine, 0.6 parts of paraformaldehyde, 40 parts of hydrochloric acid; the concentration of the hydrochloric acid is 1 mol / L;
[0049] Place 1 part of tannic acid in a reaction bottle under an ice-water bath, then add 25 parts of acetonitrile to dissolve it, then add 1 part of magnesium chloride, 2 parts of triethylamine and 0.6 parts of paraformaldehyde, and stir to dissolve to obtain a mixture; react the mixture at a temperature of 70°C for 8 hours, stop heating after the reaction, add 40 parts of 1 mol / L hydrochloric acid, and continue stirring for 30 minutes to obtain a reaction solution; concentrate the reaction solution under reduced pressure, separate it with D101 macroporous adsorption resin, elute it with 60% ethanol solution by mass, and collect the eluate; concentrate and dry the eluate to obtain an amino cross-linking agent.
[0050] Comparative Example 1
[0051] Compared with the amino cross-linking agent in Example 1, the difference is that the mixture is reacted at a temperature of 90° C. for 10 hours.
[0052] Comparative Example 2
[0053] Compared with the amino cross-linking agent in Example 1, the difference is that the mixture is reacted at a temperature of 45° C. for 10 hours.
[0054] Comparative Example 3
[0055] Compared with the amino cross-linking agent in Example 1, the difference is that the mixture is reacted at a temperature of 60° C. for 12 hours.
[0056] Comparative Example 4
[0057] Compared with the amino cross-linking agent in Example 1, the difference is that the mixture is reacted at a temperature of 60° C. for 6 hours.
[0058] Test Example 1
[0059] This test example provides an experiment for determining the aldehyde content of an amino cross-linking agent.
[0060] In this test example, the hydroxylamine hydrochloride method was used to measure the aldehyde content in the amino cross-linking agents prepared in Examples 1-5 and Comparative Examples 1-4, respectively. The results are shown in Tables 1 and 2.
[0061] Table 1 Aldehyde content in the amino crosslinking agents prepared in Examples 1-5
[0062] Example 1 Example 2 Example 3 Example 4 Example 5 Aldehyde content (mmol / g) 3.8mmol / g 3.4mmol / g 3.2mmol / g 3.5mmol / g 3.7mmol / g
[0063] Table 2 Aldehyde content in the amino crosslinking agents prepared in Comparative Examples 1-7
[0064] Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Aldehyde content (mmol / g) 3.3mmol / g 2.3mmol / g 3.5mmol / g 3.1mmol / g
[0065] As shown in Table 1, the aldehyde content in the amino cross-linking agent prepared in Examples 1-5 is relatively high, wherein the aldehyde content in the amino cross-linking agent prepared in Example 1 is the highest. As shown in Tables 1 and 2, from the comparison between Example 1 and Comparative Examples 1-4, the aldehyde content decreased by 0.5mmol / g, 1.5mmol / g, 0.3mmol / g and 0.7mmol / g, respectively, indicating that both the reaction temperature and the reaction time will affect the aldehyde content in the amino cross-linking agent. In the process of the reaction temperature affecting the reaction yield, too high a reaction temperature will destroy the structure of the reaction substrate, and too low a reaction temperature will make the reaction unable to proceed completely, both of which will reduce the reaction yield. Similarly, in the process of the reaction time affecting the reaction, too long a reaction time will bring about the occurrence of more side reactions, and too short a reaction time will make the substrate reaction incomplete, thereby reducing the reaction yield.
[0066] Test Example 2
[0067] This test example provides an amino cross-linking agent for the mechanical properties of amino materials.
[0068] Mix 1 part of the amino cross-linking agent prepared in Example 1 with 100 parts of gelatin solution to obtain a mixed solution, pour the mixed solution onto a flat plate, let it stand for 12 hours, and then dry it in an oven at 50°C for 24 hours to obtain a cross-linked biomass amino material, that is, a modified cross-linking agent added membrane material; the gelatin solution is a gelatin solution with a mass fraction of 10% prepared by distilled water.
[0069] Unmodified cross-linking agent membrane material: Mix 1 part of tannic acid used in Example 1 with 100 parts of gelatin solution to obtain a mixed solution, pour the mixed solution onto a flat plate, let it stand for 12 hours, and then dry it in an oven at 50°C for 24 hours to obtain an unmodified cross-linking agent membrane material, that is, a membrane material with added unmodified cross-linking agent; the gelatin solution is a gelatin solution with a mass fraction of 10% prepared by distilled water.
[0070] Membrane material without added crosslinking agent: directly pour 100 parts of gelatin solution onto a flat plate, let it stand for 12 hours, and then dry it in a 50°C oven for 24 hours to obtain a membrane material without added crosslinking agent; the gelatin solution is prepared by using distilled water to prepare gelatin with a mass fraction of 10%.
[0071] The membrane material with modified crosslinking agent, the membrane material with unmodified crosslinking agent and the membrane material without crosslinking agent were cut into 15mm×30mm pieces respectively as test membrane samples, and the mechanical properties of each were measured by electronic tensile testing machine. Figure 1 shown.
[0072] Depend on Figure 1 It can be obtained that the tensile displacement at break of the membrane material without adding cross-linking agent is 18 mm, and the maximum tensile force is 29 N; the tensile displacement at break of the membrane material with adding unmodified cross-linking agent is 21 mm, and the maximum tensile force is 43 N; the tensile displacement at break of the membrane material with adding modified cross-linking agent is 39 mm, and the maximum tensile force is 97 N; compared with the membrane material without adding cross-linking agent, the tensile displacement at break of the membrane material with adding modified cross-linking agent is increased by 117%, and the maximum tensile force is increased by 234%, and the mechanical properties of the membrane material with adding modified cross-linking agent are significantly improved.
[0073] Test Example 3
[0074] This test example provides an amino cross-linking agent for the mechanical properties of amino materials.
[0075] Mix 1 part of the amino cross-linking agent prepared in Example 4 with 100 parts of gelatin solution to obtain a mixed solution, pour the mixed solution onto a flat plate, let it stand for 12 hours, and then dry it in an oven at 50°C for 24 hours to obtain a cross-linked biomass amino material, that is, a modified cross-linking agent added membrane material; the gelatin solution is a gelatin solution with a mass fraction of 10% prepared by distilled water.
[0076] Unmodified cross-linking agent membrane material: Mix 1 part of the tea polyphenols used in Example 4 with 100 parts of gelatin solution to obtain a mixed solution, pour the mixed solution onto a flat plate, let it stand for 12 hours, and then dry it in an oven at 50°C for 24 hours to obtain an unmodified cross-linking agent membrane material, that is, a membrane material with added unmodified cross-linking agent; the gelatin solution is a gelatin solution with a mass fraction of 10% prepared by distilled water.
[0077] Membrane material without added crosslinking agent: directly pour 100 parts of gelatin solution onto a flat plate, let it stand for 12 hours, and then dry it in a 50°C oven for 24 hours to obtain a membrane material without added crosslinking agent; the gelatin solution is prepared by using distilled water to prepare gelatin with a mass fraction of 10%.
[0078] The membrane material with modified crosslinking agent, the membrane material with unmodified crosslinking agent and the membrane material without crosslinking agent were cut into 15mm×30mm pieces respectively as test membrane samples, and the mechanical properties of each were measured by electronic tensile testing machine. Figure 2 shown.
[0079] The tensile displacement at break of the membrane material without adding cross-linking agent is 15mm, and the maximum tensile force is 20N; the tensile displacement at break of the membrane material with adding unmodified cross-linking agent is 14mm, and the maximum tensile force is 38N; the tensile displacement at break of the membrane material with adding modified cross-linking agent is 18mm, and the maximum tensile force is 87N; compared with the membrane material without adding cross-linking agent, the tensile displacement at break of the membrane material with adding modified cross-linking agent is increased by 20%, and the maximum tensile force is increased by 335%, and the mechanical properties of the membrane material with adding cross-linking agent are significantly improved.
[0080] Test Example 4
[0081] This test example provides an amino cross-linking agent for the mechanical properties of amino materials.
[0082] One portion of the amino cross-linking agent prepared in Example 5 was mixed with 100 portions of chitosan solution to obtain a mixed solution, which was poured onto a plate, allowed to stand for 12 hours, and then dried in an oven at 50°C for 24 hours to obtain a cross-linked biomass amino material, i.e., a modified cross-linking agent-added membrane material; the chitosan solution was prepared by using an aqueous acetic acid solution with a mass fraction of 1% to prepare a chitosan solution with a mass fraction of 10%.
[0083] Unmodified cross-linking agent membrane material: Mix 1 part of tannic acid used in Example 5 with 100 parts of chitosan solution to obtain a mixed solution, pour the mixed solution onto a plate, let it stand for 12 hours, and then dry it in an oven at 50°C for 24 hours to obtain an unmodified cross-linking agent membrane material, that is, a membrane material with added unmodified cross-linking agent; the chitosan solution is a chitosan solution with a mass fraction of 10% prepared by using a 1% mass fraction acetic acid aqueous solution.
[0084] Membrane material without added crosslinking agent: 100 parts of chitosan solution were directly poured onto a plate, allowed to stand for 12 hours, and then dried in an oven at 50°C for 24 hours to obtain a membrane material without added crosslinking agent; the chitosan solution was prepared by using an aqueous acetic acid solution with a mass fraction of 1% to prepare a chitosan solution with a mass fraction of 10%.
[0085] The membrane material with modified crosslinking agent, the membrane material with unmodified crosslinking agent and the membrane material without crosslinking agent were cut into 15mm×30mm pieces respectively as test membrane samples, and the mechanical properties of each were measured by electronic tensile testing machine. Figure 3 shown.
[0086] Depend on Figure 3 It can be obtained that the breaking tensile displacement of the membrane material without adding cross-linking agent is 15mm, and the maximum tensile force is 33N; the breaking tensile displacement of the membrane material with adding unmodified cross-linking agent is 14mm, and the maximum tensile force is 39N; the breaking tensile displacement of the membrane material with adding modified cross-linking agent is 22mm, and the maximum tensile force is 78N; the breaking tensile displacement of the membrane material without adding cross-linking agent and the membrane material with modified cross-linking agent increased by 47%, and the maximum tensile force increased by 136%, and the mechanical properties of the membrane material with adding cross-linking agent were significantly improved.
[0087] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0088] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. An amino crosslinking agent, characterized in that The invention comprises the following components and raw materials in parts by weight: 0.5-2 parts of polyphenol compounds, 0.4-1 parts of paraformaldehyde, 0.5-2 parts of magnesium chloride, 1-4 parts of triethylamine, 20-40 parts of organic solvents, 40-60 parts of hydrochloric acid; The mixture of the polyphenol compound, paraformaldehyde, magnesium chloride, triethylamine and organic solvent is reacted at a temperature of 55-80° C. for 6-12 hours, then heating is stopped, and the hydrochloric acid is added and stirred to obtain a reaction solution; the reaction solution is concentrated, separated and dried to obtain the amino cross-linking agent.
2. The amino crosslinking agent according to claim 1, characterized in that The invention comprises the following components and raw materials in parts by weight: 1 part of polyphenol compound, 0.8 parts of paraformaldehyde, 1.5 parts of magnesium chloride, 3 parts of triethylamine, 30 parts of organic solvent, 50 parts of hydrochloric acid.
3. The amino crosslinking agent according to any one of claims 1 to 2, characterized in that The polyphenol compound is any one of tea polyphenols or tannic acid; And / or, the organic solvent is any one of tetrahydrofuran, acetone or acetonitrile.
4. A cross-linked biomass amino material, characterized in that: The invention comprises an amino material and the amino cross-linking agent according to any one of claims 1 to 3.
5. The cross-linked biomass amino material according to claim 4, characterized in that: The weight ratio of the amino material to the amino cross-linking agent is 80-120:
1.
6. The cross-linked biomass amino material according to claim 4, characterized in that: The amino material is any one of a gelatin solution and a chitosan solution, wherein the mass fraction of gelatin contained in the gelatin solution is 8-12%, and the mass fraction of chitosan contained in the chitosan solution is 8-12%.
7. A method for preparing the cross-linked biomass amino material according to any one of claims 4 to 6, characterized in that: The amino cross-linking agent is mixed with the amino material, and the mixture is allowed to stand and dried to obtain the cross-linked biomass amino material.
8. The method for preparing the cross-linked biomass amino material according to claim 7, characterized in that: The standing time is 8-16h; And / or, the drying temperature is 45-55° C. and the drying time is 20-26 hours.