Oxidized homogeneity starch as well as preparation method and application thereof
Through the self-polarized ceramic-enhanced ozone micro-nano bubble technology, the problem of insufficient uniformity of oxidized starch is solved, efficient starch oxidation is achieved, the performance of gel products and environmentally friendly production processes are improved, and the starch gel is expanded. Application scope.
Patent Information
- Application Number
- CN202411057157.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
AI Technical Summary
In the existing preparation methods for oxidized starch, the oxidation uniformity is insufficient, resulting in low reaction uniformity of gel products, poor strength and viscosity performance, and the wastewater generated by chemical oxidant treatment is difficult to treat, which affects the wide range of environment and application fields.
The self-polarized ceramic reinforced ozone micro-nano bubble technology is adopted to distribute the self-polarized ceramic porous tower plate in the oxidation equipment and the ozone micro-nano bubble water circulation to form a strengthened oxidation system, promote the uniform oxidation of starch, improve the oxidation uniformity and efficiency.
The uniform oxidation of starch is achieved, the hardness, adhesion and cohesion of gel products are improved, the crystallization degree of starch particles is reduced, the process is simplified, the production cost is reduced, and the application of oxidized starch in the gel field is expanded. potential.
Smart Images

Figure BDA0004976772780000081 
Figure HDA0004976772790000011 
Figure HDA0004976772790000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of oxidized starch preparation, and in particular relates to oxidized uniform starch and a preparation method and application thereof. Background Art
[0002] Oxidized starch is a widely used modified starch that can be prepared by reacting natural starch with an oxidant. Oxidized starch has good solubility, stability, high transparency, film-forming property, emulsification and adhesion, and is widely used in 3D printing, papermaking and spinning raw materials, emulsions and other fields. The chemical oxidants used to prepare oxidized starch mainly include sodium hypochlorite, gaseous chlorine, bromine, sodium bromide, periodate, permanganate and hydrogen peroxide. However, the use of chemical reagents to produce oxidized starch will lead to the generation of a large amount of toxic wastewater, which is rich in inorganic anions (such as Cl - Br - ) and rich nutrients, its chemical oxygen demand, biological oxygen demand and solid suspended matter content are high, so it is difficult to treat, and it belongs to a type of industrial wastewater with great treatment challenges. In actual treatment, starch wastewater has a large output, complex chemical composition, and high oxygen demand. Direct discharge into natural water bodies will cause great harm to the human body and the environment, limiting its practical application in food, medicine and other fields.
[0003] Compared with the expensive H2O2, O3 is widely used in starch modification due to its strong oxidation ability, simple preparation method, and environmental friendliness. Compared with O3 dissolved in water, ozone micro-nano bubble technology has been widely used in sewage treatment and organic matter degradation due to its fast mass transfer rate, long residence time, and high gas solubility. In addition, the rupture of micro-nano bubbles will produce local shear stress of 100 to 5000 bar and transient local hot spots of 2300 to 4600 K, thereby generating highly active ·OH to achieve starch oxidation. For example, patent CN 116943868 A discloses a method for preparing ozone nano-bubble oxidized starch and its application in copper-sulfur separation. In this method, a mixture of starch and water and ozone are passed into a nano-bubble generator, and ozone nano-bubbles are used to oxidize the starch to prepare ozone nano-bubble oxidized starch. This method only involves the oxidation of starch, but does not involve any description of the oxidation uniformity of starch. The oxidized starch obtained by this method is prone to low reaction uniformity and deterioration of gel properties such as strength, viscosity and water retention during the application of gel products.
[0004] Although the research on the high oxidation rate of ozone micro-nano bubbles is relatively extensive, there are fewer studies on the oxidation rate and oxidation uniformity of ozone micro-nano bubbles. In addition, due to the differences in the activity of the oxidation sites of starch molecules and the mass transfer resistance during the oxidation process, it is still challenging to achieve the uniformity of oxidized starch. On the one hand, the difference in the activity of the oxidation sites is mainly due to the competition effect between the C2 and C6 sites in the glucose unit; on the other hand, the mass transfer resistance is mainly due to the supramolecular structural characteristics of the semi-crystalline starch, which makes it difficult for the reaction reagents to contact it, thereby limiting the penetration of chemical reagents into the starch molecules. In order to overcome these limitations, an effective strategy is to select heterogeneous catalysts to catalyze the adsorption-decomposition process of O3. However, common metal-based catalysts require a lot of chemical modification and element doping to maintain strong O3 catalytic activity. Therefore, the development of materials to enhance the O3 adsorption-decomposition process and improve the uniformity of starch oxidation has become a problem that needs to be overcome urgently.
[0005] Self-polarized ceramic is a kind of ceramic with the composition of KCa3AlCa3Si4O 16 (hexagonal system, L6 symmetry, P63 space group) spontaneously polarized material. The non-centrosymmetric structure of the self-polarized ceramic and the high intrinsic electric dipole moment contributed by the K(1) polyhedron give it a high spontaneous polarization rate (0.23μC / cm 2 ) and far-infrared emissivity (0.95), pyroelectric and piezoelectric properties. Under the action of local electric field and far-infrared rays, self-polarized ceramics can activate and destroy large (H2O) n Intermolecular hydrogen bonds in the clusters generate small molecular cluster water, which strengthens the mass transfer process of the chemical reaction. In addition, studies have shown that the electric field can enhance the adsorption and decomposition of O3 on the surface of the material and the O3-liquid phase mass transfer process. Therefore, the present invention uses self-polarized ceramic to enhance the ozone micro-nano bubble technology to enhance the adsorption and decomposition of O3, overcome the mass transfer resistance of starch oxidation, accelerate the cleavage of starch glycosidic bonds, the depolymerization of starch molecular chains, and the increase of short-range ordered structures, which can expose more C2, C3 and C6 active sites on the starch molecular chains, thereby improving the degree and efficiency of oxidation and achieving uniform oxidation of starch. Achieving uniform oxidation of starch helps to more effectively improve the contact state and reactivity of the reaction reagents and starch macromolecules, thereby changing the physical and chemical properties of starch such as water solubility, gel strength and viscosity, thereby further expanding the requirements of oxidized starch in the preparation of starch gels. Summary of the invention
[0006] In view of the above problems, the present invention provides an oxidized uniform starch and a preparation method and application thereof. Under the strengthening effect of self-polarized ceramic, an enhanced oxidation system is formed with ozone micro-nano bubble circulating water, so that the oxidation process of starch is more uniform. The obtained oxidized uniform starch is applied to starch gel products, and its application properties such as adhesion, hardness and cohesion are excellent.
[0007] The present invention is achieved through the following technical solutions:
[0008] A method for preparing oxidized uniform starch comprises the following steps: distributing self-polarized ceramic porous tower plates in an oxidation device, then circulating ozone micro-nano bubble water into the oxidation device, and putting starch into the oxidation device to place the starch solution in a liquid phase enhanced oxidation system, and obtaining oxidized uniform starch after the oxidation is completed.
[0009] Furthermore, the preparation method of the self-polarized ceramic porous tower plate is: mixing the self-polarized ceramic clay with water, pressing and then opening holes, and then calcining at a high temperature of 900-1100° C. at a rate of 3-5° C. / min for 1.5-2h in an air atmosphere to obtain a self-polarized ceramic porous tower plate.
[0010] Furthermore, the mass ratio of the self-polarized clay to water is 10g:2-3mL.
[0011] Furthermore, the opening rate of the self-polarized ceramic porous tower plate is 3-5%; the aperture of the sieve used for the opening is 2-3 mm.
[0012] Furthermore, the number of self-polarized ceramic porous trays in the oxidation device is 2 to 4.
[0013] Furthermore, the mass concentration of the starch solution is 4-10%.
[0014] Furthermore, the ozone micro-nano bubble water is circulated for 0.2 to 2 hours, with a flow rate of 0.3 to 3 L / min and an O3 content of 30 to 60 mg / L.
[0015] An oxidized uniform starch prepared by the preparation method as described above.
[0016] Furthermore, the mass fraction of carboxyl groups in the oxidized uniform starch is 0.02-0.60%.
[0017] A use of the oxidized uniform starch as described above in starch gel products.
[0018] The application of the oxidized uniform starch of the present invention in the starch gel product is specifically as follows: the oxidized uniform starch and water are mixed at a mass ratio of 10g:15-20mL, stirred evenly and then transferred to a mold and sealed, heated under hydrothermal conditions of 90-100°C for 25-30min, demolded after the heating is completed, and naturally cooled to room temperature to obtain an oxidized uniform starch gel.
[0019] The self-polarized clay used in the present invention is derived from the plastic blank in the patent application of the same applicant (publication number CN 113800888A, the invention name is a kind of ecological functional Nixing pottery and its preparation method), and the plastic blank is prepared by raw material mixing, solid phase mechanical activation, wet mechanical activation, filter pressing dehydration, vacuum mud kneading and three-stage biomineralization in the patent application (CN 113800888A). The present invention mixes the self-polarized clay, i.e., the plastic blank, with water, opens holes after pressing, and then performs high-temperature calcination in an air atmosphere to obtain the self-polarized ceramic porous tower plate used in the present invention.
[0020] The preparation principle of the oxidized uniform starch of the present invention is as follows: the self-polarized ceramic porous trays are distributed in the oxidation equipment, and then ozone micro-nano bubble water is circulated into the oxidation equipment, and starch is put into the oxidation equipment to make the starch solution in a liquid phase enhanced oxidation system. After the oxidation is completed, oxidized uniform starch is obtained. In this process:
[0021] (1) The self-polarized ceramic porous tower plate is formed by mixing self-polarized ceramic clay with water, pressing with a porous template and calcining at high temperature, and has a certain open porosity. The self-polarized ceramic porous tower plate can increase the contact area between the ozone micro-nano bubble water and the self-polarized ceramic, increase the gas content in the area above the liquid phase of the bubble tower in the oxidation equipment, increase the average gas content and the proportion of tiny bubbles, so that the starch solution is in a uniform liquid phase oxidation system for oxidation.
[0022] (2) Self-polarized ceramics can reduce the hydrogen bonding of water molecules under the combined action of surface electric field and far infrared rays, produce small molecular cluster water and make it more active. The rupture of ozone micro-nano bubble water induces the piezoelectric and pyroelectric effects of self-polarized ceramics, reduces the electric dipole moment, and strengthens the adsorption-decomposition of O3 on the surface of self-polarized ceramics to generate OH.
[0023] (3) OH acts on the double helix structure of branched starch with the help of small molecular cluster water, degrading the side chains with higher polymerization degree into short-chain molecules with lower polymerization degree, increasing the oxidation degree of the crystalline structure, and making the oxidized groups evenly distributed along the starch molecular chain. The cleavage of starch glycosidic bonds, depolymerization of starch molecular chains, and increase in short-range ordered structures further expose more C2, C3, and C6 active sites on the starch molecular chains, weakening the competitive effect of C2 and C6, reducing the formation of hemiacetal byproducts, and improving the uniformity of oxidation sites.
[0024] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0025] 1. The present invention forms an enhanced oxidation system with ozone micro-nano bubble circulating water under the strengthening effect of self-polarized ceramic, so that the oxidation process of starch is more uniform. The oxidation process occurs in the side chains with higher polymerization degree of branched starch in the crystalline region, which reduces the proportion of side chains with high polymerization degree and increases the proportion of side chains with lower polymerization degree. This method reduces the degree of crystallization of starch granules, promotes the oxidation process to penetrate into the starch molecules, and the oxidized groups are evenly distributed on the straight chain and branched starch molecules, thereby improving the reaction efficiency and reaction uniformity. The oxidation sites of the oxidized uniformity starch of the present invention are distributed at the C2, C3, and C6 sites, which weakens the competitive effect of C2 and C6, reduces the formation of hemiacetal by-products, and makes the distribution of starch oxidation active sites more uniform.
[0026] 2. The self-polarized ceramic used in the present invention ionizes water molecules under the combined action of the surface electric field and far infrared rays, reduces the hydrogen bonding effect, produces small molecular cluster water and makes it more active. Compared with macromolecular water, small molecular cluster water has a tighter binding force with starch molecules, which shortens the relaxation time. Small molecular cluster water penetrates into the double helix structure of the crystallization area in the form of tightly bound water, enhances the mass transfer diffusion process, and improves the uniformity of the distribution of oxidized groups along the starch double helix structure.
[0027] 3. The mass fraction of the oxidized uniform starch of the present invention is 0.02-0.60%, and the cross-linking structure between the starch and water molecules is highly uniform, so that the hardness, chewiness, elasticity and other properties of the gel product are improved, and the stable structure of the starch gel is enhanced. The starch gel product made from the oxidized uniform starch has a hardness of 5.64-13.42N, an adhesion of 0.86-1.18N·mm, a cohesion of 0.88-1.72%, an elasticity of 3.18-7.56mm, and a chewiness of 15.62-39.80mJ. The adhesion and cohesion of the starch gel product are improved, and the product has good application performance.
[0028] 4. The preparation method of the oxidized uniform starch of the present invention is an ozone micro-nano bubble oxidation method, which has simple process, convenient operation, mild conditions, and low production cost. In the preparation method, the raw material of the self-polarized ceramic porous tower plate used is healthy and environmentally friendly self-polarized ceramic clay, and the tower plate preparation process only requires opening holes and high-temperature calcination. The operation is simple, no external reagents are required, and the preparation cost is low. It has good practical application value for the preparation of oxidized uniform starch. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The present invention is a process flow chart for preparing oxidized uniform starch.
[0030] Figure 2 The XRD patterns of native starch and oxidized uniform starch prepared in Example 1.
[0031] Figure 3 The oxidized uniform starch prepared by the original starch and Example 1 1 H NMR and 13 C NMR spectrum.
[0032] Figure 4 The ozone micro-nano bubble water before and after starch oxidation in Example 1 17 O NMR spectrum.
[0033] Figure 5 LF-NMR graph of ozone micro-nano bubble water before and after starch oxidation in Example 1.
[0034] Figure 6 This is a viscosity performance analysis chart of native starch and oxidized uniform starch prepared in Example 1.
[0035] Figure 7 These are SEM images of native starch and oxidized uniform starch prepared in Example 1. DETAILED DESCRIPTION
[0036] The present invention is further described in detail below by way of examples. These examples are only used to illustrate the present invention and do not limit the protection scope of the present invention.
[0037] The process flow chart of the present invention for preparing oxidized uniform starch is as follows: Figure 1 As shown in the process flow chart, the oxidation equipment used mainly includes an ozone generator, a micro-nano bubble generator, a bubbling tower and an ozone tail gas treatment device.
[0038] The ozone generator is connected to the micro-nano bubble generator to circulate ozone micro-nano bubble water into the bubbling tower, and the ozone micro-nano bubble water enters the bubbling tower through the water inlet and circulates to the micro-nano bubble generator through the water outlet of the bubbling tower. The water inlet is a pressurized water inlet, which can push the starch particles on the side wall or bottom of the bubbling tower when the ozone micro-nano bubble water is introduced to ensure that the starch material is fully mixed in the solution.
[0039] The bubbling tower is equipped with self-polarized ceramic porous plates, which can increase the contact area between ozone micro-nano bubble water and self-polarized ceramic, increase the gas content and micro-bubble ratio in the upper liquid phase of the bubbling tower, and form a liquid phase enhanced oxidation system with ozone micro-nano bubble circulating water under the strengthening effect of self-polarized ceramic, making the oxidation process of starch more uniform. The filter on the top of the bubbling tower can capture starch particles to ensure that they are always oxidized inside the bubbling tower.
[0040] The gas escaping from the bubbling tower is treated by an ozone tail gas treatment device.
[0041] When preparing oxidized uniform starch, ozone micro-nano bubble water is first circulated into the bubbling tower, and then starch is fed into the bubbling tower from the feed inlet for oxidation reaction. After the oxidation is completed, the oxidized starch solution is received from the discharge port, filtered and dried to obtain oxidized uniform starch.
[0042] Example 1
[0043] Preparation of oxidized uniform starch:
[0044] 50.0g of self-polarized ceramic clay was mixed with 10.0mL of water, and after pressing, a 3mm sieve was used to make holes, and then calcined at 1050°C for 1.5h (heating rate 5°C / min) in an air atmosphere to obtain a self-polarized ceramic porous tower plate with an opening rate of 5%. Two self-polarized ceramic porous tower plates were distributed in the oxidation device. After the oxidation device was prepared, ozone micro-nano bubble water was stirred and circulated at room temperature for 2h, with a flow rate of 3L / min and an O3 content of 60mg / L, and 200.0g of cassava starch was put into the oxidation device to make the starch solution mass concentration of 10%. After the oxidation was completed, the oxidized starch solution was centrifuged, dehydrated and filtered, and dried at 40°C for 8h to obtain oxidized uniform starch.
[0045] Through detection and analysis, the mass fraction of carboxyl groups in the oxidized uniform starch prepared in this embodiment is 0.60%.
[0046] Example 2
[0047] Preparation of oxidized uniform starch:
[0048] 50.0g of self-polarized clay was mixed with 15.0mL of water, and after pressing, a 2mm sieve was used to make holes, and then calcined at 1100°C for 2.0h (heating rate 5°C / min) in an air atmosphere to obtain a self-polarized ceramic porous tower plate with an opening rate of 3%. Three self-polarized ceramic porous tower plates were distributed in an oxidation device. After the oxidation device was prepared, ozone micro-nano bubble water was stirred and circulated at room temperature for 1h, with a flow rate of 2L / min and an O3 content of 50mg / L. 200.0g of cassava starch was added to the oxidation device to make the starch solution mass concentration of 8%. After the oxidation was completed, the oxidized starch solution was centrifuged, dehydrated and filtered, and dried at 40°C for 8h to obtain oxidized uniform starch.
[0049] Through detection and analysis, the mass fraction of carboxyl groups in the oxidized uniform starch prepared in this embodiment is 0.42%.
[0050] Example 3
[0051] Preparation of oxidized uniform starch:
[0052] 50.0g of self-polarized ceramic clay was mixed with 10.0mL of water, and after pressing, a 3mm sieve was used to make holes, and then calcined at 900°C for 1.5h (heating rate 3°C / min) in an air atmosphere to obtain a self-polarized ceramic porous tower plate with an opening rate of 4%. Four self-polarized ceramic porous tower plates were distributed in the oxidation device, and after the oxidation device was prepared, ozone micro-nano bubble water was stirred and circulated at room temperature for 0.5h, with a flow rate of 1L / min and an O3 content of 40mg / L, and 200.0g of cassava starch was thrown into the oxidation device to make the starch solution mass concentration of 6%. After the oxidation was completed, the oxidized starch solution was centrifuged, dehydrated and filtered, and dried at 40°C for 8h to obtain oxidized uniform starch.
[0053] Through detection and analysis, the mass fraction of carboxyl groups in the oxidized uniform starch prepared in this embodiment is 0.21%.
[0054] Example 4
[0055] Preparation of oxidized uniform starch:
[0056] 50.0g of self-polarized ceramic clay was mixed with 12.0mL of water, and after pressing, a 3mm sieve was used to make holes, and then calcined at 1000°C for 2h (heating rate 5°C / min) in an air atmosphere to obtain a self-polarized ceramic porous tower plate with an opening rate of 5%. Two self-polarized ceramic porous tower plates were distributed in an oxidation device, and after the oxidation device was prepared, ozone micro-nano bubble water was stirred and circulated at room temperature for 0.2h, with a flow rate of 0.3L / min and an O3 content of 30mg / L, and 200.0g of cassava starch was thrown into the oxidation device to make the starch solution mass concentration of 4%. After the oxidation was completed, the oxidized starch solution was centrifuged, dehydrated and filtered, and dried at 40°C for 8h to obtain oxidized uniform starch.
[0057] Through detection and analysis, the mass fraction of carboxyl in the oxidized uniform starch prepared in this embodiment is 0.02%.
[0058] Material Characterization Analysis
[0059] The cassava native starch and the oxidized uniform starch prepared in Example 1 of the present invention were characterized and analyzed.
[0060] (I) X-ray diffraction (XRD) analysis
[0061] X-ray diffraction (XRD) was used to characterize the uniformity of the distribution of oxidized groups of cassava native starch and the oxidized uniform starch prepared in Example 1. The characterization results are as follows: Figure 2 As shown. Figure 2It can be seen that the native starch is type A crystal, with main peaks at 15°, 17°, 17.8° and 23°, and small peaks at 11.25°, 19° and 26°. The relative crystallinity of the oxidized uniform starch decreased significantly, the small peaks at 11.25°, 19° and 26° disappeared, and the main peak intensity at 17° and 17.8° weakened, forming a gentle broad peak. This shows that the method of Example 1 can oxidize the crystalline region of starch, promote the oxidation process to penetrate into the starch molecules, and the oxidized groups are evenly distributed on the linear and branched starch molecules, thereby improving the reaction efficiency and reaction uniformity.
[0062] (II) H NMR spectroscopy ( 1 H NMR) and carbon nuclear magnetic resonance spectroscopy ( 13 C NMR analysis
[0063] Using H NMR spectroscopy ( 1 H NMR) and carbon nuclear magnetic resonance spectroscopy ( 13 C NMR) was used to characterize the uniformity of oxidation sites of cassava native starch and the oxidized uniform starch prepared in Example 1. The characterization results are as follows: Figure 3 shown. Figure 3 In the left figure, the native starch is at 5.50, 5.40 and 4.58 ppm. 1 The H NMR chemical shifts can be assigned to OH2, OH3 and OH6, respectively. The hydroxyl peaks at 5.50, 5.40 and 4.58 ppm of oxidized starch disappeared / weakened, indicating that the oxidation active sites were evenly distributed at C2, C3 and C6 sites. Figure 3 In the right figure, the native starch is at 163.53ppm 13 A new peak appeared in the C NMR chemical shift, which was attributed to the characteristic peak of the carboxyl group at the C6 site, indicating that the C6 site was oxidized to generate a carboxyl group. The preferential oxidation reaction at the C6 site can reduce the formation of intramolecular / intermolecular hemiacetal structures and improve the oxidation uniformity of the starch hydroxyl site.
[0064] (III) Nuclear Magnetic Resonance Oxygen Spectroscopy ( 17 O NMR) analysis
[0065] Nuclear magnetic resonance oxygen spectroscopy ( 17 O NMR was used to characterize and analyze the ozone micro-nano bubble water before and after the oxidation of cassava starch in Example 1. The characterization results are as follows: Figure 4 shown. Figure 4In the experiment, before starch oxidation (i.e., original starch), ozone micro-nano bubble water is macromolecular water with a half-peak width of 128.27Hz, and after starch oxidation (i.e., oxidized uniform starch), ozone micro-nano bubble water is small molecular cluster water with a half-peak width of 49.90Hz. This shows that self-polarized ceramic can ionize water molecules under the combined action of surface electric field and far infrared rays, reduce hydrogen bonding, reduce the size of small molecular cluster water, and make small molecular cluster water more active.
[0066] (IV) Low-field nuclear magnetic resonance (LF-NMR) analysis
[0067] Low field nuclear magnetic resonance (LF-NMR) was used to characterize and analyze the ozone micro-nano bubble water before and after cassava starch oxidation in Example 1. The characterization results are as follows: Figure 5 shown. Figure 5 In the experiment, before starch oxidation (i.e., native starch), ozone micro-nano bubble water is macromolecular water, and after starch oxidation (i.e., oxidized uniform starch), ozone micro-nano bubble water is small molecular cluster water. 21 / 2b (0.01~3.0ms) and T 22 (4.0~90ms) represent tightly bound water and weakly bound water respectively. There is a peak of weakly bound water (90~1000ms) in the native starch-water system, but weakly bound water is difficult to detect accurately, so this part of water is removed during analysis.
[0068] Compared with native starch, the T 21 / 2b The relaxation time is decreasing, and the relaxation time is shortened from 0.30ms to 0.25ms. This is because compared with large molecular water clusters, small molecular cluster water has a tighter binding force with starch molecules, and small molecular cluster water penetrates into the double helix structure of the crystallization area in the form of tightly bound water, which enhances the mass transfer diffusion process and improves the uniformity of the distribution of oxidized groups along the starch double helix structure.
[0069] (V) Viscosity performance analysis
[0070] The viscosity properties of cassava starch and the oxidized uniform starch prepared in Example 1 were analyzed. The results are as follows: Figure 6 As shown. Compared with native cassava starch, the gelatinization temperature of oxidized uniform starch is reduced from 71.2℃ to 61.3℃. This is because the small molecular clusters generated under the self-polarization strengthening effect can better penetrate the double helix structure of the crystalline area of starch (the size of the A-type crystalline area>1nm), which deepens the depolymerization of the side chains of amylopectin. After the uniformity of the distribution of oxidized groups along the starch molecular chain is improved, the short-range structure of the starch molecules in the crystalline area is further increased, which ultimately reduces the gelatinization temperature of oxidized uniform starch.
[0071] Compared with native cassava starch, the viscosity of oxidized uniform starch decreased. This is because the self-polarization treatment promoted the oxidation of -OH and the partial cleavage of glycosidic bonds, increased the content of hydrophilic groups (-COOH) and broken branched starch fragments, reduced the hydrogen bonds between oxidized starch molecules, weakened the structure of starch granules, and reduced the shear resistance of starch granules.
[0072] (VI) Scanning electron microscopy (SEM) analysis
[0073] The macroscopic morphology of the cassava starch and the oxidized uniform starch prepared in Example 1 were characterized and analyzed using a scanning electron microscope (SEM). Figure 7 As shown. Figure 7 It can be seen that the original cassava starch has a full granular structure, and the surface of the oxidized starch collapses due to uniform oxidation. This is mainly because the piezoelectric effect of the self-polarized pottery can promote the bursting of ozone micro-nano bubbles, continuously adsorb and decompose ozone to produce active oxygen components that act on starch particles, thereby enhancing the depth of oxidation mass transfer diffusion into the starch interior.
[0074] Application Example 1
[0075] Take 10.0 g of the oxidized uniform starch prepared in Example 1 into a 100 mL beaker, add 17.5 mL of water and stir evenly, then transfer to a 2×2×2 cm mold and seal it, heat it under hydrothermal conditions at 100° C. for 30 min, demold it after heating, and naturally cool it to room temperature to obtain an oxidized uniform starch gel.
[0076] Application Example 2
[0077] The difference between Application Example 2 and Application Example 1 is that the oxidized uniform starch prepared in Example 2 is used in Application Example 2, and the other preparation conditions are the same as those in Application Example 1.
[0078] Application Example 3
[0079] The difference between Application Example 3 and Application Example 1 is that the oxidized uniform starch prepared in Example 3 is used in Application Example 3, and the other preparation conditions are the same as those in Application Example 1.
[0080] Application Example 4
[0081] The difference between Application Example 4 and Application Example 1 is that the oxidized uniform starch prepared in Example 4 is used in Application Example 4, and the other preparation conditions are the same as those in Application Example 1.
[0082] The oxidized uniform starch gels in Application Examples 1-4 were tested for texture properties and compared with native cassava starch gels (prepared in the same manner as in Application Example 1). The test results are shown in Table 1 below.
[0083]
[0084] As can be seen from Table 1, the hardness, adhesion, cohesion, elasticity and chewiness of the oxidized uniform starch gel in Application Examples 1-4 are higher than those of the cassava native starch gel. As for the elasticity index of the starch gel, the elasticity of the oxidized uniform starch gel is increased by more than 15.64% compared with the cassava native starch gel. The mass fraction of the carboxyl group of the oxidized uniform starch in Examples 1-4 is 0.02-0.60%, and the cross-linking structure between the oxidized uniform starch and the water molecules is highly uniform, so that the hardness, chewiness, elasticity and other properties of the gel product are improved, and the stable structure of the starch gel is enhanced.
[0085] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing oxidized uniform starch, It is characterized in that The following steps are involved: The self-polarized ceramic porous tower plates are distributed in the oxidation equipment, and then ozone micro-nano bubble water is circulated into the oxidation equipment, and starch is put into the oxidation equipment to make the starch solution in a liquid phase enhanced oxidation system. After the oxidation is completed, oxidized uniform starch is obtained.
2. The method for preparing oxidized uniform starch according to claim 1, It is characterized in that The preparation method of the self-polarized ceramic porous tower plate is as follows: mixing the self-polarized ceramic clay with water, pressing and then opening holes, and then calcining at a high temperature of 900-1100° C. at a rate of 3-5° C. / min for 1.5-2 hours in an air atmosphere to obtain the self-polarized ceramic porous tower plate.
3. The method for preparing oxidized uniform starch according to claim 2, It is characterized in that The mass ratio of the self-polarized clay to water is 10 g:2-3 mL.
4. The method for preparing oxidized uniform starch according to claim 2, It is characterized in that The opening rate of the self-polarized ceramic porous tower plate is 3-5%; the aperture of the sieve used for the opening is 2-3mm.
5. The method for preparing oxidized uniform starch according to claim 1, It is characterized in that The number of the self-polarized ceramic porous tower plates in the oxidation device is 2 to 4.
6. The method for preparing oxidized uniform starch according to claim 1, It is characterized in that The mass concentration of the starch solution is 4-10%.
7. The method for preparing oxidized uniform starch according to claim 1, It is characterized in that The ozone micro-nano bubble water is circulated for 0.2 to 2 hours at a flow rate of 0.3 to 3 L / min. 3 The content is 30-60 mg / L.
8. An oxidized uniform starch obtained by the preparation method according to any one of claims 1 to 7.
9. The oxidized uniform starch according to claim 8, It is characterized in that The mass fraction of carboxyl groups in the oxidized uniform starch is 0.02-0.60%.
10. Use of the oxidized uniform starch according to claim 8 in starch gel products.