Fluorine alcohol modified acrylate type polymer surfactant as well as preparation method and application thereof

Through the polymerization of fluoroalcohol and maleic anhydride ring opening and acrylate monomer, fluoroalcohol modified acrylate surfactants are prepared, which solves the high preparation cost and environmental pollution of existing fluoromodified acrylate surfactants. The problem of this has achieved efficient and environmentally friendly surfactant performance.

CN118955815APending Publication Date: 2024-11-15AFCONA CHEM HAIMEN +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411197237.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing fluorine-modified acrylate surfactants are cost-effective and have high environmental pollution. Long-chain perfluoroalkyl groups may be decomposed into potential carcinogens PFOA and PFOS, affecting environmental and biological safety.

Method used

Fluoroethanol and maleic anhydride ring-opening reaction to form fluorocarbon-containing monomers, and polymerize with hydrophobic and hydrophilic acrylate monomers in the presence of free radical initiators and solvents to prepare fluoroalcohol-modified acrylate type high Molecular surfactant, control reaction conditions to improve efficiency and environmental protection.

Benefits of technology

It has achieved low-cost and efficient preparation of fluoroalcohol modified acrylate surfactants, which have good compatibility, foam inhibition and anti-pore properties, and is more environmentally friendly, and its performance is not inferior to that of traditional fluoro modified acrylate surfactants. agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955815A_ABST
    Figure CN118955815A_ABST
Patent Text Reader

Abstract

The invention provides a fluoroalcohol modified acrylate type polymer surfactant as well as a preparation method and application thereof. The preparation method comprises the following steps: (1) performing ring-opening reaction on fluorocarbon alcohol and maleic anhydride at 70-130 DEG C to obtain a fluorine-containing monomer; and (2) carrying out polymerization reaction on the fluorine-containing monomer in the step (1), a hydrophobic acrylate monomer and a hydrophilic acrylate monomer in the presence of a free radical initiator and a solvent to obtain the fluorine alcohol modified acrylate type high-molecular surfactant. The fluoroalcohol modified acrylate type surfactant has the performance equivalent to or even better than that of an existing fluorine modified acrylate type surfactant, and meanwhile, the preparation cost is low, and the fluoroalcohol modified acrylate type surfactant is greener and more environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer surfactants, and particularly relates to a fluoroalcohol-modified acrylate polymer surfactant, a preparation method thereof and an application thereof. Background Art

[0002] With the development of social economy, people's living standards are getting higher and higher. The coatings and coatings industry has become closer and closer to the lives of everyone on the earth and has become an indispensable part of people's lives. The improvement of people's awareness of healthy living has also put forward higher and higher requirements for the development of coatings, so that modern coatings must develop in the direction of high performance, high efficiency, high environmental protection and high-end decorative effects.

[0003] As a special additive, polymer surfactants play an important role in improving the performance of coatings. Their main functions include improving the wettability, dispersibility, leveling of coatings and reducing the surface tension of coatings. These characteristics are essential for improving the comprehensive performance of coatings. By adding polymer surfactants, the uniformity and stability of coatings can be significantly improved, thereby improving the overall quality and use effect of coatings.

[0004] Surfactant molecules are usually composed of long-chain lipophilic groups and polar hydrophilic groups distributed at both ends of the molecule. The non-polar groups of ordinary surfactants are hydrocarbon chains, that is, hydrocarbon surfactants, which have poor performance. The H atoms on the CH chain in hydrocarbon surfactants are replaced by F atoms, becoming fluorocarbon surfactants with higher surface activity than hydrocarbon surfactants. Hydrocarbon chains in which all hydrogen atoms are replaced by fluorine are called perfluorinated surfactants, and those in which some are replaced by fluorine are called partial fluorinated surfactants. Most of the fluorinated surfactants currently used are perfluorinated surfactants.

[0005] At present, the fluorocarbon surfactants at home and abroad are mainly acrylate copolymers with long-chain perfluoroalkyl groups, most of which are perfluoroalkyl groups with 6 to 10 carbon atoms, and the performance is best when the carbon atoms of the perfluoro chain segment are 8. However, the research report of the US Environmental Protection Agency pointed out that long-chain perfluoroalkyl groups (with 8 or more carbon atoms) may decompose or degrade into PFOA (perfluorooctanoic acid and its salts) or PFOS (perfluorooctane sulfonyl compounds). PFOA and PFOS do not decompose in the environment and in organisms, have high bioaccumulation, and may be potential carcinogens.

[0006] In recent years, there have been reports that attempt to reduce the length of the perfluoroalkyl chain to replace the long-chain perfluoroalkyl in the original structure. For example, in patent US2005027063, acrylates with perfluoroalkyl groups of 3 to 4 carbon atoms are used and multiple curing points are introduced into the copolymer; in patent US2006205864, the fluorine-containing monomer is an α-substituted acrylate, and the number of carbon atoms in the perfluoroalkyl group is 1 to 6. Although the harm of PFOA or PFOS to the environment and organisms is avoided, the receding dynamic contact angle is correspondingly reduced, the surface energy is increased, and the performance of the resulting copolymer is reduced.

[0007] Fluorinated acrylate is an important monomer for synthesizing fluorinated acrylate polymers. Although the introduction of fluoroalkyl chains can make acrylic surfactants have excellent properties such as high surface activity, high heat stability, high chemical stability, and both water and oil repellency, the synthesis conditions of fluorinated modified acrylic acid are usually harsh and the yield is low, which leads to high preparation costs of existing fluorinated modified acrylate surfactants and relatively large pollution to the environment. For example, patent CN1927894A discloses a method for synthesizing octafluoropentyl acrylate, which uses concentrated sulfuric acid as a catalyst and toluene as a solvent and a water-carrying reagent. Water is continuously separated during the reaction process. The reaction yield of this method is low, and it is difficult to recover the solvent after the reaction is completed, and a large amount of waste acid and waste liquid is generated. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a fluorocarbon surfactant with good comprehensive performance, low preparation cost and green environmental protection.

[0009] In order to solve the above technical problems, a technical solution adopted by the present invention is:

[0010] The first aspect of the present invention provides a method for preparing a fluoroalcohol-modified acrylate-type polymer surfactant, the preparation method comprising the following steps:

[0011] (1) subjecting fluorocarbon alcohol and maleic anhydride to a ring-opening reaction at 70° C. to 130° C. to obtain a fluorine-containing monomer;

[0012] (2) polymerizing the fluorine-containing monomer of step (1) with a hydrophobic acrylate monomer and a hydrophilic acrylate monomer in the presence of a free radical initiator and a solvent to obtain the fluoroalcohol-modified acrylate polymer surfactant.

[0013] In an embodiment of the present invention, the fluorocarbon alcohol in step (1) is a monohydric alcohol.

[0014] In an embodiment of the present invention, the molar ratio of the fluorocarbon alcohol to the maleic anhydride is (0.95-1.05):1.

[0015] A fluorine-containing monomer containing a reactive carbon-carbon unsaturated double bond and a -COOH group is obtained through step (1).

[0016] According to some embodiments of the present invention, the fluorocarbon alcohol in step (1) is one or more of octafluoropentanol (1H, 1H, 5H-octafluoropentan-1-ol), 1H, 1H, 2H, 2H-perfluorohexan-1-ol, 1H, 1H, 2H, 2H-perfluorooctanol, perfluorodecanol, 1H, 1H, 11H-perfluoro-1-undecanol, and 1, 1, 2, 2-tetrahydroperfluorododecanol. Taking octafluoropentanol as an example, the reaction formula is as follows:

[0017]

[0018] According to some embodiments of the present invention, the reaction temperature in step (1) is 90° C. to 110° C. When the reaction temperature is too low, the reaction speed is slow; when the reaction temperature is too high, the reaction speed is too fast, maleic anhydride is easy to sublime, difficult to control, and the polymer content increases.

[0019] In an embodiment of the present invention, the reaction in step (1) is carried out under the protection of an inert gas.

[0020] In an embodiment of the present invention, the hydrophobic propionate monomer in step (2) is one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, n-butyl methacrylate, isooctyl acrylate, lauryl acrylate, octadecyl acrylate, and isobornyl acrylate.

[0021] In an embodiment of the present invention, the hydrophilic acrylate monomer in step (2) is one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and polyoxyethylene acrylate.

[0022] In an embodiment of the present invention, the free radical initiator in step (2) is 2,2'-azobisisobutyronitrile, potassium persulfate, 2,2'-azobis(amidinopropane) dihydrochloride and an alkyl hydroperoxide, such as benzoyl peroxide, tert-butyl perbenzoate, hydroxyisopropyl peroxide, terpene hydroperoxide.

[0023] In an embodiment of the present invention, the solvent in step (2) is one or more organic solvents selected from the group consisting of aromatic hydrocarbons, esters, alcohols, ketones and chlorinated hydrocarbons.

[0024] According to some specific embodiments of the present invention, the solvent in step (2) is one or more of toluene, xylene, methyl isobutyl ketone, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, n-butanol, tert-butanol, and chloroform.

[0025] In an embodiment of the present invention, in the step (2), the molar ratio of the fluorine-containing monomer, the hydrophobic acrylate and the hydrophilic acrylate is 1:(10-20):(1-5).

[0026] Furthermore, the molar ratio of the fluorine-containing monomer, the hydrophobic acrylate and the hydrophilic acrylate is 1:(12-18):(1-5).

[0027] Furthermore, the molar ratio of the fluorine-containing monomer, the hydrophobic acrylate and the hydrophilic acrylate is 1:(14-16):(2-4).

[0028] In an embodiment of the present invention, the reaction in step (2) is carried out under the protection of an inert gas.

[0029] The second aspect of the present invention provides a fluoroalcohol-modified acrylate-type polymer surfactant prepared by the above-mentioned preparation method.

[0030] The third aspect of the present invention provides the use of the fluoroalcohol-modified acrylate polymer surfactant prepared by the above preparation method in solvent-based baking varnish, polyurethane coating, epoxy resin coating or alkyd resin coating.

[0031] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0032] The fluoroalcohol modified acrylate surfactant of the present invention can effectively reduce the surface tension of the organic coating system, has good compatibility and strong anti-foaming property; more specifically, it can effectively improve the leveling property of the coating, help the wetting of the substrate, does not affect the interlayer adhesion and the recoatability, has good anti-shrinkage and orange peel elimination performance, and its comprehensive performance is not inferior to the existing fluorine-modified acrylate surfactant. The new fluoroalcohol modified acrylate monomer used in the fluoroalcohol modified acrylate surfactant of the present invention can not only effectively participate in the free radical polymerization of acrylic acid, but also its preparation method is more efficient and environmentally friendly than the preparation method of the traditional fluorine-modified acrylate monomer. Therefore, the fluoroalcohol modified acrylate surfactant of the present invention has a low preparation cost and is more environmentally friendly while having comparable or even better performance than the existing fluorine-modified acrylate surfactant. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the infrared spectrum of Example 1 when it is not reacted;

[0034] Figure 2 This is the infrared spectrum of Example 1 when the reaction is complete;

[0035] Figure 3The defoaming effect diagram of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 in the hydroxy acrylic resin 1753 in the initial stage (10 minutes of shaking and then standing for 10 minutes);

[0036] Figure 4 The defoaming effect diagram of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 in the hydroxy acrylic resin 1753 in the middle and middle stages (10 minutes of shaking and then standing for 20 minutes);

[0037] Figure 5 The defoaming effect diagram of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 in hydroxy acrylic resin 1753 at the end stage (shaking for 10 minutes and then standing for 30 minutes);

[0038] Figure 6 The figures are the foam suppression effect of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 in hydroxy acrylic resin 1753;

[0039] Figure 7 The effect diagram of the clarity of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 in hydroxy acrylic resin 1753;

[0040] Figure 8 It is a diagram showing the leveling effect of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1, and Comparative Example 2 in hydroxy acrylic resin 1753;

[0041] Fig. 9 The anti-shrinkage effect diagram of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 in hydroxy acrylic resin 1753;

[0042] Fig.10 The effect diagram of measuring the dyne value of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1 and Comparative Example 2 in hydroxy acrylic resin 1753;

[0043] Fig.11 This is a diagram showing the effect of measuring the dyne value of the surfactants of Example 1, Example 2, Example 3, Example 4, Example 5, Comparative Example 1, and Comparative Example 2 in the low-hydroxy acrylic resin YK304. DETAILED DESCRIPTION

[0044] The present invention is further described below in conjunction with the examples. However, the present invention is not limited to the following examples. The implementation conditions used in the examples can be further adjusted according to the different requirements of specific use, and the implementation conditions not specified are conventional conditions in the industry. The technical features involved in each embodiment of the present invention can be combined with each other as long as they do not conflict with each other.

[0045] Unless otherwise specified, the raw materials used in the following examples and comparative examples were purchased from commercial channels.

[0046] Example 1

[0047] This embodiment provides a fluoroalcohol-modified acrylate-type polymer surfactant, and its preparation method is as follows:

[0048] (1) Preparation of fluorine-containing monomer: 80 g of octafluoropentanol (1H,1H,5H-octafluoropentan-1-ol) and 42.24 g of maleic anhydride were placed in a 250 ml four-necked flask, and the temperature was slowly raised to 100°C-110°C under the protection of inert gas N2. The temperature rise process took about 2 hours. After 1 hour of heating, 20 g of octafluoropentanol was added and the temperature was kept at 100°C-110°C for 4 hours to ensure that the anhydride was completely ring-opened. The acid value Av was 170.1 and the iodine value I was 76.9. The product was a fluorine-containing monomer with a slightly light yellow transparent appearance.

[0049] (2) 31.5 g of n-butyl acrylate, 31.5 g of isooctyl acrylate, 12 g of polyoxyethylene acrylate (Mn=540), 15 g of the fluorine-containing monomer of step (1), 9 g of hydroxyethyl methacrylate, and 3.96 g of 2,2'-azobisisobutylcyanide were mixed uniformly in a 200 ml beaker; 1 / 5 (by mass) of the mixed monomers in the beaker and 46.5 g of propylene glycol methyl ether acetate were placed in a 250 ml four-necked flask, and then heated to 75°C to 80°C under the protection of inert gas N2. After keeping warm for half an hour, the remaining 4 / 5 of the mixed monomers were added to a constant temperature funnel at 75°C to 80°C and dripped into the four-necked flask over about 3.5 hours. After the addition was completed, the temperature was kept at 75°C to 80°C for 1 hour, and 0.6 g of 2,2'-azobisisobutylcyanide, continue to keep at 75℃~80℃ for 3 hours; the solid content of the obtained reaction solution is 69.1%, and infrared measurement shows that the double bond peak has completely disappeared ( Figure 1 When there is no reaction in the middle, the double bond peaks are 1638 and 812; Figure 2 When the reaction is finished, the two peaks 1638 and 812 completely disappear), indicating that the reaction has been completely completed. The propylene glycol methyl ether acetate is removed by vacuum rotary evaporation to obtain a fluoroalcohol-modified acrylate polymer surfactant, which has a light yellow transparent liquid appearance.

[0050] Example 2

[0051] This embodiment provides another fluoroalcohol-modified acrylate-type polymer surfactant, the preparation method of which is as follows:

[0052] (1) Preparation of fluorine-containing monomer: same as step (1) in Example 1.

[0053] (2) 31.5 g of n-butyl acrylate, 31.5 g of isooctyl acrylate, 12 g of polyoxyethylene acrylate (Mn=540), 15 g of the fluorine-containing monomer of step (1), 9 g of hydroxyethyl methacrylate, and 4 g of benzoyl peroxide were mixed uniformly in a 200 ml beaker; 1 / 5 (by mass) of the mixed monomers in the beaker and 46.5 g of propylene glycol methyl ether acetate were placed in a 250 ml four-necked flask, and then heated to between 100° C. and 105° C. under the protection of inert gas N2. After keeping warm for half an hour, the remaining 4 g of propylene glycol methyl ether acetate were added to the flask. / 5 of the mixed monomers are placed in a constant temperature dropping funnel at 100°C-105°C, and the mixture is dropped into a four-necked flask over about 3.5 hours. After the dropping is completed, the temperature is kept at 100°C-105°C for 1 hour, 0.65g of benzoyl peroxide is added, and the temperature is kept at 100°C-105°C for another 3 hours. The solid content of the obtained reaction solution is 69.15%, and infrared measurement shows that the double bond peak has completely disappeared, indicating that the reaction has been completely completed. Propylene glycol methyl ether acetate is removed by reduced pressure rotary evaporation to obtain a fluoroalcohol-modified acrylate polymer surfactant, which has the appearance of a light yellow transparent liquid.

[0054] Example 3

[0055] This embodiment provides another fluoroalcohol-modified acrylate-type polymer surfactant, the preparation method of which is as follows:

[0056] (1) Preparation of fluorine-containing monomer: same as step (1) in Example 1.

[0057] (2) 31.5 g of n-butyl acrylate, 31.5 g of isooctyl acrylate, 12 g of polyoxyethylene acrylate (Mn=540), 15 g of the fluorine-containing monomer of step (1), 9 g of hydroxyethyl methacrylate, and 4 g of tert-butyl perbenzoate were mixed uniformly in a 200 ml beaker; 1 / 5 (by mass) of the mixed monomers in the beaker and 46.5 g of propylene glycol methyl ether acetate were placed in a 250 ml four-necked flask, and then heated to between 130° C. and 135° C. under the protection of inert gas N2. After keeping warm for half an hour, the remaining 4 g of tert-butyl perbenzoate were added to the flask. / 5 of the mixed monomers were placed in a constant temperature dropping funnel at 130°C-135°C, and the mixture was dropped into a four-necked flask over about 3.5 hours. After the dropping was completed, the temperature was kept at 100°C-105°C for 1 hour, 0.65g of tert-butyl perbenzoate was added, and the temperature was kept at 130°C-135°C for 3 hours. The solid content of the obtained reaction solution was 69.13%, and infrared measurement showed that the double bond peak had completely disappeared, indicating that the reaction had been completely completed. Propylene glycol methyl ether acetate was removed by reduced pressure rotary evaporation to obtain a fluoroalcohol-modified acrylate type polymer surfactant, which had the appearance of a light yellow transparent liquid.

[0058] Example 4

[0059] This embodiment provides another fluoroalcohol-modified acrylate-type polymer surfactant, the preparation method of which is as follows:

[0060] (1) Preparation of fluorine-containing monomer: 70 g of perfluorohexanol (1H, 1H, 2H, 2H-perfluorohexan-1-ol) and 37.12 g of maleic anhydride were placed in a 250 ml four-necked flask, and the temperature was slowly raised to 100° C. to 110° C. under the protection of inert gas N2. The temperature rise process took about 2 hours. After 1 hour of heating, 30 g of perfluorohexanol was added and the temperature was kept at 100° C. to 110° C. for 4 hours to ensure that the anhydride was completely ring-opened. The acid value Av was 155.1 and the iodine value I was 70.09. The product was a fluorine-containing monomer with a slightly light yellow transparent appearance.

[0061] (2) 31.5 g of n-butyl acrylate, 31.5 g of isooctyl acrylate, 12 g of polyoxyethylene acrylate (Mn=540), 15 g of the fluorine-containing monomer of step (1), 9 g of hydroxyethyl methacrylate, and 3.96 g of 2,2'-azobisisobutylcyanide were mixed uniformly in a 200 ml beaker; 1 / 5 (by mass) of the mixed monomers in the beaker and 46.5 g of propylene glycol methyl ether acetate were placed in a 250 ml four-necked flask, and then heated to 75°C to 80°C under the protection of inert gas N2. After keeping warm for half an hour, the remaining 4 / 5 of the mixed monomers were added to a constant temperature funnel at 75°C to 80°C and dripped into the four-necked flask over about 4 hours. After the addition was completed, the temperature was kept at 75°C to 80°C for 1 hour, and 0.6 g of 2,2'-azobisisobutylcyanide, continue to keep warm at 75℃~80℃ for 3 hours; the solid content of the obtained reaction solution is 69.11%, and infrared measurement shows that the double bond peak has completely disappeared, indicating that the reaction has been completely completed, and propylene glycol methyl ether acetate is removed by vacuum rotary evaporation to obtain a fluoroalcohol-modified acrylate type polymer surfactant, which has the appearance of a light yellow transparent liquid.

[0062] Example 5

[0063] This embodiment provides another fluoroalcohol-modified acrylate-type polymer surfactant, the preparation method of which is as follows:

[0064] (1) Preparation of fluorine-containing monomer: 65 g of perfluorooctanol (1H, 1H, 2H, 2H-perfluorooctanol) and 26.92 g of maleic anhydride were placed in a 250 ml four-necked flask, and the temperature was slowly raised to 100°C-110°C under the protection of inert gas N2. The temperature rise process took about 2 hours. After 1 hour of heating, 35 g of perfluorooctanol was added and the temperature was kept at 100°C-110°C for 4 hours to ensure that the anhydride was completely ring-opened. The acid value Av was 121.39 and the iodine value I was 54.89. The product was a fluorine-containing monomer with a slightly light yellow transparent appearance.

[0065] (2) 31.5 g of n-butyl acrylate, 31.5 g of isooctyl acrylate, 12 g of polyoxyethylene acrylate (Mn=540), 15 g of the fluorine-containing monomer of step (1), 9 g of hydroxyethyl methacrylate, and 3.96 g of 2,2'-azobisisobutylcyanide were mixed uniformly in a 200 ml beaker; 1 / 5 (by mass) of the mixed monomers in the beaker and 46.5 g of propylene glycol methyl ether acetate were placed in a 250 ml four-necked flask, and then heated to 75°C to 80°C under the protection of inert gas N2. After keeping warm for half an hour, the remaining 4 / 5 of the mixed monomers were added to a constant temperature funnel at 75°C to 80°C and dripped into the four-necked flask over about 4 hours. After the addition was completed, the temperature was kept at 75°C to 80°C for 1 hour, and 0.6 g of 2,2'-azobisisobutylcyanide, continue to keep warm at 75℃~80℃ for 3 hours; the solid content of the obtained reaction solution is 69.08%, and infrared measurement shows that the double bond peak has completely disappeared, indicating that the reaction has been completely completed, and propylene glycol methyl ether acetate is removed by vacuum rotary evaporation to obtain a fluoroalcohol-modified acrylate type polymer surfactant, which has the appearance of a light yellow transparent liquid.

[0066] Comparative Example 1

[0067] This comparative example provides a fluorine-modified acrylate type polymer surfactant, and its preparation method is as follows:

[0068] 22.5g of n-butyl acrylate, 22.5g of isooctyl acrylate, 30g of polyoxyethylene acrylate (Mn=540), 15g of octafluoropentyl acrylate, 9g of hydroxyethyl methacrylate, and 3.96g of 2,2'-azobisisobutylcyanide were mixed evenly in a 200ml beaker; 1 / 5 (by mass) of the mixed monomers in the above beaker and 46.5g of propylene glycol methyl ether acetate were put into a 250ml four-necked flask, and then heated to 75°C to 80°C under the protection of inert gas N2. After keeping warm for half an hour, the remaining 4 / 5 of the mixed monomers were added to a constant temperature funnel at 75°C to 80°C, and dripped into the four-necked flask over about 4 hours. After the addition was completed, the temperature was kept at 75°C to 80°C for 1 hour, and 0.6g of 2,2'-azobisisobutylcyanide, continue to keep warm at 75℃~80℃ for 3 hours; the solid content of the obtained reaction solution is 69.12%, and infrared measurement shows that the double bond peak has completely disappeared, indicating that the reaction has been completely completed, and propylene glycol methyl ether acetate is removed by vacuum rotary evaporation to obtain a fluorine-modified acrylate type polymer surfactant, which has the appearance of a light yellow transparent liquid.

[0069] Comparative Example 2

[0070] This comparative example provides a fluorine-modified acrylate type polymer surfactant, and its preparation method is as follows:

[0071] 22.5g of n-butyl acrylate, 22.5g of isooctyl acrylate, 30g of polyoxyethylene acrylate (Mn=540), 15g of hexafluorobutyl acrylate, 9g of hydroxyethyl methacrylate, and 3.96g of 2,2'-azobisisobutylcyanide were mixed evenly in a 200ml beaker; 1 / 5 of the mixed monomers (by mass) in the beaker and 46.44g of propylene glycol methyl ether acetate were placed in a 250ml four-necked flask, and then heated to 75°C to 80°C under the protection of inert gas N2. After keeping warm for half an hour, the remaining 4 / 5 of the mixed monomers were added to a constant temperature funnel at 75°C to 80°C, and dripped into the four-necked flask over about 4 hours. After the addition was completed, the temperature was kept at 75°C to 80°C for 1 hour, and 0.6g of 2,2'-azobisisobutylcyanide, continue to keep warm at 75℃~80℃ for 3 hours; the solid content of the obtained reaction solution is 69.1%, and infrared measurement shows that the double bond peak has completely disappeared, indicating that the reaction has been completely completed, and propylene glycol methyl ether acetate is removed by vacuum rotary evaporation to obtain a fluorine-modified acrylate type polymer surfactant, which has the appearance of a light yellow transparent liquid.

[0072] Performance Testing:

[0073] 1. Defoaming, anti-foaming and shrinkage performance test

[0074] The high molecular surfactant prepared in the above-mentioned embodiments and comparative examples was added into different systems at an addition amount of 0.3 wt %, and after being sealed and shaken in a shaker for 10 min, it was taken out for observation and its application performance was evaluated.

[0075] Anti-foaming performance: The liquid level before shaking is recorded as H0, and the final height of the bubble after shaking is recorded as liquid level H1. The liquid level change rate (%) = (H1-H0) / H0*100%. The anti-foaming ability is evaluated based on the liquid level change rate.

[0076] The standard for grading the foam suppression ability is as follows: 1: 0-1%; 2: 1-5%; 3: 5-15%; 4: 15-30%; 5: >30%; +: better; -: worse; the smaller the value, the better the foam suppression effect, and the larger the value, the worse the foam suppression effect.

[0077] Bubble breaking performance: After the above-mentioned shaken test sample is left to stand for 1 hour, the bubble condition is observed and graded. The classification standard is: A: no bubbles at all; B: almost no bubbles; C: few bubbles, only some bubbles in the upper half of the liquid layer; D: many bubbles and not very tight; E: many bubbles, no liquid is visible; +: better; - worse.

[0078] Clarity evaluation: Level 1: clear and transparent; Level 2: turbid light, foggy, translucent, and you can see the object on the opposite side through the bottle; Level 3: Severely turbid light, but still partially translucent; Level 4: Turbid, looking from top to bottom, you can slightly see the bottom of the bottle; Level 5: Turbid and completely opaque.

[0079] Leveling and anti-crater test:

[0080] The varnish containing the test sample (colored by adding the color paste of the corresponding system grinding for the convenience of photography) was scraped onto the polyester sheet using a wire-wound rod with a wet film thickness of 60 μm.

[0081] The varnish formula is:

[0082] Resin: A4203: solvent: pigment = 15:4:21:10 (mass ratio);

[0083] Note: The solvent used for hydroxy acrylic acid 1753 is XYL:PMA=1:1;

[0084] The solvent used for polyester 325 is XYL:BAC:n-butanol=4:1:1;

[0085] The solvent used for low hydroxyl acrylic acid YK304 is PMA:BAC=1:1;

[0086] The solvent used for epoxy 128 is AGE (C12-14 alkyl glycidyl ether);

[0087] A4203: Efcona Polymers Co., Ltd.

[0088] Pigment: Blue pigment, BASF AG.

[0089] The leveling evaluation criteria are as follows: Level 1: The coating is smooth, continuous and flat; Level 2: The coating is relatively smooth and continuous, but there will be some unevenness upon closer inspection; Level 3: The coating surface is not very smooth and flat; Level 4: The coating has orange grain and orange peel phenomenon; Level 5: The coating has shrinkage holes.

[0090] The criteria for shrinkage evaluation are: yes or no.

[0091] The test system includes: hydroxyl acrylic resin 1753, low hydroxyl acrylic resin YK304, polyester resin 325, and epoxy resin 128.

[0092] Figures 3 to 9 The figure shows the comparison of the foam suppression, defoaming, leveling, crater shrinkage and clarity of the surfactants in the above-mentioned embodiments and comparative examples in hydroxy acrylic resin 1753.

[0093] The evaluation results of foam suppression, defoaming, leveling, crater shrinkage and clarity of the surfactants of the above-mentioned embodiments and comparative examples in different test systems are shown in Table 1.

[0094] Table 1

[0095]

[0096]

[0097] Table 1 shows that the defoaming, foam suppression and pore shrinkage performance of the fluorine-modified acrylate polymer surfactants in the above examples are comparable to or even better than those of the fluorine-modified acrylate polymer surfactants in the comparative examples.

[0098] 2. Dyne value test

[0099] Weigh 0.15 g of each of the polymer surfactants prepared in the above embodiments and comparative examples, respectively, and place them in different shaking bottles, then add 50 g of varnish (1753 varnish or YK304 varnish) respectively, shake for 10 minutes, let it stand, and after there are no bubbles in the bottle, add curing agent (1753 varnish: Bayer N3390 = 5:1, YK304 varnish: CAB = 4:1.5) and stir evenly, and apply it on the tinplate with a 60 μm wire winding rod. After it is completely dried, doodle on the paint film with a dyne pen.

[0100] Preparation of 1753 varnish: hydroxy acrylic resin 1753: XYL: PMA = 8:1:1 (mass ratio).

[0101] Preparation of YK304 varnish: low hydroxyl acrylic resin YK304: PMA: BAC = 8:1:1 (mass ratio)

[0102] The dyne value test results are shown in Table 2.

[0103] Table 2

[0104]

[0105] Table 2 shows that the dyne value of the varnish with the fluorine-modified acrylate polymer surfactant of each of the above examples is slightly larger than the dyne value of the varnish with the fluorine-modified acrylate polymer surfactant of each of the above comparative examples, indicating that the varnishes with the addition of Examples 1 to 5 are more easily wetted.

[0106] 3. Water contact angle test

[0107] Weigh 0.15g of the surfactants of the above embodiments and comparative examples and place them in different oscillation bottles, respectively, add 50g of varnish (1753 varnish or YK304 varnish), shake for 10min, let stand, and after there are no bubbles in the bottle, add curing agent (1753 varnish: Bayer N3390 = 5:1, YK304 varnish: CAB = 4:1.5) and stir evenly, add solvent (the solvent of 1753 is XYL:PMA = 1:1; the solvent of YK304 is PMA:BAC = 1:1) and adjust to an appropriate viscosity (viscosity is 25mPa·s) and then spray it on a tinplate. After completely drying, the water contact angle is tested with a contact angle meter. The blank is a varnish without adding a surfactant. The test results are shown in Table 3.

[0108] Table 3

[0109]

[0110] As can be seen from Table 3, in 1753, the water contact angles of Examples 1 to 5 are significantly smaller than those of Comparative Examples 1 and 2, and slightly smaller than the blank, so it is easier to infiltrate after adding Examples 1 to 5; while in YK304, although the water contact angles of Examples 1 to 5 are larger than those of the blank, they are still smaller than those of Comparative Examples 1 and 2, which shows that the wetting ability of Examples 1 to 5 is better than that of Comparative Examples 1 and 2.

[0111] The above test results show that the new fluoroalcohol-modified acrylate surfactants prepared in Examples 1 to 5 have better performance than the acrylate surfactants prepared from the traditional acrylic fluorine monomers in Comparative Examples 1 and 2. The new fluoroalcohol-modified acrylate monomers used in the polymerization reaction in Examples 1 to 5 can not only effectively participate in the free radical polymerization of acrylic acid, but also the preparation method thereof is more efficient and environmentally friendly than the preparation method of the traditional fluorine-modified acrylate monomer. Therefore, the fluoroalcohol-modified acrylate surfactants in Examples 1 to 5 have comparable or even better performance than the existing fluorine-modified acrylate surfactants, while having low preparation costs and being more environmentally friendly.

[0112] The above detailed description of the present invention is intended to enable persons familiar with the art to understand the contents of the present invention and implement them. It does not limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a fluoroalcohol-modified acrylate-type polymer surfactant, characterized in that: The preparation method comprises the following steps: (1) subjecting fluorocarbon alcohol and maleic anhydride to a ring-opening reaction at 70° C. to 130° C. to obtain a fluorine-containing monomer; (2) polymerizing the fluorine-containing monomer of step (1) with a hydrophobic acrylate monomer and a hydrophilic acrylate monomer in the presence of a free radical initiator and a solvent to obtain the fluoroalcohol-modified acrylate polymer surfactant.

2. The preparation method according to claim 1, characterized in that: The fluorocarbon alcohol in step (1) is a monohydric alcohol, and the molar ratio of the fluorocarbon alcohol to the maleic anhydride is (0.95-1.05):

1.

3. The preparation method according to claim 2, characterized in that: The fluorocarbon alcohol in step (1) is one or more of 1H,1H,5H-octafluoropentan-1-ol, 1H,1H,2H,2H-perfluorohexan-1-ol, 1H,1H,2H,2H-perfluorooctanol, perfluorodecanol, 1H,1H,11H-perfluoro-1-undecanol, and 1,1,2,2-tetrahydroperfluorododecanol.

4. The preparation method according to claim 1, characterized in that: The reaction temperature in step (1) is 90° C. to 110° C.; and / or the reaction in step (1) is carried out under the protection of an inert gas.

5. The preparation method according to claim 1, characterized in that: The hydrophobic propionate monomer in step (2) is one or more of methyl acrylate, ethyl acrylate, n-butyl acrylate, n-butyl methacrylate, isooctyl acrylate, lauryl acrylate, octadecyl acrylate, and isobornyl acrylate; And / or, the hydrophilic acrylate monomer in step (2) is one or more of hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, and polyoxyethylene acrylate; And / or, the free radical initiator in step (2) is 2,2'-azobisisobutyronitrile, potassium persulfate, 2,2'-azobis(amidinopropane) dihydrochloride and alkyl hydroperoxide, such as benzoyl peroxide, tert-butyl perbenzoate, hydroxyisopropylbenzene peroxide, terpene hydroperoxide; And / or, the solvent in step (2) is one or more of aromatic hydrocarbons, esters, alcohols, ketones or chlorinated hydrocarbon organic solvents.

6. The preparation method according to claim 5, characterized in that: The solvent in step (2) is one or more of toluene, xylene, methyl isobutyl ketone, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, n-butanol, tert-butanol, and chloroform.

7. The preparation method according to claim 1, characterized in that: In the step (2), the molar ratio of the fluorine-containing monomer, the hydrophobic acrylate and the hydrophilic acrylate is 1:(10-20):(1-5).

8. The preparation method according to claim 1, characterized in that: The reaction in step (2) is carried out under the protection of an inert gas.

9. A fluoroalcohol-modified acrylate-type polymer surfactant prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the fluoroalcohol-modified acrylate polymer surfactant prepared by the preparation method according to any one of claims 1 to 8 in solvent-based baking varnish, polyurethane coating, epoxy resin coating or alkyd resin coating.