Lignin-coated nano titanium-zinc compound with anti-aging function and preparation method of lignin-coated nano titanium-zinc compound
By shearing, stirring and drying lignin, nano zinc oxide and nano titanium dioxide in the torque rheometer, solid phase preparation of lignin-encapsulated nano titanium-zinc composite is achieved, and the cumbersome preparation process in the prior art is solved. The high cost problem significantly improves the material's UV aging resistance.
Patent Information
- Application Number
- CN202411200137.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the preparation process of lignin-encapsulated nano-titanium-zinc composites is complicated and requires a solvent system, which leads to high costs and complex steps, and lacks a simple solid-phase solvent-free preparation method.
After drying, lignin, nano zinc oxide and nano titanium dioxide are mixed, and a shear reaction is carried out in a torque rheometer. The lignin-encapsulated nano titanium-zinc composite is obtained through shear stirring, which simplifies the preparation process and realizes the Solid phase preparation.
The preparation process is simplified, the cost is reduced, the operation ease is improved, and the anti-UV aging performance of polymer materials is significantly improved.
Smart Images

Figure CN118956009A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of anti-aging materials, and in particular relates to a lignin-wrapped nano titanium-zinc composite with anti-aging function and a preparation method thereof. Background Art
[0002] Under the influence of environmental factors such as ultraviolet rays, temperature and oxygen, many plastic products used outdoors are facing the problem of gradual aging. Among them, light aging caused by ultraviolet rays is an important component of polymer material aging. Ultraviolet radiation can be divided into four bands according to wavelength: long-wave UVA (315-400nm), medium-wave UVB (280-315nm) and short-wave UVC (100-280nm), of which UVC and most UVB (98%) are absorbed by the ozone layer. Therefore, in order to improve the anti-UV aging performance of polymer plastics, ultraviolet absorbers that can absorb UVA are often used as additives to polymer plastics, such as benzophenone and benzotriazole ultraviolet absorbers. However, small molecules of ultraviolet absorbers have poor stability in polymer systems, and the improvement of the anti-aging performance of plastic products is limited.
[0003] Nano zinc oxide can absorb UVA with a wavelength of 320-400nm, and nano titanium dioxide has a stronger ultraviolet absorption capacity in the band of 330-350nm, so the two can be used in combination to comprehensively improve the material's anti-UV aging performance. In addition, lignin can capture free radicals generated by nanomaterials and polymer materials during the aging process, further improving the anti-aging performance, and lignin and polymer systems often have better compatibility, which is convenient for improving stable dispersibility. Therefore, lignin-nano titanium dioxide-nano zinc oxide composites are expected to significantly improve the anti-aging performance of polymer systems. Patent CN117510995A introduces a method for preparing purified lignin-coated nano zinc oxide / titanium dioxide modifiers, which can be used to improve the UV aging resistance of asphalt, but the method is completed in a solvent system and requires steps such as reflux, filtration, washing, and drying. The preparation process is relatively cumbersome and the cost is high.
[0004] Up to now, there is no simple method to achieve solid-phase, solvent-free preparation of lignin-coated nano-titanium-zinc composites. Summary of the invention
[0005] The present invention aims to solve the key problem that the current preparation process of lignin-coated nano-titanium-zinc composite is complicated, and provides a lignin-coated nano-titanium-zinc composite with a simple preparation method, easy operation and industrialization and a preparation method thereof.
[0006] The method for preparing the lignin-wrapped nano-titanium-zinc composite of the present invention comprises the following steps:
[0007] (1) First, lignin, nano zinc oxide, and nano titanium dioxide are dried;
[0008] (2) Then, lignin, nano zinc oxide, and nano titanium dioxide are mixed and added to a torque rheometer for shear reaction, and the sample after the reaction is taken out to obtain a lignin-wrapped nano titanium zinc composite.
[0009] Preferably, the lignin is dealkalized lignin.
[0010] Preferably, the particle size of the nano zinc oxide is 10-40 nanometers.
[0011] Preferably, the nano titanium dioxide has a rutile phase particle size of 10-50 nanometers.
[0012] Preferably, the drying is carried out at a temperature of 60-80° C. and for a time of 6-10 hours.
[0013] Preferably, the mass ratio of lignin: nano zinc oxide: nano titanium dioxide is 1:(3-10):(3-10).
[0014] Preferably, the shear reaction in the torque rheometer has a rotation speed of 50-150 rpm, a time of 10-25 min, and a temperature of 170-200°C.
[0015] Preferably, the shear reaction in the torque rheometer is performed at a temperature of 170° C., a rotation speed of 80-100 rpm, and shear stirring for 25 min.
[0016] The present invention also provides a lignin-wrapped nano-titanium-zinc composite prepared according to the above preparation method.
[0017] The present invention also provides the anti-aging application of the lignin-wrapped nano-titanium-zinc composite in polyethylene film.
[0018] The present invention also provides the use of the lignin-wrapped nano titanium-zinc complex as an anti-aging aid in polyethylene film.
[0019] The methods in the prior art are mostly completed in a solvent system, requiring at least filtering, washing, drying and other steps, and the preparation process is relatively cumbersome and costly. The present invention realizes the solid phase, solvent-free preparation of lignin-coated nano-titanium-zinc composites, which is easy to operate and reduces costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a transmission electron microscope image of the lignin-wrapped nano-titanium-zinc composite prepared in Example 1.
[0021] Figure 2 This is a transmission electron microscope image of the lignin-wrapped nano-titanium-zinc composite prepared in Example 2. DETAILED DESCRIPTION
[0022] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0023] The lignin in this embodiment is dealkalized lignin, the particle size of nano zinc oxide is 10-40 nanometers, and the particle size of nano titanium dioxide is rutile phase, and the particle size is 10-50 nanometers.
[0024] Embodiment 1:
[0025] First, lignin, nano zinc oxide, and nano titanium dioxide were placed in an oven and dried at 80°C for 10 hours. Then, lignin, nano zinc oxide, and nano titanium dioxide were mixed in a mass ratio of 1:10:10 and added to a torque rheometer, the temperature was set to 170°C, the speed was set to 80 rpm, and shear stirring was performed for 25 minutes. Finally, the reacted sample was taken out to obtain a nano titanium zinc composite wrapped with lignin.
[0026] Transmission electron microscopy characterization: The lignin-coated nano-titanium-zinc composite prepared in this example was ultrasonically dispersed in an ethanol solution, and then a sample was taken to measure the surface morphology using a high-resolution transmission electron microscope. The results showed that lignin was successfully coated on the surface of the nano-titanium-zinc composite. Figure 1 shown.
[0027] Characterization of anti-aging performance: A polyethylene plastic film with anti-aging effect, the components of which are calculated by weight: 100 parts of polyethylene resin, 1 part of lignin-wrapped nano-titanium-zinc composite. According to the ratio, the components are uniformly mixed by high-speed stirring, extruded, granulated, dried, and blow-molded at a temperature of 160°C to obtain a polyethylene plastic film 1 with anti-aging effect. At the same time, according to the same method, without adding the lignin-wrapped nano-titanium-zinc composite, only polyethylene resin is used for blow molding to obtain polyethylene plastic film 0 as a control. The aging performance of the two polyethylene plastic films obtained is tested, and the test standards are: tensile strength and elongation at break are tested according to GB\T1040.3-2006 standard, and ultraviolet light aging is tested according to GB\T16422-2006 standard. The test results are shown in the following table.
[0028] performance Polyethylene plastic film1 Polyethylene plastic film0 Tensile strength, MPa 20 18 Elongation at break, % 216 168 UV aging 100h, elongation at break retention rate, % 87 77
[0029] Embodiment 2:
[0030] First, lignin, nano zinc oxide, and nano titanium dioxide were placed in an oven at 80°C for 10 hours. Then, lignin, nano zinc oxide, and nano titanium dioxide were mixed in a mass ratio of 2:10:10 and added to a torque rheometer. The temperature was set to 170°C, the speed was set to 100 rpm, and the shear stirring was performed for 25 minutes. Finally, the reacted sample was taken out to obtain a nano titanium zinc composite wrapped with lignin.
[0031] Transmission electron microscopy characterization: The lignin-coated nano-titanium-zinc composite prepared in this example was ultrasonically dispersed in an ethanol solution, and then a sample was taken to measure the surface morphology using a high-resolution transmission electron microscope. The results showed that lignin was successfully coated on the surface of the nano-titanium-zinc composite. Figure 2 shown.
[0032] Characterization of anti-aging performance: A polyethylene plastic film with anti-aging effect, the components of which are calculated by weight: 100 parts of polyethylene resin, 1 part of lignin-wrapped nano-titanium-zinc composite. According to the ratio, the components are mixed evenly by high-speed stirring, extruded, granulated, dried, and blow-molded at a temperature of 160°C to obtain a polyethylene plastic film 2 with anti-aging effect. At the same time, according to the same method, without adding the lignin-wrapped nano-titanium-zinc composite, only polyethylene resin is used for blow molding to obtain polyethylene plastic film 0 as a control. The aging performance of the two polyethylene plastic films obtained is tested, and the test standards are: tensile strength and elongation at break are tested according to GB\T1040.3-2006 standard, and ultraviolet light aging is tested according to GB\T16422-2006 standard. The test results are shown in the following table.
[0033] performance Polyethylene plastic film2 Polyethylene plastic film0 Tensile strength, MPa 20 18 Elongation at break, % 220 168 UV aging 100h, elongation at break retention rate, % 89 77
[0034] Comparative Example 1:
[0035] First, lignin, nano zinc oxide, and nano titanium dioxide were placed in an oven and dried at 80° C. for 10 hours. Then, lignin, nano zinc oxide, and nano titanium dioxide were added into a high-speed mixer in a mass ratio of 1:10:10 and stirred to obtain a mixture.
[0036] Characterization of anti-aging performance: A polyethylene plastic film, the components of which are calculated by weight are as follows: 100 parts of polyethylene resin and 1 part of the above mixture. According to the ratio, the components are mixed evenly by high-speed stirring, extruded, granulated, dried, and blow-molded at a temperature of 160°C to obtain a polyethylene plastic film 3. At the same time, according to the same method, without adding the mixture, only polyethylene resin is used for blow molding to obtain a polyethylene plastic film 0 as a control. The aging performance of the obtained two polyethylene plastic films is tested, and the test standards are: tensile strength and elongation at break are tested according to GB\T1040.3-2006 standard, and ultraviolet light aging is tested according to GB\T16422-2006 standard. The test results are shown in the following table.
[0037]
[0038]
Claims
1. A method for preparing a lignin-coated nano-titanium-zinc composite, characterized in that: The following steps are involved: (1) First, lignin, nano zinc oxide, and nano titanium dioxide are dried; (2) Then, lignin, nano zinc oxide, and nano titanium dioxide are mixed and added to a torque rheometer for shear reaction, and the sample after the reaction is taken out to obtain a lignin-wrapped nano titanium zinc composite.
2. The preparation method according to claim 1, characterized in that: The lignin is dealkalized lignin.
3. The preparation method according to claim 1, characterized in that: The particle size of the nano zinc oxide is 10-40 nanometers.
4. The preparation method according to claim 1, characterized in that: The nano titanium dioxide has a rutile phase particle size of 10-50 nanometers.
5. The preparation method according to claim 1, characterized in that: The drying process is carried out at a temperature of 60-80°C and a time of 6-10 hours.
6. The preparation method according to claim 1, characterized in that: The mass ratio of lignin: nano zinc oxide: nano titanium dioxide is 1:(3-10):(3-10).
7. The preparation method according to claim 1, characterized in that: The shear reaction in the torque rheometer has a rotation speed of 50-150 rpm, a time of 10-25 min, and a temperature of 170-200°C.
8. The preparation method according to claim 1, characterized in that: The shear reaction in the torque rheometer is set at a temperature of 170° C., a rotation speed of 80-100 rpm, and shear stirring for 25 minutes.
9. A lignin-coated nano-titanium-zinc composite prepared according to any preparation method of claims 1-8.
10. Application of the lignin-wrapped nano-titanium-zinc composite according to claim 9 in anti-aging applications in polyethylene films or in anti-aging aids in polyethylene films.