Novel high-temperature-resistant rubber material for automobile radiator rubber tube and preparation method of novel high-temperature-resistant rubber material
Through the new rubber material formula and preparation process, the problem of insufficient heat resistance performance of ethylene propylene ternary rubber at high temperatures was solved, and a radiator hose that can be used for a long time in high temperature environments was prepared, which extended the service life and reduced production costs.
Patent Information
- Application Number
- CN202411289636.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
AI Technical Summary
The existing ethylene propylene rubber radiator hoses have insufficient heat resistance in high temperature environments and are prone to aging and cracking, which cannot meet the demands of the automobile industry for higher temperature requirements in the future.
Using new rubber material formulas, including POR elastomers, stearic acid, magnesium oxide, anti-aging agents, reinforcement agents, plasticizers, heat-resistant additives, tackifying resins, vulcanizing agents and cross-linking additives, through plasticizing, The preparation, kneading and vulcanization of heat-resistant premixed glue can be prepared to produce hose materials with higher heat resistance.
It extends the service life of the hose and can be used for a long time in a high temperature environment of 125 to 150℃, significantly improves physical performance, reduces the engine failure rate and production costs, and enhances market competitiveness.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber materials, and in particular relates to a novel rubber material for a high-temperature resistant automobile radiator hose and a preparation method thereof. Background Art
[0002] The automobile radiator hose is a flexible pipe connecting the automobile engine and the radiator, which is mainly used to transport coolant to ensure the safe and normal operation of the engine. Since the main components of the coolant are water, ethylene glycol and preservatives, the materials used for the radiator hose must have excellent liquid resistance. As the automobile develops in the direction of lightness, efficiency and economy, the body and engine structure are becoming more and more compact, the temperature under the hood of the automobile engine is getting higher and higher, and the use temperature of the automobile hose is also more demanding. At present, the temperature around the radiator hose is kept at 120-150℃ for a long time, and the maximum temperature can reach 175℃. In China, EPDM rubber is a commonly used rubber material for automobile radiator hoses, but its long-term heat resistance temperature is 150℃, and its heat resistance at higher temperatures is greatly reduced. The prepared radiator hose will age and crack easily after long-term use, and the service life of the hose will be greatly shortened. Obviously, the traditional EPDM rubber radiator hose cannot meet the future faster development of the automobile industry. Therefore, it is a trend to develop a new type of high-temperature resistant radiator hose rubber material, which is also very necessary and has good economic benefits and practical value. Summary of the invention
[0003] The purpose of the present invention is to provide a new type of high temperature resistant rubber material for automobile radiator hose, reduce the dependence of automobile radiator hose on EPDM rubber, and at the same time increase the long-term use temperature of the radiator hose, delay thermal aging, and extend the service life, so as to better meet the use requirements of the automobile industry at present and in a certain period of time in the future.
[0004] A new type of high-temperature resistant rubber material for automobile radiator hose, whose raw materials include, by weight: 100 parts of POR elastomer, 1-1.5 parts of stearic acid, 5-8 parts of magnesium oxide, 2-4 parts of antioxidant, 80-110 parts of reinforcing agent, 20-30 parts of plasticizer, 8-12 parts of heat-resistant auxiliary agent, 3-5 parts of tackifying resin, 2.0-3.5 parts of vulcanizing agent, and 0.5-2.0 parts of cross-linking auxiliary agent.
[0005] Preferably, the raw materials include, by weight: 100 parts of POR elastomer, 1.5 parts of stearic acid, 7 parts of magnesium oxide, 3 parts of antioxidant, 110 parts of reinforcing agent, 30 parts of plasticizer, 12 parts of heat-resistant additive, 3 parts of tackifying resin, 3 parts of vulcanizing agent, and 1.0 part of cross-linking aid.
[0006] Preferably, the heat-resistant auxiliary agent is composed of modified nano cerium oxide and heat-resistant agent Luck MR-30E, and the mass fraction of modified nano cerium oxide is not less than 2 parts.
[0007] Preferably, the modified nano-cerium oxide is modified by using a titanate coupling agent.
[0008] Preferably, the reinforcing agent consists of carbon black N539 and SRF, and the mass fraction of SRF in 80 to 110 parts of the reinforcing agent is 50 to 70 parts.
[0009] Preferably, the plasticizer is any one or both of high flash point paraffin oil and liquid polybutadiene.
[0010] Preferably, the antioxidant consists of antioxidant 445 and antioxidant MB.
[0011] Preferably, the vulcanizing agent is dicumyl peroxide; and the tackifying resin is p-tert-butylphenol polyacetylene resin.
[0012] Preferably, the cross-linking auxiliary agent is any one or both of N,N-phenylbismaleimide and triallyl isocyanurate.
[0013] A method for preparing the novel high temperature resistant rubber material for automobile radiator hose according to claim 1, comprising the following steps: 1) Plasticizing: Plasticize the POR elastomer on an open mill, keep the roller distance at 1mm, and plasticize until the Mooney viscosity ML1+4 reaches 50-60; 2) Preparation of heat-resistant premixed rubber: Take 20%-30% of the POR elastomer after plastication in step 1, add it to the open mill and roll it, keep the roller distance at 0.5-1mm, the roller temperature at 40-50℃, add the heat-resistant additive, and pass the rubber material 5-6 times to obtain the premixed rubber; 3) Mixing: Mixing is performed using an open mill, and the roller temperature is maintained at 40-50°C. First, the remaining plasticized POR elastomer in step 1 is rolled, and the premixed rubber in step 2 is added. After thinning through 3 times, the roller is rolled, and the roller spacing is enlarged to 2-3 mm. Then, stearic acid, antioxidant, magnesium oxide, and tackifying resin are added in sequence. Mixing is performed for 3 minutes, and the mixture is turned left and right for 3 times. Then, a reinforcing agent and a plasticizer are added. Mixing is performed for 5 minutes, and triangle packing is performed alternately left and right for 5 times. Finally, a vulcanizing agent and a cross-linking aid are added. Mixing is performed for 2 minutes, and the mixture is thinned through 4-6 times, and the mixture is turned left and right for 3 times. Sheets are produced to obtain a mixed rubber. 4) Vulcanization: The mixed rubber is vulcanized at a temperature of 175°C and a pressure of 10±1 MPa for 10 minutes to obtain a new type of high temperature resistant rubber material for automobile radiator hose.
[0014] Advantages of the present invention: 1. The rubber material prepared by the present invention has better high temperature resistance. The rubber hose made of it can meet the working environment of 125-150°C around the radiator, and can even maintain excellent physical properties after long-term use in a working environment of 180°C, which more effectively prolongs the service life of the rubber hose; 2. The rubber material prepared by the present invention alleviates the dependence of domestic radiator hoses on EPDM rubber. At the same time, the rubber material has good coolant resistance, and the hose made from it is not easy to leak, which effectively extends the working time of the engine, reduces the production cost of the enterprise, improves the economic benefits and also enhances the market competitiveness of the enterprise. DETAILED DESCRIPTION
[0015] Example 1 A new type of high temperature resistant rubber material for automobile radiator hose, the raw materials of which include, by weight: 100 parts of POR elastomer, 1 part of stearic acid, 5 parts of magnesium oxide, 4 parts of antioxidant, 90 parts of reinforcing agent, 20 parts of plasticizer, 8 parts of heat resistant additive, 3 parts of tackifying resin, 2.5 parts of vulcanizing agent, and 2.0 parts of cross-linking additive; The antioxidant is a mixture of antioxidant 445 and antioxidant MB in a mass ratio of 5:3; The reinforcing agent is composed of carbon black N539 and SRF, wherein SRF is 60 parts; The plasticizer is high flash point paraffin oil; The heat-resistant auxiliary agent is a mixture of modified nano cerium oxide and heat-resistant agent Luck MR-30E in a mass ratio of 1:3; The crosslinking aid is a mixture of N,N-p-phenylbismaleimide and triallyl isocyanurate, with a mass ratio of 3:1; The tackifying resin is p-tert-butylphenol polyacetylene resin; A method for preparing a novel high temperature resistant rubber material for automobile radiator hose comprises the following steps: 1) Plasticizing: Plasticize the POR elastomer on an open mill, keep the roller distance at 1mm, and plasticize until the Mooney viscosity ML1+4 reaches 50-60; 2) Preparation of heat-resistant premixed rubber: Take 25% of the POR elastomer after plastication in step 1, add it to the open mill and roll it, keep the roller distance at 0.7mm, the roller temperature at 45°C, add the heat-resistant additive, and pass the rubber material 5 to 6 times to obtain the premixed rubber; 3) Mixing: Use an open mill for mixing, and keep the roller temperature at 40°C. First, roll the remaining plasticized POR elastomer in step 1, add the premixed rubber in step 2, pass it through three times, and then roll it. The roller spacing is enlarged to 3mm. Then add small ingredients such as stearic acid, antioxidant, magnesium oxide, and tackifying resin in turn, mix for 3 minutes, turn it left and right for three times, then add reinforcing agent and plasticizer, mix for 5 minutes, alternately make triangle bags left and right for 5 times, finally add vulcanizer and cross-linking aid, mix for 2 minutes, pass it through 4 to 6 times, turn it left and right for 3 times, and sheet it out to obtain a mixed rubber; 4) Vulcanization: The mixed rubber is vulcanized at a temperature of 175°C and a pressure of 10±1 MPa for 10 minutes to obtain a new type of high temperature resistant rubber material for automobile radiator hose.
[0016] Example 2 A new type of high temperature resistant rubber material for automobile radiator hose, the raw materials of which include, by weight: 100 parts of POR elastomer, 1 part of stearic acid, 6 parts of magnesium oxide, 3 parts of antioxidant, 90 parts of reinforcing agent, 25 parts of plasticizer, 9 parts of heat resistant additive, 3 parts of tackifying resin, 3.5 parts of vulcanizing agent, and 0.5 parts of cross-linking additive; The antioxidant is a mixture of antioxidant 445 and antioxidant MB in a mass ratio of 2:1; The plasticizer is a mixture of high flash point paraffin oil and liquid polybutadiene, and the high flash point paraffin oil accounts for 60% of the weight of the plasticizer; The crosslinking agent is a mixture of N,N-p-phenylbismaleimide and triallyl isocyanurate, with a mass ratio of 3:2; The heat-resistant auxiliary agent is a mixture of modified nano cerium oxide and heat-resistant agent Luck MR-30E in a mass ratio of 1:2; The crosslinking aid is a mixture of N,N-p-phenylbismaleimide and triallyl isocyanurate, with a mass ratio of 3:2; Others are the same as in Example 1; A method for preparing a novel high temperature resistant rubber material for automobile radiator hose comprises the following steps: 1) Plasticizing: Plasticize the POR elastomer on an open mill, keep the roller distance at 1mm, and plasticize until the Mooney viscosity ML1+4 reaches 50-60; 2) Preparation of heat-resistant premixed rubber: Take 20% of the POR elastomer after plastication in step 1, add it to the open mill and roll it, keep the roller distance at 1mm, the roller temperature at 50℃, add the heat-resistant additive, and pass the rubber material 5 to 6 times to obtain the premixed rubber; 3) Mixing: Use an open mill for mixing, and keep the roller temperature at 50°C. First, roll the remaining plasticized POR elastomer in step 1, add the premixed rubber in step 2, pass it through three times, and then roll it. The roller spacing is enlarged to 2mm. Then add small ingredients such as stearic acid, antioxidant, magnesium oxide, and tackifying resin in turn, mix for 3 minutes, turn it left and right for 3 times, then add reinforcing agent and plasticizer, mix for 5 minutes, alternately make triangle bags left and right for 5 times, finally add vulcanizer and cross-linking aid, mix for 2 minutes, pass it through 4 to 6 times, turn it left and right for 3 times, and sheet it out to obtain a mixed rubber; 4) Vulcanization: The mixed rubber is vulcanized at a temperature of 175°C and a pressure of 10±1 MPa for 10 minutes to obtain a new type of high temperature resistant rubber material for automobile radiator hose.
[0017] Example 3 A new type of high temperature resistant rubber material for automobile radiator hose, the raw materials of which include, by weight: 100 parts of POR elastomer, 1.5 parts of stearic acid, 7 parts of magnesium oxide, 3 parts of antioxidant, 110 parts of reinforcing agent, 30 parts of plasticizer, 12 parts of heat resistant additive, 3 parts of tackifying resin, 3 parts of vulcanizing agent, and 1.0 part of cross-linking additive; The antioxidant is a mixture of antioxidant 445 and antioxidant MB in a mass ratio of 2:1; The reinforcing agent is a mixture of carbon black N539 and SRF, with SRF carbon black accounting for 70 parts; The plasticizer is a mixture of high flash point paraffin oil and liquid polybutadiene, and the high flash point paraffin oil accounts for 30% of the weight of the plasticizer; The heat-resistant auxiliary agent is a mixture of modified nano-cerium oxide and Luck MR-30E in a mass ratio of 1:1; The cross-linking auxiliary agent is triallyl isocyanurate; Others are the same as in Example 1; A method for preparing a novel high temperature resistant rubber material for automobile radiator hose comprises the following steps: 1) Plasticizing: Plasticize the POR elastomer on an open mill, keep the roller distance at 1mm, and plasticize until the Mooney viscosity ML1+4 reaches 50-60; 2) Preparation of heat-resistant premixed rubber: Take 30% of the POR elastomer after plastication in step 1, add it to the open mill and roll it, keep the roller distance at 1mm, the roller temperature at 50℃, add the heat-resistant additive, and pass the rubber material 5 to 6 times to obtain the premixed rubber; 3) Mixing: Use an open mill for mixing, and keep the roller temperature at 45°C. First, roll the remaining plasticized POR elastomer in step 1, add the premixed rubber in step 2, pass it through three times, and then roll it. The roller spacing is enlarged to 2mm. Then add small ingredients such as stearic acid, antioxidant, magnesium oxide, and tackifying resin in turn, mix for 3 minutes, turn it left and right for three times, then add reinforcing agent and plasticizer, mix for 5 minutes, alternately make triangle bags left and right for 5 times, finally add vulcanizer and cross-linking aid, mix for 2 minutes, pass it through 4 to 6 times, turn it left and right for 3 times, and sheet it out to obtain a mixed rubber; 4) Vulcanization: The mixed rubber is vulcanized at a temperature of 175°C and a pressure of 10±1 MPa for 10 minutes to obtain a new type of high temperature resistant rubber material for automobile radiator hose.
[0018] Example 4 A new type of high temperature resistant rubber material for automobile radiator hose, the raw materials of which include, by weight: 100 parts of POR elastomer, 1.5 parts of stearic acid, 8 parts of magnesium oxide, 2 parts of antioxidant, 80 parts of reinforcing agent, 20 parts of plasticizer, 10 parts of heat resistant additive, 5 parts of tackifying resin, 2.0 parts of vulcanizing agent, and 1.8 parts of cross-linking additive; The antioxidant is a mixture of antioxidant 445 and antioxidant MB in a mass ratio of 3:2; The reinforcing agent is a mixture of carbon black N539 and SRF, with SRF carbon black accounting for 50 parts; The plasticizer is a mixture of high flash point paraffin oil and liquid polybutadiene, and the high flash point paraffin oil accounts for 40% of the weight of the plasticizer; The heat-resistant auxiliary agent is a mixture of modified nano-cerium oxide and Luck MR-30E in a mass ratio of 2:3; The crosslinking aid is a mixture of N,N-p-phenylbismaleimide and triallyl isocyanurate, with a mass ratio of 2:1; Others are the same as in Example 1 A method for preparing a novel high temperature resistant rubber material for automobile radiator hose comprises the following steps: 1) Plasticizing: Plasticize the POR elastomer on an open mill, keep the roller distance at 1mm, and plasticize until the Mooney viscosity ML1+4 reaches 50-60; 2) Preparation of heat-resistant premixed rubber: Take 20% of the POR elastomer after plastication in step 1, add it to the open mill and roll it, keep the roller distance at 0.5mm, the roller temperature at 40℃, add the heat-resistant additive, and pass the rubber material 5 to 6 times to obtain the premixed rubber; 3) Mixing: Use an open mill for mixing, and keep the roller temperature at 50°C. First, roll the remaining plasticized POR elastomer in step 1, add the premixed rubber in step 2, pass it through three times, and then roll it. The roller spacing is enlarged to 2mm. Then add small ingredients such as stearic acid, antioxidant, magnesium oxide, and tackifying resin in turn, mix for 3 minutes, turn it left and right for 3 times, then add reinforcing agent and plasticizer, mix for 5 minutes, alternately make triangle bags left and right for 5 times, finally add vulcanizer and cross-linking aid, mix for 2 minutes, pass it through 4 to 6 times, turn it left and right for 3 times, and sheet it out to obtain a mixed rubber; 4) Vulcanization: The mixed rubber is vulcanized at a temperature of 175°C and a pressure of 10±1 MPa for 10 minutes to obtain a new type of high temperature resistant rubber material for automobile radiator hose.
[0019] Comparative Example 1 The nano-cerium oxide is not modified, and the other steps are the same as those in Example 3.
[0020] Comparative Example 2 The heat-resistant auxiliary agent is modified nano cerium oxide, and the rest is the same as in Example 3.
[0021] Comparative Example 3 The raw materials are the same as in Example 3: A method for preparing a novel high temperature resistant rubber material for automobile radiator hose comprises the following steps: 1) Plasticizing: Plasticize the POR elastomer on an open mill, keep the roller distance at 1mm, and plasticize until the Mooney viscosity ML1+4 reaches 50-60; 2) Mixing: Use an open mill for mixing, and keep the roller temperature at 45°C. Wrap the POR elastomer after plastication in step 1 with a roller, add a heat-resistant additive, pass it thinly 3 times, and then wrap it with a roller. The roller spacing is enlarged to 2mm. Then add small materials such as stearic acid, antioxidant, magnesium oxide, and tackifying resin in turn, mix for 3 minutes, turn it left and right 3 times, then add a reinforcing agent and a plasticizer, mix for 5 minutes, alternately make triangle bags left and right 5 times, finally add a vulcanizer and a cross-linking agent, mix for 2 minutes, pass it thinly 4 to 6 times, turn it left and right 3 times, and produce a sheet to obtain a mixed rubber; 3) Vulcanization: The mixed rubber is vulcanized at a temperature of 175°C and a pressure of 10±1 MPa for 10 minutes to obtain a new type of high temperature resistant rubber material for automobile radiator hose.
[0022] Comparative Example 4 The formula of the currently used EPDM radiator hose was selected for comparative test, including 100 parts of EPDM rubber, 5 parts of magnesium oxide, 1 part of stearic acid, 105 parts of carbon black N774, 25 parts of paraffin oil, 1.5 parts of antioxidant MB, 1.0 parts of antioxidant RD, 2.0 parts of vulcanizing agent BIBP and 1.0 parts of vulcanizing aid PDM.
[0023] Performance testing: The rubber samples prepared according to Examples 1-4 and Comparative Examples 1-4 were placed in a flat vulcanizer at 175°C for vulcanization for 10 minutes, and the samples were prepared according to GB / T2941, and the following performance tests were performed: 1. Tensile performance test: measured in accordance with GB / T528 2. Hardness test: measured in accordance with GB / T531.1 3. Hot air aging performance test: measured in accordance with GB / T3512-2014 4. Liquid resistance test: Tested in accordance with GB / T1690-2010 The test results are shown in Table 1: Table 1 .
[0024] From the results in Table 1, it can be seen that the rubber materials prepared in Examples 1-4 of the present invention have excellent heat-resistant air aging performance, good coolant resistance and good physical and mechanical properties. The heat resistance of the prepared radiator hose is greatly improved, and it can be used at high temperature (180°C) for a long time, which prolongs the service life of the hose and can better meet the requirements of the automotive industry at present and in a certain period of time in the future.
[0025] Compared with Comparative Examples 1-4, the rubber material of Example 3 has better mechanical properties, and its heat air aging resistance and coolant resistance are both the best, indicating that the modified nano-cerium oxide and the heat-resistant additive Luck MR-30E in the rubber material have a synergistic effect. At the same time, the modification of nano-cerium oxide and the preparation of heat-resistant premixed rubber are also indispensable links, and their combined effects can significantly improve the heat resistance, mechanical properties and coolant resistance of the rubber material.
[0026] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered as limiting the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A new type of high temperature resistant rubber material for automobile radiator hose, It is characterized in that The raw materials include, by weight: 100 parts of POR elastomer, 1-1.5 parts of stearic acid, 5-8 parts of magnesium oxide, 2-4 parts of antioxidant, 80-110 parts of reinforcing agent, 20-30 parts of plasticizer, 8-12 parts of heat-resistant additive, 3-5 parts of tackifying resin, 2.0-3.5 parts of vulcanizing agent, and 0.5-2.0 parts of cross-linking additive.
2. According to claim 1, the new type of high temperature resistant rubber material for automobile radiator hose, It is characterized in that In parts by weight, the raw materials include: 100 parts of POR elastomer, 1.5 parts of stearic acid, 7 parts of magnesium oxide, 3 parts of antioxidant, 110 parts of reinforcing agent, 30 parts of plasticizer, 12 parts of heat-resistant additive, 3 parts of tackifying resin, 3 parts of vulcanizing agent, and 1.0 part of cross-linking additive.
3. The new type of high temperature resistant rubber material for automobile radiator hose according to claim 1 or 2, It is characterized in that The heat-resistant auxiliary agent consists of modified nano cerium oxide and heat-resistant agent Luck MR-30E, and the mass fraction of the modified nano cerium oxide is not less than 2 parts.
4. According to claim 3, the new type of high temperature resistant rubber material for automobile radiator hose, It is characterized in that The modified nano cerium oxide is modified by using a titanate coupling agent.
5. According to claim 1, the new type of high temperature resistant rubber material for automobile radiator hose, It is characterized in that The reinforcing agent consists of carbon black N539 and SRF, and the mass fraction of SRF in 80 to 110 parts of the reinforcing agent is 50 to 70 parts.
6. The new type of high temperature resistant rubber material for automobile radiator hose according to claim 1, It is characterized in that The plasticizer is any one or both of high flash point paraffin oil and liquid polybutadiene.
7. The new type of high temperature resistant rubber material for automobile radiator hose according to claim 1, It is characterized in that The antioxidant consists of antioxidant 445 and antioxidant MB.
8. The new type of high temperature resistant rubber material for automobile radiator hose according to claim 1, It is characterized in that The vulcanizing agent is dicumyl peroxide; and the tackifying resin is p-tert-butylphenol polyacetylene resin.
9. The new type of high temperature resistant rubber material for automobile radiator hose according to claim 1, It is characterized in that The cross-linking auxiliary agent is any one or two of N,N-p-phenylbismaleimide and triallyl isocyanurate.
10. A method for preparing the novel high temperature resistant rubber material for automobile radiator hose according to claim 1, It is characterized in that The following steps are involved: Plasticizing: Plasticize the POR elastomer on an open mill, keep the roller distance at 1mm, and plasticize until the Mooney viscosity ML1+4 reaches 50-60; 2) Preparation of heat-resistant premixed rubber: Take 20%-30% of the POR elastomer after plastication in step 1, add it to the open mill and roll it, keep the roller distance at 0.5-1mm, the roller temperature at 40-50℃, add the heat-resistant additive, and pass the rubber material 5-6 times to obtain the premixed rubber; 3) Mixing: Mixing is performed using an open mill, and the roller temperature is maintained at 40-50°C. First, the remaining plasticized POR elastomer in step 1 is rolled, and the premixed rubber in step 2 is added. After thinning through 3 times, the roller is rolled, and the roller spacing is enlarged to 2-3 mm. Then, stearic acid, antioxidant, magnesium oxide, and tackifying resin are added in sequence. Mixing is performed for 3 minutes, and the mixture is turned left and right for 3 times. Then, a reinforcing agent and a plasticizer are added. Mixing is performed for 5 minutes, and triangle packing is performed alternately left and right for 5 times. Finally, a vulcanizing agent and a cross-linking aid are added. Mixing is performed for 2 minutes, and the mixture is thinned through 4-6 times, and the mixture is turned left and right for 3 times. Sheets are produced to obtain a mixed rubber. 4) Vulcanization: The mixed rubber is vulcanized at a temperature of 175°C and a pressure of 10±1 MPa for 10 minutes to obtain a new type of high temperature resistant rubber material for automobile radiator hose.