Watertight power cable sheath material and preparation method thereof
By using fluorine-containing additives and phosphorus-nitrogen synergistic flame retardant elements in the watertight cable sheath, combined with nano-inorganic fillers, a cross-linking network structure is formed, which solves the increase in weight, influence of conductivity and decreasing flame retardant effect of traditional watertight cables. Problem, cable sheath material with high flame retardant, low smoke volume and excellent hydrophobic effect is achieved.
Patent Information
- Application Number
- CN202411134894.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-15
AI Technical Summary
The water-retardant paste seal of traditional watertight cables has problems such as increasing the weight of the cable, affecting the conductivity, serious joint pollution, difficulty in cleaning and difficult filling process. At the same time, inorganic flame retardant causes the mechanical properties of the sheath material to become worse, and organic flame retardant The effect decreases over time.
采用含丰富氟元素的助剂和磷-氮协同阻燃元素,通过酯化反应制备助剂,形成杂化交联网络结构,结合纳米无机填料和聚乙烯树脂,实现高阻燃、低发烟 and excellent hydrophobic effect.
The high flame retardant, low smoke volume, low harmfulness and long-term stable hydrophobic effects of cable sheath material are achieved, improving the safety and performance of the cable.
Smart Images

Figure BDA0004999111340000021 
Figure BDA0004999111340000031 
Figure BDA0004999111340000032
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cables, and in particular relates to a watertight power cable sheath material and a preparation method thereof. Background Art
[0002] Watertight cables are commonly used in underwater equipment, outdoor equipment, ships, marine engineering, mines, etc. They can transmit power, signals and data to meet the needs of different applications. Traditional watertight cables are sealed with water-blocking paste. After the water-blocking paste is cured at room temperature, it tightly combines the various component structures together to form a solid whole to achieve a water-blocking effect. Although water-blocking paste can improve the waterproof performance of watertight cables to a certain extent, its shortcomings cannot be ignored, especially increasing the weight of the cable, affecting the conductivity, seriously polluting the cable joints, making cleaning difficult, and the filling process difficult to control.
[0003] The cable sheath is the outermost layer of the cable. As the most important barrier to maintain the safety of the internal structure of the cable, it plays the role of water immersion resistance, fire resistance and flame retardancy. The flame retardants of cable sheath materials are mainly divided into organic and inorganic types. Among them, inorganic flame retardants usually use mica, magnesium oxide, magnesium hydroxide, aluminum hydroxide and other materials. The amount of inorganic flame retardant components added is usually as high as 50% or more. Although it has high fire resistance and flame retardancy, it will cause the mechanical properties of the sheath material to deteriorate. Organic flame retardants are usually added to the sheath material by physical mixing, and the flame retardant effect is easy to gradually decrease over time. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a watertight power cable sheath material and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A watertight power cable sheath material comprises the following raw materials in parts by weight: 100-110 parts of polyethylene resin, 20-30 parts of ethylene-vinyl acetate copolymer, 20-30 parts of inorganic filler, 10-15 parts of compatibilizer, 7-12 parts of auxiliary agent, 2-5 parts of coupling agent, 2-4 parts of lubricant, 1.5-4 parts of antioxidant, 1.5-4 parts of ultraviolet absorber and 0.5-1 part of crosslinking agent.
[0007] Furthermore, the inorganic filler is one or more of nano calcium carbonate, nano silicon dioxide, nano titanium dioxide, magnesium hydroxide, aluminum hydroxide, and talc.
[0008] Furthermore, the compatibilizer is maleic anhydride grafted polyethylene.
[0009] Furthermore, the auxiliary agent is prepared by the following steps:
[0010] S1. First, blow nitrogen gas into a dry brown three-necked flask for 30 minutes to drive away the air in the flask, then add 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, pyridine and benzene, stir and dissolve, then slowly add a mixed solution of 1,5-hexadienol and benzene and stir continuously. After the addition is completed, stir and react at room temperature for 12 hours. After the reaction is completed, distill under reduced pressure, purify by column chromatography (a mixed solvent of benzene and acetone is selected as the eluent, and the volume ratio of benzene to acetone is 9:1), and distill under reduced pressure to obtain intermediate 1; the amount ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, 1,5-hexadienol, pyridine and benzene is 23.8 g:9.7 mL:7.8 mL:180 mL;
[0011] Pyridine is used as an acid-binding agent, and the molar ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide and 1,5-hexadienol is controlled to be 1:1.05-1.1, then 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide and 1,5-hexadienol undergo an esterification reaction, and the reaction equation is as follows:
[0012]
[0013] S2. Replace the air in a dry brown three-necked flask with nitrogen at room temperature, then add intermediate 1, triethylamine and DMSO (dimethyl sulfoxide), stir and dissolve, then slowly add a mixed solution of 2-methylene-1,3-propanediol and DMSO and stir continuously, stir and react at room temperature for 12 hours after the addition is completed, and distill under reduced pressure to obtain intermediate 2; the amount ratio of intermediate 1, 2-methylene-1,3-propanediol, triethylamine and DMSO is 26.3 g:6.5 mL:12.5 mL:200 mL;
[0014] Triethylamine is used as an acid binding agent to control the molar ratio of intermediate 1 and 2-methylene-1,3-propylene glycol to be 1:1.05-1.1, and then intermediate 1 and 2-methylene-1,3-propylene glycol undergo esterification reaction. The reaction process is as follows:
[0015]
[0016] S3. Under nitrogen protection, add cyanuric chloride, triethylamine and DMSO into a dry three-necked flask, stir until completely dissolved, then slowly add 1H,1H-undecylfluorohexylamine, and after the addition is completed, control the temperature at 0°C to react for 8 hours. After the reaction is completed, distill under reduced pressure, purify by column chromatography (a mixed solvent of benzene and ethyl acetate is selected as the eluent, and the volume ratio of benzene and ethyl acetate is 8:2), and distill under reduced pressure to obtain intermediate 3; the amount ratio of cyanuric chloride, 1H,1H-undecylfluorohexylamine, triethylamine and DMSO is 14.8 g:31.5 mL:23 mL:160 mL;
[0017] In the presence of triethylamine, -Cl of cyanuric chloride and -NH- of intermediate 1 undergo nucleophilic substitution reaction. The reaction process is as follows:
[0018]
[0019] S4. Under nitrogen protection, dissolve intermediate 2 in DMF (N,N-dimethylformamide), stir evenly, add the mixed solution of intermediate 3 and DMF, and stir and react at room temperature for 6 hours. During this period, adjust the pH value of the system to 7 with 10wt% sodium carbonate solution. After the reaction, cool to room temperature, wash with deionized water for 3 times by centrifugation, then wash with anhydrous ethanol for 3 times by centrifugation, and finally dry at 80°C for 12 hours to obtain an auxiliary agent. The dosage ratio of intermediate 2, intermediate 3 and DMF is 22.6g:35.5g:200mL.
[0020] Under heating conditions, the -OH of intermediate 2 and the -Cl of intermediate 3 undergo a substitution reaction, and the reaction process is as follows:
[0021]
[0022] The additive contains abundant fluorine, which has a strong electronegativity, which enables the fluorine to polarize the CF bond in the additive molecule, making it more polar than water molecules, thus showing hydrophobic properties. Adding additives rich in fluorine into cable sheath materials can give the sheath materials excellent hydrophobic effects, so that they can be used as sheath materials for watertight power cables.
[0023] The additives, through the synergistic effect of the halogen-free flame retardant elements nitrogen and phosphorus, not only prevent the decomposition products generated by combustion from escaping, dilute the combustible gas, but also inhibit the thermal decomposition of the sheath material, achieving the purpose of high flame retardancy, low smoke emission, and low harmfulness. Adding phosphorus-nitrogen synergistic flame retardant additives to the cable sheath material can give the cable an efficient and safe flame retardant and smoke suppression effect.
[0024] The additive contains multiple terminal carbon-carbon double bonds, which can react chemically with the unreacted carbon-carbon double bonds at the ends of the matrix resin under the action of the cross-linking agent, so that the additive can be grafted and cross-linked with the matrix resin. The additive is therefore not easy to migrate and fall out, and can exert its hydrophobic, flame retardant and smoke suppression effects in a long-lasting and stable manner.
[0025] At the same time, the carbon-carbon double bonds in the additive can also react chemically with the double bonds on the coupling agent under the action of the cross-linking agent, and there is a chemical bond between the siloxy group of the coupling agent and the inorganic filler. Therefore, a hybrid cross-linked network structure is formed between the matrix resin, additives and fillers. This structure promotes the dispersion and stabilization of the additives and fillers, thereby making the sheath material have excellent hydrophobic effect and flame retardant and smoke suppression effect for a long time.
[0026] Furthermore, the coupling agent is one or more of vinyl tri(2-methoxyethoxy)silane, 3-(methacryloyloxy)propyl trimethoxysilane, vinyl trimethoxysilane, and vinyl triethoxysilane.
[0027] Furthermore, the lubricant is one or more of magnesium stearate, zinc stearate, calcium stearate, polyethylene wax, and polydimethylsiloxane.
[0028] Furthermore, the antioxidant is one or more of antioxidant 1010, antioxidant 2246, antioxidant 1076, antioxidant DSTP, and antioxidant 168.
[0029] Furthermore, the ultraviolet absorber is one or more of ultraviolet absorber UV-531, ultraviolet absorber UVP-327, light stabilizer GW-540, and light stabilizer 744.
[0030] Furthermore, the cross-linking agent is one or more of dicumyl peroxide, di-tert-butyl peroxide, dibenzoyl peroxide, and di-tert-butyl peroxide isopropylbenzene.
[0031] A method for preparing a watertight power cable sheath material comprises the following steps:
[0032] Weigh each raw material by weight, stir and mix the polyethylene resin and ethylene-vinyl acetate copolymer, then add inorganic filler and coupling agent, stir and mix, then add compatibilizer, additive, lubricant, antioxidant, ultraviolet absorber and cross-linking agent, continue to stir and mix, and send into a twin-screw extruder for melt extrusion to obtain a watertight power cable sheath material.
[0033] Beneficial effects of the present invention: chemical reactions exist between the matrix resin, the additives and the fillers, forming a hybrid cross-linked network structure, which promotes the dispersion and stabilization of the additives and the fillers, and thus the additives rich in fluorine elements, phosphorus-nitrogen flame retardant components and the inorganic fillers can fully play their roles, so that the sheath material of the present invention has excellent hydrophobic effects and flame retardant and smoke suppression effects for a long time, and can be used as a sheath material for watertight power cables. DETAILED DESCRIPTION
[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] Example 1
[0036] Preparation of auxiliary agent, the specific steps are as follows:
[0037] S1. Blow nitrogen gas into a 500 mL dry brown three-necked flask for 30 min, then add 23.8 g of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, 7.8 mL of pyridine and 160 mL of benzene, stir and dissolve, then slowly add 9.7 mL of a mixed solution of 1,5-hexadienol and 20 mL of benzene and stir continuously. After the addition is completed, stir and react at room temperature for 12 h. After the reaction is completed, distill under reduced pressure, purify by column chromatography (a mixed solvent of benzene and acetone is selected as the eluent, and the volume ratio of benzene to acetone is 9:1), and distill under reduced pressure to obtain intermediate 1;
[0038] S2. Replace the air in a 500 mL dry brown three-necked flask with nitrogen at room temperature, then add 26.3 g of intermediate 1, 12.5 mL of triethylamine and 180 mL of DMSO, stir to dissolve, then slowly add 6.5 mL of a mixed solution of 2-methylene-1,3-propanediol and 20 mL of DMSO and stir continuously. After the addition is completed, stir and react at room temperature for 12 h. After the reaction is completed, distill under reduced pressure to obtain intermediate 2;
[0039] S3, under nitrogen protection, 14.8 g of cyanuric chloride, 23 mL of triethylamine and 160 mL of DMSO were added to a 500 mL dry three-necked flask, stirred until completely dissolved, and then 31.5 mL of 1H,1H-undecylfluorohexylamine was slowly added. After the addition was completed, the temperature was controlled at 0°C to react for 8 hours. After the reaction was completed, it was distilled under reduced pressure, purified by column chromatography (a mixed solvent of benzene and ethyl acetate was selected as the eluent, and the volume ratio of benzene and ethyl acetate was 8:2), and distilled under reduced pressure to obtain intermediate 3;
[0040] S4. Under nitrogen protection, 22.6 g of intermediate 2 was dissolved in 100 mL of DMF, and after stirring evenly, a mixed solution of 35.5 g of intermediate 3 and 100 mL of DMF was added, and the mixture was stirred at room temperature for 6 h. During this period, the pH value of the system was adjusted to 7 with a 10 wt% sodium carbonate solution. After the reaction was completed, the mixture was cooled to room temperature, washed by centrifugation with deionized water for 3 times, and then washed by centrifugation with anhydrous ethanol for 3 times, and finally dried at 80° C. for 12 h to obtain an auxiliary agent.
[0041] Example 2
[0042] Preparation of cable sheath material, the specific steps are as follows:
[0043] Weigh each raw material by weight, stir and mix 100 parts of polyethylene resin and 20 parts of ethylene-vinyl acetate copolymer, then add 5 parts of nano calcium carbonate, 5 parts of nano titanium dioxide, 10 parts of magnesium hydroxide, 2 parts of vinyl tri(2-methoxyethoxy) silane, stir and mix, then add 10 parts of maleic anhydride grafted polyethylene, 7 parts of the auxiliary agent obtained in Example 1, 2 parts of magnesium stearate, 1 part of antioxidant 1010, 0.5 parts of antioxidant 168, 1.5 parts of ultraviolet absorber UV-531 and 0.5 part of diisopropylbenzene peroxide, continue to stir and mix, and send into a twin-screw extruder for melt extrusion to obtain a watertight power cable sheath material.
[0044] Example 3
[0045] Preparation of cable sheath material, the specific steps are as follows:
[0046] Weigh each raw material by weight, stir and mix 105 parts of polyethylene resin and 27 parts of ethylene-vinyl acetate copolymer, then add 26 parts of magnesium hydroxide and 3 parts of 3-(methacryloyloxy)propyltrimethoxysilane, stir and mix, then add 12 parts of maleic anhydride grafted polyethylene, 10 parts of the additive prepared in Example 1, 3 parts of polyethylene wax, 3 parts of antioxidant 2246, 2 parts of ultraviolet absorber UV-531, 1 part of light stabilizer GW-540 and 0.8 part of di-tert-butyl peroxide, continue to stir and mix, and send into a twin-screw extruder for melt extrusion to obtain a watertight power cable sheath material.
[0047] Example 4
[0048] Preparation of cable sheath material, the specific steps are as follows:
[0049] Weigh each raw material by weight, stir and mix 110 parts of polyethylene resin and 30 parts of ethylene-vinyl acetate copolymer, then add 5 parts of nano silicon dioxide, 5 parts of nano titanium dioxide, 10 parts of magnesium hydroxide, 10 parts of aluminum hydroxide, 5 parts of vinyl tri(2-methoxyethoxy) silane, stir and mix, then add 15 parts of maleic anhydride grafted polyethylene, 12 parts of the auxiliary agent obtained in Example 1, 2 parts of zinc stearate, 2 parts of polydimethylsiloxane, 2 parts of antioxidant 1076, 1 part of antioxidant DSTP, 1 part of antioxidant 168, 4 parts of ultraviolet absorber UVP-327, light stabilizer 744 and 1 part of dibenzoyl peroxide, continue to stir and mix, and send into a twin-screw extruder for melt extrusion to obtain a watertight power cable sheath material.
[0050] Comparative Example 1
[0051] Preparation of cable sheath material, the specific steps are as follows:
[0052] The remaining steps remain unchanged, and the auxiliary agent in Example 4 is removed to prepare the cable sheath material.
[0053] Comparative Example 2
[0054] Preparation of cable sheath material, the specific steps are as follows:
[0055] The remaining steps remain unchanged, and the auxiliary agent in Example 4 is replaced by 4 parts of melamine, 4 parts of ammonium polyphosphate, and 4 parts of 1H,1H-undecylfluorohexylamine to prepare a cable sheath material.
[0056] Performance Testing
[0057] The cable sheath materials prepared in Examples 2-4 and Comparative Examples 1-2 were made into corresponding samples according to different standards, and the tensile strength and elongation at break were tested according to GB / T1040.3-2006; the limiting oxygen index was tested using the method specified in GB / T 2406.2-2009; and the vertical burning grade was tested using UL94. The test results are shown in Table 1 below:
[0058] Table 1
[0059] Test items Tensile strength MPa Elongation at break % Limiting oxygen index % Vertical burning level Example 2 19.5 345 40.1 V-0 Example 3 19.8 347 40.3 V-0 Example 4 20.1 349 40.6 V-0 Comparative Example 1 19.1 332 26.9 V-2 Comparative Example 2 19.3 337 32.7 V-0
[0060] It can be seen from the test results in Table 1 that the cable sheath materials prepared in Examples 2-4 of the present invention have excellent flame retardant properties, tensile strength and elongation at break.
[0061] The cable sheath materials prepared in Examples 2-4 and Comparative Examples 1-2 were cut into 1.5 cm 3 The small cubes were immersed in distilled water at 10℃ and 40℃ for 30 days respectively, and the changes in the morphology of the small cubes were observed. The test results are shown in Table 2 below:
[0062] Table 2
[0063] Test items 10℃ distilled water 40℃ distilled water Example 2 No change No change Example 3 No change No change Example 4 No change No change Comparative Example 1 Volume expansion rate 8.1% Volume expansion rate 20.5% Comparative Example 2 Volume expansion rate 4.3% Volume expansion rate 12.6%
[0064] It can be seen from the test results in Table 2 that the cable sheath material prepared in Examples 2-4 of the present invention has excellent hydrophobicity and can be used as a watertight power cable sheath material.
[0065] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0066] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A watertight power cable sheath material, characterized in that: The invention comprises the following raw materials in parts by weight: 100-110 parts of polyethylene resin, 20-30 parts of ethylene-vinyl acetate copolymer, 20-30 parts of inorganic filler, 10-15 parts of compatibilizer, 7-12 parts of auxiliary agent, 2-5 parts of coupling agent, 2-4 parts of lubricant, 1.5-4 parts of antioxidant, 1.5-4 parts of ultraviolet absorber and 0.5-1 parts of crosslinking agent; Wherein, the auxiliary agent is prepared by the following steps: S1, nitrogen purged into a flask, added 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, pyridine and benzene, stirred, added 1,5-hexadienol and benzene, reacted at room temperature for 12 hours, distilled under reduced pressure, purified by column chromatography, and distilled under reduced pressure to obtain intermediate 1; S2, replace the air in the bottle with nitrogen, add intermediate 1, triethylamine and DMSO, stir, add 2-methylene-1,3-propanediol and DMSO, react at room temperature for 12 hours, and distill under reduced pressure to obtain intermediate 2; S3, under nitrogen protection, add cyanuric chloride, triethylamine and DMSO into a flask, stir, add 1H,1H-undecylfluorohexylamine, react at 0°C for 8h, distill under reduced pressure, purify by column chromatography, and distill under reduced pressure to obtain intermediate 3; S4. Under nitrogen protection, the intermediate 2 is dissolved in DMF, and the intermediate 3 and DMF are added, and the reaction is carried out at room temperature for 6 hours. The pH value of the system is adjusted to 7. After the reaction is completed, the system is cooled, washed, and dried to obtain an auxiliary agent.
2. A watertight power cable sheath material according to claim 1, characterized in that: The amount ratio of 3,9-dichloro-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane 3,9-dioxide, 1,5-hexadienol, pyridine and benzene in step S1 is 23.8 g:9.7 mL:7.8 mL:180 mL; the amount ratio of intermediate 1,2-methylene-1,3-propanediol, triethylamine and DMSO in step S2 is 26.3 g:6.5 mL:12.5 mL:200 mL; the amount ratio of cyanuric chloride, 1H,1H-undecylfluorohexylamine, triethylamine and DMSO in step S3 is 14.8 g:31.5 mL:23 mL:160 mL; the amount ratio of intermediate 2, intermediate 3 and DMF in step S4 is 22.6 g:35.5 g:200 mL.
3. The watertight power cable sheath material according to claim 1, characterized in that: The inorganic filler is one or more of nano calcium carbonate, nano silicon dioxide, nano titanium dioxide, magnesium hydroxide, aluminum hydroxide and talcum powder.
4. The watertight power cable sheath material according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polyethylene.
5. The watertight power cable sheath material according to claim 1, characterized in that: The coupling agent is one or more of vinyl tri(2-methoxyethoxy)silane, 3-(methacryloyloxy)propyl trimethoxysilane, vinyl trimethoxysilane and vinyl triethoxysilane.
6. The watertight power cable sheath material according to claim 1, characterized in that: The lubricant is one or more of magnesium stearate, zinc stearate, calcium stearate, polyethylene wax, and polydimethylsiloxane.
7. The watertight power cable sheath material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant 1010, antioxidant 2246, antioxidant 1076, antioxidant DSTP, and antioxidant 168.
8. The watertight power cable sheath material according to claim 1, characterized in that: The ultraviolet absorber is one or more of the ultraviolet absorber UV-531, the ultraviolet absorber UVP-327, the light stabilizer GW-540, and the light stabilizer 744.
9. The watertight power cable sheath material according to claim 1, characterized in that: The cross-linking agent is one or more of dicumyl peroxide, di-tert-butyl peroxide, dibenzoyl peroxide, and di-tert-butyl peroxycumene.
10. The method for preparing a watertight power cable sheath material according to claim 1, characterized in that: The following steps are involved: Weigh the raw materials by weight, stir and mix the polyethylene resin and ethylene-vinyl acetate copolymer, then add the inorganic filler and coupling agent, stir and mix, then add the compatibilizer, additive, lubricant, antioxidant, ultraviolet absorber and cross-linking agent, continue to stir and mix, and finally send them into a twin-screw extruder for melt extrusion to obtain a watertight power cable sheath material.
Citation Information
Cited By
Special cable applied to solar photovoltaic module and preparation process thereof
CN119852010A
Corrosion-resistant cable sheath material for aerial cable and preparation method of corrosion-resistant cable sheath material
CN120988390A