Underwater long-term stable hydrogel and preparation method thereof
By combining water-soluble and water-insoluble polymers in the hydrogel, forming a hydrophilic interface, and optimizing the network structure with fillers and additives, the problem of hydrogel swelling in water is solved, and high mechanical long-term stability in water is achieved Performance, suitable for a variety of application scenarios.
Patent Information
- Application Number
- CN202411186581.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-15
AI Technical Summary
Hydrogels are prone to swelling when used in water for a long time, resulting in significant attenuation of mechanical properties. The existing technical solutions are complex or toxic solvents are used, making it difficult to achieve stable reliability.
Water-soluble polymers containing hydroxy, amide or carboxylic functional groups combined with water-insoluble polymers form a hydrophilic interface, and optimize the polymer network through fillers and additives to form stable hydrocoagulation through coating molding and drying. glue.
A long-term stable hydrogel in water has been achieved, with a ductility greater than 100%, a tensile stress greater than 500kPa in fracture, and a Young's modulus of 50kPa-5 MPa. It can be soaked in water for more than 3 months and its mechanical properties remain stable, with simple operation. , low cost.
Smart Images

Figure CN118956078A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a hydrogel, and in particular to an underwater long-term stable hydrogel and a preparation method thereof. Background Art
[0002] Similar to biological tissues, hydrogels are continuous colloid or polymer network structure materials containing a large amount of water. They are considered to be the most promising biomimetic engineering materials and have a wide range of applications and research value in the fields of drug release, tissue engineering, bionic organs and in vitro cell culture. However, biological tissue materials can be immersed in tissue fluid for a long time and have high stability, while hydrogels will swell in solvents (water), causing their mechanical properties to significantly decay and hydrogels to have poor adaptability. Therefore, the development of hydrogel materials that can be used in water for a long time has important application value.
[0003] At present, solving the swelling problem of hydrogels, improving the long-term stability of hydrogels in water, and especially stable and reliable mechanical properties have received more and more extensive research attention. The disclosed technical solutions (Science, 2014, 343, 873-875; Adv. Mater. 2015, 27, 7407-7411) show that by introducing unique hydrophobic polymer segments into the hydrogel network and adjusting the hydrophilic-hydrophobic interactions of the polymer, the swelling problem of the hydrogel in water can be well controlled. In addition, it has also been proven that the formation of localized interactions between polymer chains by solvent substitution can achieve gels with good water resistance (Adv. Mater. 2020, 2004579), which can be immersed in water for more than 7 days, but the organic solvents used in the process may cause residues, affecting the use of the gel.
[0004] Although the prior art discloses a variety of solutions to improve the swelling resistance and stability of hydrogels in water and increase the reliability of long-term use of the gel in water, the relevant technologies require complex photocuring molding or involve the use of biotoxic organic solvents. Therefore, it is still technically challenging to develop more efficient technical solutions to achieve swelling-resistant hydrogels that can be used for a long time.
[0005] In order to improve the long-term stability of the gel in water, it is necessary to solve the problem of water absorption and swelling of the gel polymer network in water. Usually, the water is isolated by an outer layer to form a physical isolation layer at the interface between the gel and water, but this hinders the medium transfer between the gel and water, thus limiting the application scenarios of the gel. Secondly, the efficiency of physical isolation is poor, and the destruction of the physical isolation layer will cause the solution to fail quickly. Summary of the invention
[0006] The purpose of the present invention is to solve the problem that the hydrogel material is immersed in water / salt water and causes structural swelling, resulting in significant deterioration of the mechanical toughness of the gel, and to provide a long-term stable underwater hydrogel.
[0007] Specifically, a hydrogel that is stable underwater for a long time has an elongation greater than 100%, a tensile stress at break greater than 500kPa-2MPa, and a Young's modulus of 50kPa-5MPa. It is mainly prepared from 10-60 parts of a water-soluble polymer, 10-60 parts of a water-insoluble polymer, 0-10 parts of a filler, 0-5 parts of an additive, and 20-80 parts of water.
[0008] Among them, the water-soluble polymer is a polymer that can absorb water to form a gel structure, and contains hydroxyl, amide or carboxyl functional groups, which can be one or more combinations of polyvinyl alcohol, polyacrylic acid, sodium polyacrylate, polyhydroxyethyl acrylate, water-soluble cellulose, sodium alginate and chitosan.
[0009] Among them, the non-water-soluble polymer can interact with the water-soluble polymer to form hydrogen bond interactions, electrostatic interactions, hydrophobic interactions, etc., thereby forming a stable hydrophilic-hydrophobic interface and increasing the structural stability of the water-soluble polymer. It can be one or more combinations of polyethylene-vinyl acetate copolymer (EVA), polyurethane, polytetrafluoroethylene, silicone and fluoroelastomer.
[0010] Furthermore, the water-insoluble polymer is an aqueous emulsion to increase the uniformity of the water-insoluble polymer and the water-soluble polymer during the mixing process and promote the formation of a stable phase separation.
[0011] The filler increases the structural strength of the gel, promotes the gel to form a stable polymer network, and plays a role in enhancing the mechanical properties of the gel. It can be an inorganic material for adjusting the structural strength and stability of the gel, and can be one or more of silicon dioxide, magnesium oxide, aluminum oxide, diatomaceous earth and magnesium aluminum hydrotalcite.
[0012] Among them, the auxiliary agent increases the stability of the preparation process system, avoids the instability and phase separation of the mixed liquid system, and extends the process operation time; secondly, the auxiliary agent also increases the surface smoothness of the gel molding, reduces the interface adhesion and other effects, and can be a surfactant, such as polyvinyl pyrrolidone, F127, etc., or small molecule alcohols, such as ethanol, isopropanol, ethylene glycol or propylene glycol. One or more.
[0013] Another object of the present invention is to provide a method for preparing the hydrogel.
[0014] Specifically, the method for preparing the hydrogel comprises the following steps:
[0015] S1: dissolving 10-60 parts of a water-soluble polymer in water, then adding 0-30 parts of a filler and 0-5 parts of an auxiliary agent and mixing evenly to obtain a mixed solution 1;
[0016] S2: 10-60 parts of non-water-soluble polymer emulsion are mixed with the above mixed solution, stirred and mixed, and degassed to obtain mixed solution 2;
[0017] S3: coating the mixed solution 2 on a substrate to form a thin film;
[0018] S4: Drying and molding;
[0019] S5: The dried film is immersed in water to hydrate and form a hydrogel.
[0020] In step S1, a water-soluble polymer is dissolved in water to form an aqueous solution with a polymer mass fraction of 1% to 30%.
[0021] In step S2, the content of the water-insoluble polymer in the emulsion is 10%-70%.
[0022] In step S2, a planetary degassing machine or a vacuum degassing machine is used for 5-20 minutes to remove bubbles in the solution.
[0023] In step S3, the coating thickness is 10 micrometers to 2000 micrometers. The coating can be carried out by a wire rod coater, a doctor blade, a slit coater or a spray coater, etc. The substrate can be glass, PET or other flat substrates.
[0024] In step S4, hot air drying or infrared drying is used for drying, the drying temperature is 60-150 degrees, and the drying time is 1 minute to 360 minutes.
[0025] In step S5, the film is immersed in water at a temperature of 20-50 degrees for 30 minutes to 24 hours. The water can be pure water, salt water, alcohol-water mixture or biological culture medium. The salt water can be a salt solution such as NaCl, KCl, etc., with a salt concentration of 0.01-10%; the alcohol-water mixture can be an aqueous solution of ethanol, isopropanol, ethylene glycol or glycerol, with an alcohol concentration of 0.01-30%.
[0026] The beneficial effects of the present invention compared with the prior art are as follows:
[0027] 1. Controlling the hydrogel polymer network to form a hydrophilic and hydrophobic two-phase structure is the basic principle of hydrogel anti-swelling, and realizes the preparation of hydrogels that can be stable in water for a long time. Therefore, the focus of the present invention is how to promote the formation of a strong interactive two-phase interface and a structurally stable two-phase structure between water-soluble polymers and water-insoluble polymers.
[0028] (1) Type of hydrophilic polymer. The hydrophilic polymer absorbs water to form a fluffy network, which is the prerequisite for the formation of hydrogel. Without the hydrophilic polymer, gel cannot be formed. However, the unlimited swelling of the hydrophilic polymer until it dissolves is also the fundamental reason that restricts the long-term use of hydrogel in water. The hydrophilic polymer selected in the present invention is a polymer containing hydroxyl, amide or carboxyl functional groups, which can be partially hydrated in water to form a gel. At the same time, the interaction between polymer chains and the presence of hydrophobic microphases of polymer chains limit their complete dissolution in water.
[0029] (2) Formation of hydrophilic-hydrophobic interface. The introduction of non-water-soluble polymers can form a hydrophilic-hydrophobic interface with the water-soluble polymer. The result of this action is similar to anchoring the water-soluble polymer molecular chain to the periphery of the non-water-soluble polymer through the hydrophilic-hydrophobic interface to form a continuous hydrophilic-hydrophobic network. The formation of this hydrophilic-hydrophobic interface is during step S4, by drying to remove water, and the mixed solution forms a solid film. During the hydration process of step S5, the water-soluble polymer can absorb water again to form a gel, while the non-water-soluble polymer cannot be rehydrated, thus forming a hydrogel network supported by the non-water polymer.
[0030] (3) Introduction of fillers: The fillers of the present invention can be filled in the polymer network to improve the structural stability of the gel and increase the mechanical strength of the gel.
[0031] (3) Selection of additives. Additives are used to promote the formation of hydrophilic-hydrophobic interfaces. They increase the stability of water-soluble polymer and water-insoluble polymer emulsions, improve the dispersion stability of fillers in them, avoid phase separation, and help form a uniform and continuous two-phase microstructure.
[0032] 2. The hydrogel obtained by the present invention has excellent anti-swelling properties and can be stored or used in water for a long time. The elongation of the hydrogel is greater than 100%, the tensile stress at break is greater than 500kP, and the Young's modulus is 50kPa-5 MPa. The hydrogel can be soaked in water, physiological saline or biological culture fluid for a long time, and the soaking time exceeds 3 months. The mechanical properties of the gel before and after soaking remain stable, and the mass change rate before and after soaking is less than 10%.
[0033] 3. Compared with the prior art, the technical method provided by the present invention is simple, and the gel can be obtained only by coating and molding, which is simple to operate and highly efficient. In addition, the present invention does not involve polymerization reaction, and the raw materials are bulk raw materials in the market, and no toxic or harmful monomer raw materials are used, which is low in cost.
[0034] 4. The hydrogel obtained by the present invention can be used as an engineering gel for underwater use, and can be applied in flexible electronic materials, medical dressings, tissue engineering materials, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1The stress-strain relationship curves of polyvinyl alcohol / polyethylene-vinyl acetate copolymer (EVA) hydrogels with different EVA contents.
[0036] Figure 2 The stress-strain curves of cellulose / polyethylene-vinyl acetate copolymer (EVA) hydrogels with different EVA contents.
[0037] Figure 3 This is the mass change of polyvinyl alcohol / polyethylene-vinyl acetate copolymer (EVA) hydrogel when immersed in water.
[0038] Figure 4 The stress-strain changes of polyvinyl alcohol / polyethylene-vinyl acetate copolymer (EVA) hydrogel when immersed in water.
[0039] Figure 5 The stress-strain curves of polyvinyl alcohol / polyurethane hydrogels with different polyurethane contents.
[0040] Figure 6 The stress-strain curves of polyvinyl alcohol / fluoroelastomer hydrogels with different fluoroelastomer contents. DETAILED DESCRIPTION
[0041] Example 1 Polyvinyl alcohol / polyethylene-vinyl acetate copolymer (EVA) type hydrogel
[0042] 20 grams of polyvinyl alcohol was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly to obtain a mixed solution 1.
[0043] Take 10 grams, 20 grams, 30 grams, 40 grams and 50 grams of polyethylene-vinyl acetate copolymer (EVA) and use an emulsion with a concentration of 50%.
[0044] Mixed solution 1 was mixed with the above-mentioned EVA emulsion, and then mechanically stirred for 30 minutes at a stirring speed of 1000rpm to obtain mixed solution 2. Mixed solution 2 was vacuum degassed for 10 minutes. Mixed solution 2 was coated on a substrate to form a film using a scraper coater. The scraper spacing was 100 microns, the coating speed was 600mm / min, and the coating substrate was glass. After coating, it was placed in a hot air oven for drying at a drying temperature of 70 degrees and a drying time of 120 minutes. The dried film was removed and immersed in pure water at a soaking temperature of 30 degrees and a soaking time of 2 hours to obtain a polyvinyl alcohol / polyethylene-vinyl acetate copolymer (EVA) type hydrogel. The stress-strain curve of the obtained gel is shown in the attached figure. Figure 1 shown.
[0045] Example 2 Cellulose / polyethylene-vinyl acetate copolymer (EVA) type hydrogel
[0046] 20 grams of water-soluble cellulose was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly to obtain a mixed solution 1.
[0047] Take 10 grams, 30 grams and 50 grams of polyethylene-vinyl acetate copolymer (EVA) and use an emulsion with a concentration of 50%.
[0048] Take mixed solution 1, mix it with the above-mentioned EVA emulsion, and then stir it mechanically for 30 minutes at a stirring speed of 1000rpm to obtain mixed solution 2. Degas the mixed solution 2 in vacuum for 10 minutes. Use a scraper coater to coat the mixed solution 2 on the substrate to form a film. The scraper spacing is 100 microns, the coating speed is 600mm / min, and the coating substrate is glass. After coating, put it into a hot air oven to dry. The drying temperature is 70 degrees and the drying time is 120 minutes; remove the dried film and soak it in pure water. The soaking temperature is 30 degrees and the soaking time is 2 hours to obtain a cellulose type / polyethylene-vinyl acetate copolymer (EVA) hydrogel. The stress-strain curve of the gel is shown in the attached figure. Figure 2 shown.
[0049] Example 3 Long-term stability of polyvinyl alcohol / polyethylene-vinyl acetate copolymer (EVA) type hydrogel in water
[0050] The polyvinyl alcohol hydrogel containing 20 g of EVA in Example 1 was immersed in pure water at a temperature of 25 degrees. The mass of the gel after different immersion times was weighed, and the stress and strain of the gel before and after immersion were tested. The changes in gel mass are shown in the attached figure. Figure 3 The stress-strain of the gel is shown in the attached Figure 4 shown.
[0051] Example 4 Polyvinyl alcohol / polyurethane type hydrogel
[0052] 20 grams of polyvinyl alcohol was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly to obtain a mixed solution 1.
[0053] Take 10g, 20g, 30g, 40g and 50g of polyurethane emulsion with a concentration of 30%.
[0054] Take mixed solution 1, mix it with the above-mentioned polyurethane emulsion, and then stir it mechanically for 30 minutes at a stirring speed of 1000rpm to obtain mixed solution 2. Degas the mixed solution 2 in vacuum for 10 minutes. Use a scraper coater to coat the mixed solution 2 on the substrate to form a film. The scraper spacing is 100 microns, the coating speed is 600mm / min, and the coating substrate is glass. After coating, put it into a hot air oven to dry. The drying temperature is 70 degrees and the drying time is 120 minutes. Remove the dried film and soak it in pure water. The soaking temperature is 30 degrees and the soaking time is 2 hours to obtain a polyvinyl alcohol / polyurethane type hydrogel. The stress-strain curve of the obtained gel is shown in the attached figure. Figure 5 shown.
[0055] Example 6 Polyvinyl alcohol / fluoroelastomer type hydrogel
[0056] 20 grams of polyvinyl alcohol was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly to obtain a mixed solution 1.
[0057] Take 10 g, 20 g and 30 g of fluoroelastomer emulsion with a concentration of 20%.
[0058] Take mixed solution 1, mix it with the above 5 parts of fluoroelastomer emulsion, and then stir it mechanically for 30 minutes at a stirring speed of 1000rpm to obtain mixed solution 2. Degas the mixed solution 2 in vacuum for 10 minutes. Use a scraper coater to coat the mixed solution 2 on the substrate to form a film. The scraper spacing is 100 microns, the coating speed is 600mm / min, and the coating substrate is glass. After coating, put it into a hot air oven to dry. The drying temperature is 70 degrees and the drying time is 120 minutes. Remove the dried film and soak it in pure water. The soaking temperature is 30 degrees and the soaking time is 2 hours to obtain a polyvinyl alcohol / fluoroelastomer hydrogel. The stress-strain curve of the obtained gel is shown in the attached figure. Figure 6 shown.
Claims
1. A long-term stable underwater hydrogel, characterized in that: The invention is mainly prepared from 10-60 parts of water-soluble polymer, 10-60 parts of water-insoluble polymer, 0-10 parts of filler, 0-5 parts of auxiliary agent and 20-80 parts of water.
2. The underwater long-term stable hydrogel according to claim 1, characterized in that: The water-soluble polymer is a polymer containing a hydroxyl group, an amide group or a carboxyl group functional group.
3. The underwater long-term stable hydrogel according to claim 2, characterized in that: The water-soluble polymer is one or more combinations of polyvinyl alcohol, polyacrylic acid, sodium polyacrylate, polyhydroxyethyl acrylate, water-soluble cellulose, sodium alginate and chitosan.
4. The underwater long-term stable hydrogel according to claim 2, characterized in that: The water-insoluble polymer is one or more combinations of polyethylene-vinyl acetate copolymer, polyurethane, polytetrafluoroethylene, silicone and fluoroelastomer.
5. The underwater long-term stable hydrogel according to claim 4, characterized in that: The water-insoluble polymer is an aqueous emulsion.
6. The underwater long-term stable hydrogel according to claim 1, characterized in that: The filler is one or more combinations of silicon dioxide, magnesium oxide, aluminum oxide, diatomaceous earth and magnesium aluminum hydrotalcite.
7. The underwater long-term stable hydrogel according to claim 1, characterized in that: The auxiliary agent is a surfactant or a small molecule alcohol.
8. The method for preparing the underwater long-term stable hydrogel according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1: dissolving 10-60 parts of a water-soluble polymer in water, then adding 0-30 parts of a filler and 0-5 parts of an auxiliary agent and mixing evenly to obtain a mixed solution 1; S2: 10-60 parts of the water-insoluble polymer emulsion are mixed with the mixed solution 1, stirred and mixed, and degassed to obtain a mixed solution 2; S3: coating the mixed solution 2 on a substrate to form a thin film; S4: Drying and molding; S5: The dried film is immersed in water to hydrate and form a hydrogel.
9. The method for preparing underwater long-term stable hydrogel according to claim 8, characterized in that: In the step S1, the water-soluble polymer is dissolved in water to form an aqueous solution with a polymer mass fraction of 1%-30%; in the step S2, the content of the water-insoluble polymer in the water-insoluble polymer emulsion is 10%-70%.
10. The method for preparing underwater long-term stable hydrogel according to claim 8, characterized in that: In the step S2, a planetary degassing machine or a vacuum degassing machine is used, and the degassing time is 5-20 minutes; in the step S3, the coating thickness is 10 microns to 2000 microns; in the step S4, hot air drying or infrared drying is used for drying, the drying temperature is 60-150 degrees, and the drying time is 1 minute to 360 minutes; in the step S5, the film is immersed in water at a temperature of 20-50 degrees, and the immersion time is 30 minutes to 24 hours.