Medical PVC pump pipe material and production process thereof

Through the combination of modified PVC resin and hyperbranched polyester, the problem of insufficient antibacterial and mechanical properties of PVC materials is solved, and its antibacterial and mechanical properties are improved, which extends the service life and enhances biocompatibility and heat resistance.

CN118956085AInactive Publication Date: 2024-11-15NINGBO TIANYI MEDICAL APPLIANCE CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411455163.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Pure PVC materials lack antibacterial ability and mechanical properties, which can easily lead to bacterial adhesion and shorten service life, making it difficult to meet medical needs.

Method used

Modified PVC resin and modified hyperbranched polyester, through compounds such as triglycidyl isocyanurate, N,N-dimethylformamide, 2,2-dihydroxymethylpropionic acid and p-toluenesulfonic acid. The reaction is to prepare modified hyperbranched polyester and combine it with PVC resin to increase the mechanical properties and antibacterial properties of the material.

Benefits of technology

It improves the mechanical properties, antibacterial properties and hydrophilicity of PVC materials, extends service life, and enhances biocompatibility and heat resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of PVC materials, and discloses a medical PVC pump pipe material and a production process thereof. The medical PVC pump pipe material is prepared from the following raw materials in parts by weight: 100 parts of modified PVC resin, 8 to 15 parts of polyurethane elastomer, 35 to 55 parts of plasticizer, 5 to 10 parts of modified hyperbranched polyester, 0.5 to 1 part of heat stabilizer, 0.5 to 1.5 parts of antioxidant and 0.1 to 0.5 part of lubricant, according to the material, modified PVC resin is used as matrix resin, and various auxiliaries are added to improve the comprehensive performance of the PVC material; due to the addition of the modified hyperbranched polyester, the mechanical property, the heat resistance and the antibacterial property of the matrix are improved; due to modification treatment of the PVC resin, the antibacterial property, the mechanical property and the hydrophilicity of the matrix are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PVC materials, and in particular to a medical PVC pump tube material and a production process thereof. Background Art

[0002] Medical PVC, also known as medical plastic, has good physical and mechanical properties and chemical stability, and is more suitable for use in the medical field. The product is stable and safe, and the industry has attracted much attention for its high added value, high growth rate and broad market potential. PVC material is a good medical consumable due to its good flexibility, high transparency, good quality and low price. It can be used in the production of PVC pump tubes to meet different medical needs.

[0003] However, pure PVC material does not have antibacterial ability, and it is a hydrophobic material. It is easy for bacteria to attach to form biofilm during use, causing material failure or causing infection in patients. Therefore, PVC needs to be effectively modified for antibacterial properties. In addition, PVC hoses may be squeezed multiple times during use, and squeezing will cause the mechanical properties of PVC materials to decrease, thereby affecting their service life. Therefore, when using PVC materials for medical use, they must have good biocompatibility and antibacterial properties, as well as excellent mechanical properties. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a medical PVC pump tube material and a production process thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions: A medical PVC pump tube material, comprising the following raw materials in parts by weight: 100 parts of modified PVC resin, 8-15 parts of polyurethane elastomer, 35-55 parts of plasticizer, 5-10 parts of modified hyperbranched polyester, 0.5-1 parts of heat stabilizer, 0.5-1.5 parts of antioxidant, and 0.1-0.5 parts of lubricant; The modified hyperbranched polyester is prepared by the following steps: Step A1, dispersing triglycidyl isocyanurate evenly in N,N-dimethylformamide, adding diethanolamine, and heating to 70-90° C. to react for 2-5 hours. After the reaction is completed, filtering and drying are performed to obtain a first intermediate product; Step A2, under nitrogen conditions, the first intermediate product, 2,2-dihydroxymethylpropionic acid and p-toluenesulfonic acid are added to a reactor and mixed evenly, and heated to 125-145° C., reacted for 2-3 hours, the nitrogen is stopped, and the reaction is continued for 3-4 hours under vacuum conditions, and then the reaction is reduced in pressure for 2 hours. When no water is distilled out, it is cooled to room temperature, 20-40 mL of acetone is added, stirred and mixed for 10 minutes, and then recrystallized, filtered, and dried to obtain a second intermediate product; Step A3, slowly heating the second intermediate product, methyl laurate, dibutyltin dilaurate and p-hydroxyanisole to 110-120° C. under stirring, maintaining the top temperature of the fractionation column at 55-65° C., and keeping the reaction for 2-5 hours. After the reaction is completed, distilling under reduced pressure to obtain a hyperbranched polyester; Step A4, mixing epichlorohydrin in methanol uniformly, and heating to 55-65° C., adding hyperbranched polyester under stirring, and continuing stirring for 4-6 hours, distilling under reduced pressure, washing, and drying to obtain modified hyperbranched polyester; Further, in step A1, the usage ratio of triglycidyl isocyanurate, N,N-dimethylformamide and diethanolamine is 0.3-0.35 mol:200 mL:0.1 mol; Further, in step A2, the molar ratio of the first intermediate product to 2,2-dimethylolpropionic acid is 1:12, and the amount of p-toluenesulfonic acid used is 0.5% of the total mass of the first intermediate product and 2,2-dimethylolpropionic acid; Further, in step A3, the molar ratio of the second intermediate product to methyl laurate is 1:24, the mass of dibutyltin dilaurate is 0.3%-0.4% of the total mass of the second intermediate product and methyl laurate, and the mass of p-hydroxyanisole is 0.001-0.002 g; Furthermore, in step A4, the usage ratio of epichlorohydrin, hyperbranched polyester and methanol is 10-30 mL: 2-5 g: 200 mL.

[0006] The modified PVC resin is prepared by the following steps: Step B1, adding cellulose to isopropanol for dispersion, raising the temperature to 60-70°C for reaction for 10-20 minutes, then raising the temperature to 80-85°C, adding 1,2-epoxy-5-hexene, and continuing the reaction for 8-12 hours, then filtering, washing, and drying to obtain pre-treated cellulose; Step B2, grind the PVC resin into powder, add dibenzoyl peroxide and 1,2-dichloroethane and stir evenly, then add 1-vinylimidazole, heat to 65-75°C under nitrogen and react for 2-3h, then add pre-treated cellulose and continue to react for 2-3h, then add methanol, filter, wash and dry to obtain modified PVC resin; Further, in step B1, the ratio of cellulose, isopropanol and 1,2-epoxy-5-hexene is 1-3 g:50 mL:0.5-2 g; Furthermore, in step B2, the usage ratio of PVC resin, dibenzoyl peroxide, 1,2-dichloroethane, 1-vinylimidazole, pre-treated cellulose and methanol is 5-10 g: 0.2-0.4 g: 100 mL: 0.5-0.8 g: 1-2 g: 100 mL.

[0007] A production process of medical PVC pump tube material comprises the following steps: Weigh the raw materials by weight, add the modified PVC resin, polyurethane elastomer, plasticizer, modified hyperbranched polyester, heat stabilizer, antioxidant and lubricant into a twin-screw extruder in sequence, and perform extrusion, granulation and air cooling to obtain a medical PVC pump tube material; Furthermore, the processing temperature of the twin-screw extruder is 60-70°C for stage 1, 100-110°C for stage 2, 80-90°C for stage 3, 100-110°C for stage 4, and 115-125°C for stage 5.

[0008] Beneficial effects of the present invention: The medical PVC pump tube material applied for by the present invention uses modified PVC resin as the base resin, and adds various additives to improve the comprehensive performance of the PVC material; the addition of modified hyperbranched polyester improves the mechanical properties, heat resistance and antibacterial properties of the base; the modification treatment of PVC resin improves the antibacterial properties, mechanical properties and hydrophilicity of the base.

[0009] In the modified hyperbranched polyester, the epoxy group in triglycidyl isocyanurate is firstly reacted with the secondary amine in diethanolamine to generate a first intermediate product containing a tertiary amine structure; the terminal hydroxyl group in the first intermediate product is reacted with the carboxyl group in 2,2-dihydroxymethylpropionic acid to generate a second intermediate product; the terminal hydroxyl group in the second intermediate product is then reacted with the ester group in methyl laurate to generate a hyperbranched polyester; finally, the chlorine atom in epichlorohydrin is reacted with the tertiary amine in the hyperbranched polyester to generate a modified hyperbranched polyester containing a quaternary ammonium salt structure and an epoxy group. After the modified hyperbranched polyester is added to the matrix, the long-chain alkyl at its end can be entangled with the PVC molecular chain, and this entanglement can also improve the comprehensive performance of the PVC material; wherein, the modified hyperbranched polyester has an irregular three-dimensional spherical structure, a wide molecular weight distribution and excellent biocompatibility, these characteristics make it have a certain fluidity during the processing of the PVC material, thereby improving the flexibility of the PVC material, while also improving the crystallinity of the PVC molecular chain, thereby enhancing the mechanical properties of the matrix; the epoxy group contained in the hyperbranched polymer can also capture the free radicals generated by the decomposition of the PVC molecular chain, terminate the free radical reaction of the degradation of the PVC molecular chain, slow down the degradation rate, and effectively improve the durability of the PVC material; in addition, the introduction of the heat-resistant group isocyanurate ring improves the heat resistance of the matrix, and the introduction of the quaternary ammonium salt structure further improves the antibacterial property of the matrix.

[0010] The modified PVC resin is firstly prepared by reacting the hydroxyl groups in cellulose with the epoxy groups in 1,2-epoxy-5-hexene to obtain pre-treated cellulose; then, under the action of an initiator, the pre-treated cellulose and 1-vinylimidazole are grafted onto the side chain of the PVC molecule to obtain the modified PVC resin. The modified PVC resin uses free radical grafting to graft the pre-treated cellulose and 1-vinylimidazole onto the PVC molecular chain, thereby improving the antibacterial properties, mechanical properties and hydrophilicity of the PVC resin; wherein, the introduction of the imidazole structure can synergistically act with the quaternary ammonium salt structure in the modified hyperbranched polyester to give the matrix excellent antibacterial properties; the large amount of hydrophilic groups contained in the pre-treated cellulose can improve the hydrophilicity of the PVC resin, thereby improving the cleaning ability of the PVC matrix surface, and the multiple double bond structures contained in the pre-treated cellulose also play a cross-linking role, which can increase the density of the PVC resin itself, thereby improving the mechanical properties of the PVC material. DETAILED DESCRIPTION

[0011] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0012] Example 1 The modified hyperbranched polyester is prepared by the following steps: Step A1, 0.3 mol of triglycidyl isocyanurate is evenly dispersed in 200 mL of N,N-dimethylformamide, and then 0.1 mol of diethanolamine is added, and the temperature is raised to 70° C. to react for 2 h. After the reaction is completed, the mixture is filtered and dried to obtain a first intermediate product; Step A2, under nitrogen conditions, 0.1 mol of the first intermediate product, 1.2 mol of 2,2-dimethylolpropionic acid and p-toluenesulfonic acid were added to a reactor and mixed evenly, and heated to 125° C., reacted for 2 hours, stopped introducing nitrogen, and continued to react for 3 hours under vacuum conditions, and then reacted under reduced pressure for 2 hours. When no water was distilled out, cooled to room temperature, 20 mL of acetone was added, stirred and mixed for 10 minutes, recrystallized, filtered, and dried to obtain a second intermediate product. The amount of p-toluenesulfonic acid used was 0.5% of the total mass of the first intermediate product and 2,2-dimethylolpropionic acid; Step A3, slowly heating the second intermediate product, methyl laurate, dibutyl tin dilaurate and p-hydroxyanisole to 110° C. under stirring, maintaining the top temperature of the fractionation column at 55° C., and maintaining the reaction for 2 hours. After the reaction is completed, vacuum distillation is performed to obtain a hyperbranched polyester, wherein the molar ratio of the second intermediate product to methyl laurate is 1:24, the mass of dibutyl tin dilaurate is 0.3% of the total mass of the second intermediate product and methyl laurate, and the mass of p-hydroxyanisole is 0.001 g; Step A4: Evenly mix 10 mL of epichlorohydrin in 200 mL of methanol, and heat to 55° C., add 2 g of hyperbranched polyester under stirring, and continue stirring for 4 h. Distill under reduced pressure, wash, and dry to obtain the modified hyperbranched polyester.

[0013] The modified PVC resin is prepared by the following steps: Step B1, add 1g of cellulose to 50mL of isopropanol for dispersion, raise the temperature to 60°C for reaction for 10min, then raise the temperature to 80°C, add 0.5g of 1,2-epoxy-5-hexene, continue the reaction for 8h, filter, wash and dry to obtain pre-treated cellulose; Step B2, grind 5g of PVC resin into powder, add 0.2g of dibenzoyl peroxide and 100mL of 1,2-dichloroethane and stir evenly, then add 0.5g of 1-vinylimidazole, heat to 65°C under nitrogen and react for 2h, then add 1g of pretreated cellulose and continue to react for 2h, then add 100mL of methanol, filter, wash and dry to obtain modified PVC resin.

[0014] Example 2 The modified hyperbranched polyester is prepared by the following steps: Step A1, 0.32 mol of triglycidyl isocyanurate was evenly dispersed in 200 mL of N, N-dimethylformamide, and then 0.1 mol of diethanolamine was added, and the temperature was raised to 80° C. to react for 3.5 hours. After the reaction was completed, the mixture was filtered and dried to obtain a first intermediate product; Step A2, under nitrogen conditions, 0.1 mol of the first intermediate product, 1.2 mol of 2,2-dimethylolpropionic acid and p-toluenesulfonic acid were added to a reactor and mixed evenly, and heated to 135° C., reacted for 2.5 hours, stopped introducing nitrogen, and continued to react for 3.5 hours under vacuum conditions, and then reacted under reduced pressure for 2 hours. When no water was distilled out, cooled to room temperature, 30 mL of acetone was added, stirred and mixed for 10 minutes, recrystallized, filtered, and dried to obtain a second intermediate product. The amount of p-toluenesulfonic acid used was 0.5% of the total mass of the first intermediate product and 2,2-dimethylolpropionic acid; Step A3, slowly heating the second intermediate product, methyl laurate, dibutyl tin dilaurate and p-hydroxyanisole to 115° C. under stirring, maintaining the top temperature of the fractionation column at 60° C., and maintaining the reaction for 3.5 hours. After the reaction is completed, vacuum distillation is performed to obtain a hyperbranched polyester, wherein the molar ratio of the second intermediate product to methyl laurate is 1:24, the mass of dibutyl tin dilaurate is 0.35% of the total mass of the second intermediate product and methyl laurate, and the mass of p-hydroxyanisole is 0.0015 g; Step A4: Evenly mix 20 mL of epichlorohydrin in 200 mL of methanol, and heat to 60° C., add 3.5 g of hyperbranched polyester under stirring, and continue stirring for 5 h. Distill under reduced pressure, wash, and dry to obtain modified hyperbranched polyester.

[0015] The modified PVC resin is prepared by the following steps: Step B1, add 2 g of cellulose to 50 mL of isopropanol for dispersion, raise the temperature to 65° C. for reaction for 15 min, then raise the temperature to 85° C., add 1 g of 1,2-epoxy-5-hexene, continue the reaction for 10 h, filter, wash, and dry to obtain pre-treated cellulose; Step B2, grind 7.5g of PVC resin into powder, add 0.3g of dibenzoyl peroxide and 100mL of 1,2-dichloroethane and stir evenly, then add 0.65g of 1-vinylimidazole, heat to 70°C under nitrogen and react for 2.5h, then add 1.5g of pretreated cellulose and continue to react for 2.5h, then add 100mL of methanol, filter, wash and dry to obtain modified PVC resin.

[0016] Example 3 The modified hyperbranched polyester is prepared by the following steps: Step A1, 0.35 mol of triglycidyl isocyanurate is evenly dispersed in 200 mL of N,N-dimethylformamide, and then 0.1 mol of diethanolamine is added, and the temperature is raised to 90° C. to react for 5 hours. After the reaction is completed, the mixture is filtered and dried to obtain a first intermediate product; Step A2, under nitrogen conditions, 0.1 mol of the first intermediate product, 1.2 mol of 2,2-dimethylolpropionic acid and p-toluenesulfonic acid were added to a reactor and mixed evenly, and heated to 145° C., reacted for 3 hours, the nitrogen was stopped, and the reaction was continued for 4 hours under vacuum conditions, and then the reduced pressure reaction was carried out for 2 hours. When no water was distilled out, it was cooled to room temperature, 40 mL of acetone was added, stirred and mixed for 10 minutes, and then recrystallized, filtered and dried to obtain a second intermediate product. The amount of p-toluenesulfonic acid used was 0.5% of the total mass of the first intermediate product and 2,2-dimethylolpropionic acid; Step A3, slowly heating the second intermediate product, methyl laurate, dibutyltin dilaurate and p-hydroxyanisole to 120° C. under stirring, maintaining the top temperature of the fractionation column at 65° C., and maintaining the reaction for 5 hours. After the reaction is completed, vacuum distillation is performed to obtain a hyperbranched polyester, wherein the molar ratio of the second intermediate product to methyl laurate is 1:24, the mass of dibutyltin dilaurate is 0.3%-0.4% of the total mass of the second intermediate product and methyl laurate, and the mass of p-hydroxyanisole is 0.002 g; Step A4: Evenly mix 30 mL of epichlorohydrin in 200 mL of methanol, and heat to 65° C., add 5 g of hyperbranched polyester under stirring, and continue stirring for 6 h. Distill under reduced pressure, wash, and dry to obtain modified hyperbranched polyester.

[0017] The modified PVC resin is prepared by the following steps: Step B1, 3 g of cellulose was dispersed in 50 mL of isopropanol, and the temperature was raised to 70° C. for reaction for 20 min, and then the temperature was raised to 85° C., and 2 g of 1,2-epoxy-5-hexene was added, and the reaction was continued for 12 h, and then filtered, washed, and dried to obtain pre-treated cellulose; Step B2, grind 10g of PVC resin into powder, add 0.4g of dibenzoyl peroxide and 100mL of 1,2-dichloroethane and stir evenly, then add 0.8g of 1-vinylimidazole, heat to 5°C under nitrogen and react for 3h, then add 2g of pretreated cellulose and continue to react for 3h, then add 100mL of methanol, filter, wash and dry to obtain modified PVC resin.

[0018] Example 4 A production process of medical PVC pump tube material comprises the following steps: 100 parts of the modified PVC resin prepared in Example 1, 8 parts of polyurethane elastomer, 35 parts of tributyl citrate, 5 parts of the modified hyperbranched polyester prepared in Example 1, 0.5 parts of calcium zinc composite stabilizer, 0.5 parts of antioxidant 1076, and 0.1 parts of stearic acid; The raw materials were weighed in parts by weight, and the modified PVC resin prepared in Example 1, polyurethane elastomer, tributyl citrate, modified hyperbranched polyester prepared in Example 1, calcium zinc composite stabilizer, antioxidant 1076 and stearic acid were added into a twin-screw extruder in sequence. After extrusion, granulation and air-cooling, medical PVC pump tube material was obtained. The processing temperature of the twin-screw extruder was 60° C. for section 1, 100° C. for section 2, 80° C. for section 3, 100° C. for section 4 and 115° C. for section 5.

[0019] Example 5 A production process of medical PVC pump tube material comprises the following steps: 100 parts of the modified PVC resin prepared in Example 2, 12 parts of polyurethane elastomer, 45 parts of tributyl citrate, 8 parts of the modified hyperbranched polyester prepared in Example 2, 0.8 parts of calcium zinc composite stabilizer, 1 part of antioxidant 1076, and 0.3 parts of stearic acid; The raw materials were weighed in parts by weight, and the modified PVC resin prepared in Example 2, polyurethane elastomer, tributyl citrate, modified hyperbranched polyester prepared in Example 2, calcium zinc composite stabilizer, antioxidant 1076 and stearic acid were added into a twin-screw extruder in sequence. After extrusion, granulation and air-cooling, medical PVC pump tube material was obtained. The processing temperature of the twin-screw extruder was 65° C. for section 1, 105° C. for section 2, 85° C. for section 3, 115° C. for section 4 and 120° C. for section 5.

[0020] Example 6 A production process of medical PVC pump tube material comprises the following steps: 100 parts of the modified PVC resin prepared in Example 3, 15 parts of polyurethane elastomer, 55 parts of tributyl citrate, 10 parts of the modified hyperbranched polyester prepared in Example 3, 1 part of calcium zinc composite stabilizer, 1.5 parts of antioxidant 1076, and 0.5 parts of stearic acid; The raw materials were weighed in parts by weight, and the modified PVC resin prepared in Example 3, polyurethane elastomer, tributyl citrate, modified hyperbranched polyester prepared in Example 3, calcium zinc composite stabilizer, antioxidant 1076 and stearic acid were added into a twin-screw extruder in sequence. After extrusion, granulation and air-cooling, medical PVC pump tube material was obtained. The processing temperature of the twin-screw extruder was 70°C for section 1, 110°C for section 2, 90°C for section 3, 110°C for section 4 and 125°C for section 5.

[0021] Comparative Example 1 This comparative example is a PVC pump tube material, which differs from Example 6 in that PVC resin is used instead of the modified PVC resin prepared in Example 3, and the rest are the same.

[0022] Comparative Example 2 This comparative example is a PVC pump tube material, which differs from Example 6 in that commercially available hyperbranched polyester is used instead of the modified hyperbranched polyester prepared in Example 3, and the rest are the same.

[0023] The PVC pump tube materials of Examples 4-6 and Comparative Examples 1-2 were subjected to performance tests: Mechanical properties test: tensile strength and elongation at break were determined according to D412-98a; Antibacterial performance test: Tested according to the method of GB / T 31402-2015; Contact angle test: The water contact angle tester tests the water contact angle on the surface of the PVC pump tube material. Before the test, use filter paper to absorb the water on the surface of the sheet; Biocompatibility test: carried out in accordance with the requirements of GB16886; The test results are shown in the following table: It can be seen from the above table that the PVC pump tube material in the present invention has excellent mechanical properties, antibacterial properties, hydrophilicity and biocompatibility.

[0024] The above contents are merely examples and explanations of the concept of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they shall all fall within the protection scope of the present invention.

Claims

1. A medical PVC pump tube material, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of modified PVC resin, 8-15 parts of polyurethane elastomer, 35-55 parts of plasticizer, 5-10 parts of modified hyperbranched polyester, 0.5-1 parts of heat stabilizer, 0.5-1.5 parts of antioxidant and 0.1-0.5 parts of lubricant; The modified hyperbranched polyester is prepared by the following steps: Step A1, dispersing triglycidyl isocyanurate evenly in N,N-dimethylformamide, adding diethanolamine, and heating to 70-90° C. to react for 2-5 hours. After the reaction is completed, filtering and drying are performed to obtain a first intermediate product; Step A2, under nitrogen conditions, the first intermediate product, 2,2-dihydroxymethylpropionic acid and p-toluenesulfonic acid are added to a reactor and mixed evenly, and heated to 125-145° C., reacted for 2-3 hours, the nitrogen is stopped, and the reaction is continued for 3-4 hours under vacuum conditions, and then the reaction is reduced in pressure for 2 hours. When no water is distilled out, it is cooled to room temperature, 20-40 mL of acetone is added, stirred and mixed for 10 minutes, and then recrystallized, filtered, and dried to obtain a second intermediate product; Step A3, slowly heating the second intermediate product, methyl laurate, dibutyltin dilaurate and p-hydroxyanisole to 110-120° C. under stirring, maintaining the top temperature of the fractionation column at 55-65° C., and keeping the reaction for 2-5 hours. After the reaction is completed, distilling under reduced pressure to obtain a hyperbranched polyester; Step A4, epichlorohydrin is mixed evenly in methanol, and the temperature is raised to 55-65° C., hyperbranched polyester is added under stirring, and stirring is continued for 4-6 hours, and vacuum distillation, washing, and drying are performed to obtain modified hyperbranched polyester.

2. A medical PVC pump tube material according to claim 1, characterized in that: In step A1, the usage ratio of triglycidyl isocyanurate, N,N-dimethylformamide and diethanolamine is 0.3-0.35 mol:200 mL:0.1 mol.

3. A medical PVC pump tube material according to claim 1, characterized in that: In step A2, the molar ratio of the first intermediate product to 2,2-dimethylolpropionic acid is 1:12, and the amount of p-toluenesulfonic acid used is 0.5% of the total mass of the first intermediate product and 2,2-dimethylolpropionic acid.

4. A medical PVC pump tube material according to claim 1, characterized in that: In step A3, the molar ratio of the second intermediate product to methyl laurate is 1:24, the mass of dibutyltin dilaurate is 0.3%-0.4% of the total mass of the second intermediate product and methyl laurate, and the mass of p-hydroxyanisole is 0.001-0.002g.

5. A medical PVC pump tube material according to claim 1, characterized in that: In step A4, the usage ratio of epichlorohydrin, hyperbranched polyester and methanol is 10-30 mL: 2-5 g: 200 mL.

6. A medical PVC pump tube material according to claim 1, characterized in that: The modified PVC resin is prepared by the following steps: Step B1, adding cellulose to isopropanol for dispersion, raising the temperature to 60-70°C for reaction for 10-20 minutes, then raising the temperature to 80-85°C, adding 1,2-epoxy-5-hexene, and continuing the reaction for 8-12 hours, then filtering, washing, and drying to obtain pre-treated cellulose; Step B2, grind the PVC resin into powder, add dibenzoyl peroxide and 1,2-dichloroethane and stir evenly, then add 1-vinylimidazole, heat to 65-75°C under nitrogen and react for 2-3h, then add pretreated cellulose and continue to react for 2-3h, then add methanol, filter, wash and dry to obtain modified PVC resin.

7. A medical PVC pump tube material according to claim 6, characterized in that: In step B1, the usage ratio of cellulose, isopropanol and 1,2-epoxy-5-hexene is 1-3 g:50 mL:0.5-2 g.

8. A medical PVC pump tube material according to claim 6, characterized in that: In step B2, the usage ratio of PVC resin, dibenzoyl peroxide, 1,2-dichloroethane, 1-vinylimidazole, pre-treated cellulose and methanol is 5-10 g: 0.2-0.4 g: 100 mL: 0.5-0.8 g: 1-2 g: 100 mL.

9. The production process of a medical PVC pump tube material according to claim 1, characterized in that: The following steps are involved: The raw materials are weighed in parts by weight, and the modified PVC resin, polyurethane elastomer, plasticizer, modified hyperbranched polyester, heat stabilizer, antioxidant and lubricant are sequentially added into a twin-screw extruder, and the medical PVC pump tube material is obtained through extrusion, granulation and air cooling.

10. The production process of a medical PVC pump tube material according to claim 9, characterized in that: The processing temperature of the twin-screw extruder is 60-70°C for stage 1, 100-110°C for stage 2, 80-90°C for stage 3, 100-110°C for stage 4, and 115-125°C for stage 5.

Citation Information

Patent Citations

  • Polymer absorbent with enhanced polydimethylsiloxane modified cellulose and preparation method thereof

    CN104987466A

  • Application of hyperbranched polyester to plastic processing

    CN105331078A

  • UV-cured water-based silicon-containing polyurethane and preparation method thereof

    CN114853975A

  • De-charge black rubber tube and preparation method thereof

    CN116199985A

  • Anti-aging PVC (polyvinyl chloride) colloidal particles and preparation method thereof