Modified yellow pigment as well as preparation method and application thereof

By kneading with acrylic resin and pigment 74 derivatives in yellow pigment, combined with iron removal and metal ion removal steps, the problems of yellow pigment agglomeration and metal residue are solved, brightness and contrast are improved, and the high response speed of the liquid crystal display is met Require.

CN118956178AActive Publication Date: 2024-11-15SHANDONG KAIRUIER OPTOELECTRONICS TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411042495.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Existing yellow pigments are prone to agglomeration when grinding and dispersing, resulting in large dispersion particle size, low brightness, low contrast, and metal ions such as sodium and iron are prone to fall off during kneading, affecting the response speed of the liquid crystal display.

Method used

Acrylic resin and pigment 74 derivatives are used as collaborative agents, kneading and post-treatment steps, including iron removal and metal ion removal, and the use of ethylenediaminetetraacetic acid disodium salt to form a stable water-soluble complex to reduce metal residue.

Benefits of technology

It improves the dispersion and particle size of yellow pigments, enhances brightness and contrast, and effectively reduces the metal ion content, meeting the high response speed requirements of liquid crystal displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention belongs to the technical field of display materials, and relates to a modified yellow pigment and a preparation method and application thereof, the modified yellow pigment comprises a yellow pigment, acrylic resin and a pigment 74 derivative; the yellow pigment is C.I. Pigment yellow 138; the molecular weight of the acrylic resin is 9000, the acid value is 125, and the solid content is 30%; pigment 74 derivatives. According to the modified yellow pigment disclosed by the invention, the acrylic resin and the pigment 74 derivative are added during kneading, so that the brightness and contrast of a color paste film formed by the pigment are improved; the pigment 74 derivative is a solid, the shear friction force of salt is increased in the kneading process, and kneading modification of the yellow pigment is facilitated; in the post-treatment process, an iron removal process is added, an iron remover is used for removing iron for the first time, HCl and EDTA disodium salt are added, hydrochloric acid is used for converting metal into metal ions, then EDTA disodium salt is added, a stable water-soluble complex is formed and removed along with water, and the metal content in the pigment is reduced to the minimum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of display materials, and in particular relates to a modified yellow pigment and a preparation method and application thereof. Background Art

[0002] Liquid Crystal Display (LCD) is a display technology that uses the properties of liquid crystal materials. LCD is widely used in various display devices, such as TVs, computer monitors, mobile phones, and smart wearable devices. With the continuous development and progress of science and technology, LCD technology is also continuously improving, moving towards higher resolution, lower energy consumption, faster response speed, and more intelligent functions.

[0003] Color filter is a key component of LCD. It forms red, green and blue patterns on transparent substrates such as glass. In order to form red and green coloring patterns, it is difficult to obtain the desired spectroscopic spectrum with only red or green pigments, so yellow pigment is mixed to adjust the spectroscopic spectrum. In order to achieve high transparency and high contrast, in addition to strict requirements on the basic red and green pigments in the color paste in the photoresist, the yellow pigment for color matching is required to be pure in color, small in particle size, stable in viscosity, and high in brightness and contrast after film formation.

[0004] When the commercially available yellow Y-138 pigment is ground and dispersed, the pigments will agglomerate due to the attraction between the pigments, resulting in a large dispersed particle size, a non-transparent liquid, low brightness (Y value), and low contrast. Even if too much dispersing aid is added during the dispersion process, it is still impossible to achieve a small particle size dispersed transparent stable state. Therefore, directly using the commercially available ordinary yellow pigment to prepare the color paste and photoresist composition cannot meet the Y value and contrast requirements and cannot be used directly. In order to improve the Y value and contrast of the ordinary yellow pigment to prepare the color paste and photoresist composition to meet the requirements, most of them currently use the kneading method for surface treatment. For the kneading of yellow pigments, salt and solvent are generally added in a kneading machine. However, although the performance is improved by directly using the kneading method of adding salt and solvent, too much dispersant needs to be added during the grinding and dispersion to achieve a stable dispersion effect. However, too much dispersant not only affects the adjustable range of the photoresist, but also affects the process dominance, so it still cannot meet the requirements of the pigment used in the display liquid crystal industry.

[0005] Chinese patent CN113881245B discloses a modified yellow pigment for photoresist, its preparation method and application, wherein a dispersant TSP (tristyrylphenol polyoxyethylene ether) is added during kneading to obtain a yellow pigment that is easy to grind and disperse, thereby ensuring that the prepared color paste has a smaller particle size and obtains a high contrast. Chinese patent CN111732840B discloses a modified yellow pigment for photoresist, its preparation method and application, wherein a dispersant DSS (sodium dioctyl sulfosuccinate) is added during kneading, and during the kneading process, DSS can be well attached to the surface of the pigment crushed by NaCl, increasing the repulsion stability between particles, making the pigment particle size more uniform and stable after kneading, thereby ensuring that the prepared color paste has a smaller particle size and obtains a high contrast. The above patents all optimize the effect of the kneading material by adding a dispersant during kneading, and the final yellow pigment can be more easily dispersed after being prepared into a color paste, and the optical values ​​after film formation are better.

[0006] In addition, the control of metal content in the pigment is also critical. If the metal content in the pigment is too high, especially sodium and iron, after the pigment is made into color paste, photoresist film and filter, the sodium and iron content is too high, which will affect the movement of liquid crystal and ultimately affect the response speed of the display. In the process of kneading yellow pigment, a large amount of salt is used. In addition to sodium ions, there are also sodium and iron ions in the salt. During the kneading process, the pigment and salt squeeze and rub, which will also cause the metal on the inner cavity wall to fall off. Therefore, it is necessary to reduce the content of metal and metal ions while improving brightness and contrast. Summary of the invention

[0007] In view of the deficiencies of the above-mentioned prior art, the present invention provides a modified yellow pigment and a preparation method and application thereof. The specific technical scheme is as follows:

[0008] The first object of the present invention is to provide a modified yellow pigment, comprising a yellow pigment, an acrylic resin and a pigment 74 derivative; the yellow pigment is CI Pigment Yellow 138; the structural formula of the pigment 74 derivative is shown in formula (1):

[0009]

[0010] The modified yellow pigment of the present invention is added with a pigment 74 derivative, which can be used as a synergist of the yellow pigment. The polarity of the acidic group is applied to the surface of the yellow pigment, and it is easy to connect with the surface of the yellow pigment. This polar group makes the pigment difficult to agglomerate. When preparing the color paste, the pigment 74 derivative and the dispersant are very easy to mix. The pigment 74 derivative is used in combination with the acrylic resin to make the final color paste particle size small, the yellow pigment is well dispersed, and the brightness and contrast are effectively improved.

[0011] Furthermore, the acrylic resin has a molecular weight of 9000, an acid value of 125, and a solid content of 30%.

[0012] Furthermore, the modified yellow pigment comprises, by weight, 100 parts of yellow pigment, 6 to 35 parts of acrylic resin and 2 to 10 parts of pigment 74 derivative.

[0013] The second object of the present invention is to provide a method for preparing the modified yellow pigment, wherein the modified yellow pigment is prepared by heating and kneading a kneaded material of yellow pigment, acrylic resin, pigment 74 derivative, salt and diethylene glycol (DEG), and then post-treating the kneaded material.

[0014] Furthermore, the mass ratio of the yellow pigment, the salt and diethylene glycol is 1:(4-15):(1-4).

[0015] Furthermore, the kneading temperature is 50 to 90° C., preferably 60 to 80° C., and the kneading time is 30 to 50 hours, preferably 35 to 45 hours.

[0016] Furthermore, the post-treatment method of the modified yellow pigment kneaded material comprises the following steps:

[0017] (1) Dispersing the kneaded material into slurry: Put the kneaded material into a dispersion barrel, add hot pure water to soak and stir to disperse until the material has no agglomerates and becomes slurry;

[0018] (2) Preliminary iron removal of slurry: The slurry enters the iron remover for circulation and is initially iron-removed by magnetic force;

[0019] (3) Secondary iron removal of slurry: Add hydrochloric acid to the slurry and stir to remove iron for the second time;

[0020] (4) Preliminary desalination and acid removal of slurry: The slurry after secondary iron removal is allowed to stand, the supernatant is extracted, and hot pure water is added. This process is repeated twice to complete the preliminary desalination and acid removal.

[0021] (5) Fine removal of metal ions from slurry: Add disodium ethylenediaminetetraacetic acid to the slurry stirred with hot pure water, stir and disperse, let stand, and extract the supernatant;

[0022] (6) Pigment cleaning: Add hot pure water again to stir and disperse the material, filter the dispersed slurry, and use pure water to filter and clean the material until the conductivity of the water discharged from the filter is the same as the initial conductivity of the pure water. Then remove the filter cake and put it into a dispersion barrel. Add hot pure water again to stir and disperse it into slurry. The dispersed slurry is circulated through the iron remover to remove iron again and then enters the plate and frame filter until the conductivity of the filter discharge is the same as the initial conductivity of the pure water. Remove the filter cake and the cleaning is completed;

[0023] (7) Drying: Drying and crushing the filter cake to obtain a modified yellow pigment.

[0024] If the metal content in the pigment is too high, especially sodium and iron, after the pigment is made into color paste and photoresist film is made into filter, the sodium and iron content is too high, which will affect the movement of liquid crystal and ultimately affect the response speed of the display. Disodium ethylenediaminetetraacetic acid is an important complexing agent that can form stable water-soluble complexes with alkaline earth metals, rare earth elements and transition metals. In the present invention, its role is to absorb the metal contained in the salt to form a water-soluble metal complex in the kneading process, dissolve in water and disappear in the washing process, and avoid metal residues in the pigment.

[0025] Furthermore, the temperature of the hot pure water is 60-70°C.

[0026] Furthermore, in the step (1), the stirring speed of the dispersion is 300 to 500 rpm, and the dispersion time is not less than 2 hours.

[0027] Furthermore, in the step (3), after the hydrochloric acid is added, the concentration of hydrochloric acid in the slurry is 1%, and the slurry is stirred for 3 to 4 hours.

[0028] Furthermore, in the step (5), the amount of disodium ethylenediaminetetraacetic acid added is 3-5% of the mass of the modified yellow pigment, and the dispersion time is not less than 1 hour.

[0029] The third object of the present invention is to provide the use of the modified yellow pigment in the preparation of yellow color paste.

[0030] Furthermore, the yellow color paste, by mass, comprises 10 parts of modified yellow pigment; 15-20 parts of resin; 5-12 parts of dispersant; 55-75 parts of solvent; the resin is an acrylic resin with a molecular weight of 3000-10000 and an acid value of 80-130.

[0031] Furthermore, the dispersant is a polymer dispersant, which may be BYK-2001, BYK-2000, BYK-2025, BYK-2050, BYK-2070, BYK-2150, BYK-167, BYK-168, BYK-170, BYK-171, BYK-181, BYK-182, etc.

[0032] Furthermore, the solvent is an organic solvent, and one or more of ether organic solvents and ether ester organic solvents can be selected, specifically ether organic solvents, such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol ethyl ether, propylene glycol butyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, etc.; ether ester organic solvents, such as ethylene glycol methyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, etc.

[0033] The beneficial effects of the present invention are:

[0034] The modified yellow pigment of the present invention improves the brightness and contrast of the pigment after being made into a color paste and film-forming by adding acrylic resin and pigment 74 derivatives during kneading; the pigment 74 derivative is solid, and the shear friction of the salt is increased during kneading, which is beneficial to the kneading modification of the yellow pigment; an iron removal process is added in the post-treatment, firstly the iron is removed once by an iron remover, and HCl and EDTA disodium salt are also added, the hydrochloric acid is used to convert the metal into metal ions, and then EDTA disodium salt is added to form a stable water-soluble complex, which is removed with water, so that the metal content in the pigment is reduced to the minimum. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a particle size diagram of the yellow color paste in Application Example 1 of the present invention;

[0036] Figure 2 This is a particle size diagram of the yellow color paste in Application Example 2 of the present invention;

[0037] Figure 3 This is a particle size diagram of the yellow color paste in Application Example 3 of the present invention;

[0038] Figure 4 This is a diagram of the particle size of the yellow color paste in comparative application example 1 of the present invention. DETAILED DESCRIPTION

[0039] The principles and features of the present invention are described below in conjunction with examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0040] Pigment 74 derivative: The trade name is PY74ASA-2, produced by KISCO Company of Korea.

[0041] Embodiment 1:

[0042] Preparation of a modified yellow pigment:

[0043] Kneading modification: In a 5-liter Inoue three-arm planetary mixer, 1700 parts of salt, 200 parts of CI Pigment Yellow 138, 4 parts of Pigment 74 derivative, 40 parts of acrylic resin (molecular weight 9000, acid value 125, solid content 30%), and 500 parts of DEG were added by mass, and the kneading temperature was controlled at 70°C and the kneading time was 40 hours to obtain a kneaded material;

[0044] Post-processing:

[0045] (1) Dispersing the kneaded material into a slurry: Put the kneaded material into a dispersion barrel, add 60-70°C hot pure water to soak and stir to disperse, the dispersion speed is 400 rpm, and the dispersion time is not less than 2 hours, until the material has no agglomerates and becomes a slurry;

[0046] (2) Preliminary iron removal of slurry: The slurry enters the 10000GS iron remover for circulation for 2 hours, and preliminary iron removal is performed by magnetic force;

[0047] (3) Secondary iron removal of slurry: Add hydrochloric acid to the slurry to make the overall hydrochloric acid concentration 1%, and stir for 4 hours to further remove iron from the pigment;

[0048] (4) Preliminary desalination and acid removal of slurry: The slurry after secondary iron removal is allowed to stand, the supernatant is extracted, and hot pure water is added. This process is repeated twice to complete the preliminary desalination and acid removal.

[0049] (5) Fine removal of metal ions from slurry: Add 5% of the modified yellow pigment disodium EDTA to the slurry stirred with hot pure water and stir and disperse for a dispersion time of not less than 1 hour. After the dispersion is completed, let it stand and extract the supernatant;

[0050] (6) Pigment cleaning: Add hot pure water again to stir and disperse the material. The dispersed slurry enters the plate and frame filter. Use pure water to filter and clean the material until the conductivity of the water discharged from the filter is the same as the initial conductivity of the pure water. Then remove the filter cake and put it into a dispersion barrel. Add hot pure water again to stir and disperse it into slurry. The dispersed slurry is circulated through the iron remover to remove iron again and then enters the plate and frame filter until the conductivity of the filter discharge is the same as the initial conductivity of the pure water. Remove the filter cake and the cleaning is completed; (pure water conductivity <2us / cm);

[0051] (7) Drying: The material to be dried is evenly spread on a tray and dried at 100°C for 24 hours. Check to confirm whether the material is dry. The dried material is crushed in a crusher to obtain modified yellow pigment Y-N1.

[0052] Embodiment 2:

[0053] Preparation of a modified yellow pigment:

[0054] Kneading modification: by weight, 2400 parts of salt, 200 parts of CI Pigment Yellow 138, 16 parts of Pigment 74 derivative, 26.7 parts of acrylic resin (molecular weight of 9000, acid value of 125, solid content of 30%), and 400 parts of DEG were added into a 5-liter Inoue three-arm planetary mixer, and the kneading temperature was controlled at 70° C. and the kneading time was 40 h to obtain a kneaded material;

[0055] The post-treatment is the same as in Example 1 and will not be repeated here to obtain a modified yellow pigment Y-N2.

[0056] Embodiment 3:

[0057] Preparation of a modified yellow pigment:

[0058] Kneading modification: In a 5-liter Inoue three-arm planetary mixer, 1000 parts of salt, 200 parts of CI Pigment Yellow 138, 10 parts of Pigment 74 derivative, 53.3 parts of acrylic resin (molecular weight 9000, acid value 125, solid content 30%), and 400 parts of DEG were added by mass, and the kneading temperature was controlled at 70°C and the kneading time was 40 hours to obtain a kneaded material;

[0059] The post-treatment is the same as in Example 1 and will not be repeated here to obtain a modified yellow pigment Y-N3.

[0060] Comparative Example 1:

[0061] Preparation of a yellow pigment:

[0062] Kneading: by weight, add 1700 parts of salt, 200 parts of CI Pigment Yellow 138, and 500 parts of DEG into a 5-liter Inoue three-arm planetary mixer, control the kneading temperature to 70°C, and knead for 40 hours to obtain a kneaded material;

[0063] The post-treatment was the same as in Example 1 and will not be described again, to obtain a modified yellow pigment YN-D1.

[0064] Comparative Example 2:

[0065] Preparation of a modified yellow pigment:

[0066] Kneading modification: the same as in Example 1, which will not be described again, to obtain a kneaded material;

[0067] Post-processing:

[0068] (1) Dispersing the kneaded material into a slurry: Put the kneaded material into a dispersion barrel, add hot pure water to soak and stir to disperse, the dispersion speed is 400 rpm, and the dispersion time is not less than 2 hours, until the material has no agglomerates and becomes a slurry;

[0069] (2) Initial desalination of slurry: let the slurry stand, extract the supernatant, and then add hot pure water. Repeat this process twice to complete the initial desalination.

[0070] (3) Pigment cleaning: Add hot pure water again to stir and disperse the material, and the dispersed slurry enters the plate and frame filter, and uses pure water to filter and clean the material until the conductivity of the water discharged from the filter is the same as the initial conductivity of the pure water. Then remove the filter cake and put it into a dispersion barrel, add hot pure water again to stir and disperse it into slurry, and the dispersed slurry enters the plate and frame filter again until the conductivity of the water discharged from the filter is the same as the initial conductivity of the pure water. Remove the filter cake and the cleaning is completed;

[0071] (4) Drying: The material to be dried is evenly spread on a tray and dried at 100°C for 24 hours. Check to confirm whether the material is dry. The dried material is crushed in a crusher to obtain modified yellow pigment YN-D2.

[0072] Application Example 1:

[0073] A yellow color paste preparation: 10g of modified yellow pigment Y-N1, 9.6g of dispersant BYK-2001, 16.7g of acrylic resin (molecular weight 3000-10000, acid value 80-130), and 63.7g of propylene glycol methyl ether acetate solvent are added to a grinder, and a 0.1mm zirconium ball is added. The grinding time is 24h. After grinding, a yellow color paste is obtained, and the particle size and viscosity are tested;

[0074] Film formation evaluation: yellow color paste: acrylic resin (molecular weight 3000-10000, acid value 80-130) = 5:0.5, and use a spin coater to spin coat on the glass surface to form a film. Pre-bake at 90°C for 90s on a front baking plate, and then post-bake at 230°C for 20min. After film formation, perform brightness (Y) and contrast tests.

[0075] Application Example 2:

[0076] This application example uses modified yellow pigment Y-N2, and the rest is the same as that of application example 1, which will not be described again here.

[0077] Application Example 3:

[0078] This application example uses modified yellow pigment Y-N3, and the rest is the same as that of application example 1, which will not be described again here.

[0079] Comparative application example 1:

[0080] This application example uses the modified yellow pigment YN-D1, and the rest is the same as that of application example 1, which will not be described again here.

[0081] Comparative application example 2:

[0082] This application example uses the modified yellow pigment YN-D2, and the rest is the same as that of application example 1, which will not be described again here.

[0083] Test methods and results:

[0084] Y value test: using high-precision color analyzer, model: HACA-3650;

[0085] Contrast test: using contrast meter, model CT-1;

[0086] Particle size test: using particle size analyzer, model: 90Plus Pals;

[0087] Viscosity test: using viscometer, model: LVDV-2T;

[0088] Fe, Na test: using ICP-OES method.

[0089] The test results are shown in Table 1 and Table 2:

[0090] Table 1 Application examples and comparative application examples Test results of yellow color paste and film performance after film formation

[0091]

[0092] Table 2 Table of sodium iron content in modified yellow pigment of Example 1 and Comparative Example 2

[0093]

[0094] From the results in Table 1, it can be seen that in Comparative Application Example 1, direct kneading is used, and although the Y value and contrast are improved, they still cannot meet the requirements; the particle size of the color paste prepared in the application example is small, and after film formation, the brightness and contrast are greatly improved, indicating that the addition of acrylic resin and pigment 74 derivatives during kneading improves the brightness and contrast of the color paste made of the pigment after film formation, and the effect is obvious.

[0095] From the results in Table 2, it can be seen that the iron and sodium contents in the modified yellow pigment are significantly reduced by using an iron remover and adding hydrochloric acid and disodium EDTA.

[0096] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A modified yellow pigment, characterized in that: It comprises a yellow pigment, an acrylic resin and a pigment 74 derivative; the yellow pigment is CI Pigment Yellow 138; the structural formula of the pigment 74 derivative is shown in formula (1):

2. The modified yellow pigment according to claim 1, characterized in that The modified yellow pigment comprises, by weight, 100 parts of yellow pigment, 6 to 35 parts of acrylic resin, and 2 to 10 parts of pigment 74 derivative.

3. A method for preparing a modified yellow pigment as claimed in claim 1 or 2, characterized in that: The modified yellow pigment is prepared by heating and kneading a yellow pigment, an acrylic resin, a pigment 74 derivative, a salt and diethylene glycol, and then post-treating the kneaded material.

4. The preparation method of modified yellow pigment according to claim 3, characterized in that, The mass ratio of the yellow pigment, the salt and the diethylene glycol is 1:(4-15):(1-4).

5. The preparation method of modified yellow pigment according to claim 3, characterized in that, The kneading temperature is 50-90° C., and the kneading time is 30-50 hours.

6. The method for preparing the modified yellow pigment according to claim 3, characterized in that: The post-treatment method of the modified yellow pigment kneaded material comprises the following steps: (1) Dispersing the kneaded material into slurry: Put the kneaded material into a dispersion barrel, add hot pure water to soak and stir to disperse until the material has no agglomerates and becomes slurry; (2) Preliminary iron removal of slurry: The slurry enters the iron remover for circulation and is initially iron-removed by magnetic force; (3) Secondary iron removal of slurry: Add hydrochloric acid to the slurry and stir to remove iron for the second time; (4) Preliminary desalination and acid removal of slurry: The slurry after secondary iron removal is allowed to stand, the supernatant is extracted, and hot pure water is added. This process is repeated twice to complete the preliminary desalination and acid removal. (5) Fine removal of metal ions from slurry: Add disodium ethylenediaminetetraacetic acid to the slurry stirred with hot pure water, stir and disperse, let stand, and extract the supernatant; (6) Pigment cleaning: Add hot pure water again to stir and disperse the material, filter the dispersed slurry, and use pure water to filter and clean the material until the conductivity of the water discharged from the filter is the same as the initial conductivity of the pure water. Then remove the filter cake and put it into a dispersion barrel. Add hot pure water again to stir and disperse it into slurry. The dispersed slurry is circulated through the iron remover to remove iron again and then enters the plate and frame filter until the conductivity of the filter discharge is the same as the initial conductivity of the pure water. Remove the filter cake and the cleaning is completed; (7) Drying: Drying and crushing the filter cake to obtain a modified yellow pigment.

7. The method for preparing the modified yellow pigment according to claim 6, characterized in that: In the step (1), the stirring speed of the dispersion is 300 to 500 rpm, and the dispersion time is not less than 2 hours.

8. The method for preparing the modified yellow pigment according to claim 6, characterized in that: In the step (3), after adding hydrochloric acid, the concentration of hydrochloric acid in the slurry is 1%, and stirring is carried out for 3 to 4 hours.

9. The modified yellow pigment according to claim 6, characterized in that In the step (5), the amount of disodium ethylenediaminetetraacetic acid added is 3-5% of the mass of the modified yellow pigment, and the dispersion time is not less than 1 hour.

10. Use of the modified yellow pigment according to claim 1 or 2 in preparing yellow color paste.

Citation Information

Patent Citations

  • Method for deep desalting of pigment

    CN104031435A

  • Solid pigment particle as well as preparation method and application thereof

    CN111454529A

  • Modified yellow pigment for photoresist and preparation method and application thereof

    CN111732840A

  • Yellow pigment for color photoresist, modification method of yellow pigment, yellow color paste containing yellow pigment, color photoresist and optical filter

    CN113817339A

  • Modified yellow pigment for photoresist as well as preparation method and application of modified yellow pigment