Controllable heat absorption VO2 (at) MXene / epoxy resin anti-corrosion composite coating and preparation method thereof
By introducing VO2@MXene into the epoxy resin coating, a VO2@Ti3C2Tx MXene/epoxy resin anti-corrosion composite coating with controllable photothermal performance is solved, and the corrosion resistance of the epoxy resin coating in high temperature and high salt environment is insufficient. The problem has achieved long-term anti-corrosion and light-thermal balance.
Patent Information
- Application Number
- CN202410863350.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-29
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-06-29
AI Technical Summary
Existing epoxy resin coatings are prone to microcracks and hole defects during long-term use, resulting in O2, Cl-, and H+ plasma penetration, reducing their anticorrosion performance, especially in high-temperature and high-salt environments that cannot be anticorrosive for a long time.
Using VO2@MXene/epoxy resin anti-corrosion composite coating, a single layer of Ti3C2Tx MXene was prepared by LiF and Ti3AlC2. The mechanical stability was improved by polydopamine coating treatment, and M-phase VO2 nanoparticles were loaded on the surface of Ti3C2Tx MXene, combined with hyperbranching. Amide compounds and bisphenol A diglycidyl ether are sprayed to form a coating with controlled photothermal properties.
It extends the service life of the coating and maintains high corrosion resistance, especially in marine environments and high salt solutions. It also reduces the coating temperature under light and improves the adhesion between the coating and the substrate. .
Smart Images

Figure CN118956233A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of polymer composite materials, and in particular relates to a controllable heat-absorbing VO2@MXene / epoxy resin anti-corrosion composite coating and a preparation method thereof. Background Art
[0002] The epoxy resin molecular structure contains active epoxy groups (-CH(O)CH-), which can react chemically with the curing agent to form a dense cross-linked network. This network structure can effectively isolate the outside air, moisture and chemicals, prevent electrochemical corrosion on the metal surface, and the surface film formed can effectively prevent mechanical wear and impact, and protect the substrate from damage by external physical factors. However, during the long-term use of a single epoxy resin coating, it is inevitably damaged by external factors, resulting in defects such as microcracks and holes in the coating. These defects cause O2, Cl - , H + Plasma can penetrate epoxy coatings through defects, thus reducing their corrosion protection.
[0003] Existing studies have shown that two-dimensional materials can be doped into epoxy resins as a physical barrier to effectively prevent the penetration of corrosive media, while also improving the mechanical properties of epoxy resins. MXene is an emerging class of two-dimensional materials with excellent photothermal conversion capabilities and electrochemical energy storage capabilities. Its local surface plasma resonance impact characteristics enable it to absorb photons in the visible and infrared regions, which are the main components of light waves. For example, Wang et al. disclosed the use of MXene's excellent internal photo-thermal conversion properties to prepare self-floating MXene films and used them in water evaporation systems. However, the direct use of MXene in self-healing coatings will cause the coating to be heated for a long time, which is not conducive to the long-term corrosion protection of the coating. Because the coating is exposed to sunlight for a long time during daily use, Ti3C2T x The heat absorption of MXene materials will lead to a decrease in the mechanical properties of the coating, and will also reduce the adhesion between the coating and the substrate, causing the coating to fall off.
[0004] Photothermal conversion is a method of utilizing solar energy, which involves collecting and converting solar radiation from photothermal materials into heat as terminal energy for beneficial use. Vanadium dioxide (VO2) is a typical strongly correlated transition metal oxygen that can undergo a first-order metal-insulator phase transition (MIPT) at an accessible temperature of 68°C. This phase transition process is accompanied by a significant change in resistivity, making VO2 have potential application value in smart windows, optoelectronic devices and other fields. For example, Wang (Q. Wang, W. Yang, C. Tao, et al. T-shaped tunable infrared optical switch based on vanadium dioxide with dual-wavelength channels [J]. Optics & Laser Technology, 2024, 168: 109972.) et al. proposed a T-shaped tunable infrared optical switch based on a plasma structure composed of metal nanorods and vanadium dioxide thin films to achieve modulation of wavelength and spectral reflection intensity.
[0005] In recent years, scholars have proposed that the anti-corrosion performance of epoxy coatings can be improved by increasing the tortuosity of the diffusion path of the corrosive medium, inhibiting the reaction between the corrosive medium and the metal substrate, increasing the hydrophobicity of the coating, and timely repairing the damaged coating. However, considering the service environment of the coating, the traditional anti-corrosion coating cannot meet the long-term anti-corrosion requirements in a high temperature and high salt environment. Therefore, the preparation of an efficient and controllable heat-absorbing anti-corrosion coating will become a future development trend and focus. Summary of the invention
[0006] In view of the technical problems existing in the background technology, the purpose of the present invention is to provide a controllable heat-absorbing VO2@MXene / epoxy resin anti-corrosion composite coating and a preparation method thereof. The VO2@MXene / epoxy resin anti-corrosion composite coating has good controllable photothermal performance and anti-corrosion performance.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] The first aspect of the present invention is to provide a method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anti-corrosion composite coating, comprising the following steps:
[0009] S1. Dissolve LiF in HCl, then add Ti3AlC2 and perform etching reaction to obtain Ti3C2T x MXene nanosheets;
[0010] S2, Ti3C2T xMXene nanosheets and VO2 powder were dispersed in Tris-HCl buffer solution, ultrasonically treated in an ice-water bath, and then DA-HCl was added to react to obtain a homogeneous solution. The reaction was continued to obtain VO2@Ti3C2T x MXene nanosheets;
[0011] S3. Preparation of VO2@MXene / epoxy resin anti-corrosion composite coating: VO2@Ti3C2T x MXene nanosheets were ultrasonically dispersed in anhydrous ethanol, and then PAMMA and DGEBA were added and mixed evenly, and then sprayed onto the pretreated substrate to obtain the VO2@MXene / epoxy resin anti-corrosion composite coating.
[0012] Preferably, in step S1, the etching temperature is 40-60° C., and the etching time is 48-60 h.
[0013] Preferably, in step S1, the dosage ratio of LiF, HCl and Ti3AlC2 is 3.0-3.2 g: 30-40 mL: 1-2 g.
[0014] Preferably, in step S2, the ultrasonic treatment time under ice-water bath conditions is 30-60 min.
[0015] Preferably, in step S2, the reaction time of adding DA-HCl is 30-40 min, and the reaction temperature is 30-40° C.; the continued reaction time is 24-32 h.
[0016] Preferably, in step S2, the Ti3C2T x The dosage ratio of MXene nanosheets, VO2 powder, Tris-HCl buffer solution, and DA-HCl is 1.0-2.0g: 2.0-4.0g: 500-600mL: 1.0-2.0g.
[0017] Preferably, in step S3, the ultrasonic treatment time is 8-20 min.
[0018] Preferably, in step S3, the VO2@Ti3C2T x The dosage ratio of MXene nanosheets, anhydrous ethanol, PAMMA, and DGEBA is 0.048-0.720 g: 5-8 mL: 1.37-2.50 g: 3.40-7.50 g.
[0019] Preferably, in step S3, the pretreated substrate is pretreated as follows: Q235 carbon steel (20mm×40mm×1mm) is used as the substrate, the steel sheet sample is connected to the copper wire, and the remaining surfaces are sealed with epoxy resin except for one side exposed to the air; then the steel sheet sample is polished using sandpaper with a particle size of 320, 600, and 800, respectively, and preliminarily washed with DI water, and then ultrasonically treated in a 50% acetone solution for 1h to remove surface oil and impurities; then, immersed in an aqueous solution containing 1wt% KH550, 8wt% DI water and 91wt% ethanol, and finally rinsed with ethanol and dried in air.
[0020] The second aspect of the present invention provides a controllable heat-absorbing VO2@MXene / epoxy resin anti-corrosion composite coating obtained by the above preparation method.
[0021] The present invention has the following beneficial effects:
[0022] (1) The present invention first uses LiF and Ti3AlC2 as raw materials to prepare a single-layer Ti3C2T x MXene; then polydopamine (PDA) was used as a binder to bond the monolayer Ti3C2T x The MXene nanosheets in MXene are coated, which not only improves the mechanical stability of MXene, but also provides a large number of "anchor points" to be used as a binder to load the M-phase VO2 nanoparticles on the Ti3C2T x MXene surface, a VO2@Ti3C2T with controllable photothermal properties was prepared x MXene nanosheets can achieve controllable light absorption and photothermal conversion, thereby extending the service life of the anti-corrosion epoxy resin coating; finally, VO2@Ti3C2T x MXene nanosheets, hyperbranched amide compounds (PAMMA) and bisphenol A diglycidyl ether (DGEBA) were blended and sprayed onto the pretreated substrate surface to construct a VO2@MXene / epoxy resin anticorrosive composite coating with good photothermal and anticorrosive properties. Experimental results show that the VO2@Ti3C2T x After being immersed in 3.5% NaCl solution for 30 days, the MXene / epoxy resin anti-corrosion composite coating still maintains a high anti-corrosion performance; under 2.80Sun irradiation, VO2@Ti3C2T x The maximum temperature of the MXene / epoxy resin anti-corrosion composite coating is about 27.3°C lower than the maximum temperature of the coating without VO2 particles, and it reaches the photothermal equilibrium state earlier.
[0023] (2) The controllable heat-absorbing VO2@MXene / epoxy resin anti-corrosion composite coating prepared by the present invention has good controllable photothermal performance and anti-corrosion performance, and therefore has certain application potential in the fields of marine anti-corrosion, wind turbine blades and modern transportation.
[0024] (3) The preparation method of the present invention has a simple synthesis process and is suitable for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 For Ti3AlC2 and Ti3C2T x FT-IR spectrum of MXene;
[0027] Figure 2 For Ti3AlC2 and Ti3C2T x XPS spectrum of MXene;
[0028] Figure 3 FT-IR spectra of VPM, PM, and 1.0-VO2;
[0029] Figure 4 Cross-sectional SEM images of different coatings: (a) P-EP coating; (b) PM-EP coating; (c) VPM-EP coating;
[0030] Figure 5 VO2, Ti3C2T x MXene, VO2@Ti3C2T x UV-visible-infrared absorption spectrum of MXene;
[0031] Figure 6 VO2, Ti3C2T x MXene, PDA-Ti3C2T x MXene, VO2@Ti3C2T x The relationship between the time and temperature of xenon lamp irradiation of MXene;
[0032] Figure 7 Polarization curves of different coatings (P-EP, PM-EP and VPM-EP coatings) after being immersed in 3.5wt% NaCl solution for 24 hours;
[0033] Figure 8A schematic flow chart of a method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anti-corrosion composite coating provided by the present invention. DETAILED DESCRIPTION
[0034] In the following description, for the purpose of illustration rather than limitation, specific details such as specific system structures and technologies are provided to provide a thorough understanding of the embodiments of the present invention. However, it should be clear to those skilled in the art that the present invention may also be implemented in other embodiments without these specific details.
[0035] Example 1
[0036] See also Figure 8 , a method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anticorrosion composite coating, comprising the following steps:
[0037] (1) Pretreatment of Q235 carbon steel: Q235 carbon steel (20 mm × 40 mm × 1 mm) was used as the substrate, the steel sheet was connected to the copper wire, and the remaining surfaces were sealed with epoxy resin except for one side exposed to the air; then the steel sheet samples were polished with sandpaper of grit 320, 600, and 800, respectively, and preliminarily washed with DI water, and then ultrasonically treated in 50% acetone solution for 1 h to remove surface oil and impurities; then, immersed in an ethanol aqueous solution containing 1 wt% KH550, 8 wt% DI water, and 91 wt% ethanol for 2 h; finally, rinsed with ethanol three times and dried in air;
[0038] (2) Ti3C2T x Preparation of MXene nanosheets: 3.2 g LiF was dissolved in a polytetrafluoroethylene reactor containing 40 ml 9 M HCl and stirred for 10 min; then, 2 g 200 mesh Ti3AlC2 powder was slowly added and etched at 40 ° C for 48 h. After the reaction, the etching solution was acid-washed with 1 M HCl solution (3500 rpm, 1 min) 2-3 times; then, it was centrifuged and washed with water multiple times (5300 rpm, 1 min) until the precipitate showed obvious swelling and the upper liquid was dark green, and then ultrasonicated in an ice-water bath for 60 min (80 KHz) under Ar atmosphere; finally, the upper liquid was taken by centrifugation (5500 rpm, 10 min) and freeze-dried to obtain a single / few-layer Ti3C2T x MXene-based Ti3C2T x MXene nanosheets;
[0039] (3)VO2@Ti3C2T x Preparation of MXene nanosheets:
[0040] First, weigh 1.0 g Ti3C2T xMXene nanosheets and 2.0 g VO2 powder were dispersed in 500 mL Tris-HCl (15 mM, pH ≥ 8.5) buffer solution and ultrasonically stirred for 30 min in an ice-water bath;
[0041] Then, 1.0 g DA-HCl was slowly added within 10 min and stirred for 2 h to obtain a homogeneous solution. The reaction was continued at 30 °C for 24 h. The reaction product was repeatedly washed and centrifuged (6000 rpm, 1 min) with DI water to remove impurities such as unloaded VO2 nanoparticles. Finally, it was freeze-dried to constant weight to obtain VO@Ti3C2T x MXene nanosheets, denoted as VPM;
[0042] (4) Preparation of VO2@MXene / epoxy resin anti-corrosion composite coating:
[0043] 0.048 g of VPM was dispersed in 5 ml of anhydrous ethanol and ultrasonically dispersed for 10 min. Then, a mixture of 1.37 g of PAMMA and 3.40 g of DGEBA was added and stirred to make the mixture completely uniform. Then, a sprayer was used to apply it on the surface of a pretreated Q235 steel plate (thickness of 100 μm), and finally a VO2@MXene / epoxy resin anti-corrosion composite coating was obtained, which was recorded as VPM-EP.
[0044] Example 2
[0045] A method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating comprises the following steps:
[0046] (1) Pretreatment of Q235 carbon steel: same as in Example 1.
[0047] (2) Ti3C2T x Preparation of MXene nanosheets: 3.0g LiF was dissolved in a polytetrafluoroethylene reactor containing 30ml 9M HCl and stirred for 10min; then, 1g 200-mesh Ti3AlC2 powder was slowly added and etched at 50°C for 55h with continuous stirring. After the reaction, the etching solution was acid-washed with 1M HCl solution (3500rmp, 1min) 2-3 times; then, it was centrifuged and washed with water multiple times (5300rmp, 1min) until the precipitate showed obvious swelling and the upper liquid was dark green, and then ultrasonicated in an ice-water bath under Ar atmosphere for 60min (80KHz); finally, the upper liquid was taken by centrifugation (5500rmp, 10min) and freeze-dried to obtain a single / few-layer Ti3C2T x MXene-based Ti3C2T x MXene nanosheets;
[0048] (3)VO2@Ti3C2T x Preparation of MXene nanosheets:
[0049] First, weigh 1.5 g Ti3C2T x MXene nanosheets and 3.0 g VO2 powder were dispersed in 550 mL Tris-HCl (15 mM, pH ≥ 8.5) buffer solution and ultrasonically stirred for 30 min under ice-water bath conditions;
[0050] Then, 1.5 g DA-HCl was slowly added within 10 min and stirred for 2 h to obtain a homogeneous solution. The reaction was continued at 30 °C for 22 h. The reaction product was repeatedly washed and centrifuged (6000 rpm, 1 min) with DI water to remove impurities such as unloaded VO2 nanoparticles. Finally, it was freeze-dried to constant weight to obtain VO@Ti3C2T x MXene nanosheets;
[0051] (4) Preparation of VO2@MXene / epoxy resin anti-corrosion composite coating:
[0052] Take 0.056g VO@Ti3C2T x MXene nanosheets were dispersed in 7 ml of anhydrous ethanol and ultrasonically dispersed for 10 min; then a mixture of 1.85 g of PAMMA and 5.40 g of DGEBA was added and stirred to make the mixture completely uniform. Then, a sprayer was used to apply it on the surface of a pretreated Q235 steel plate (thickness of 100 μm), and finally a VO2@MXene / epoxy resin anti-corrosion composite coating was obtained.
[0053] Example 3
[0054] A method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating comprises the following steps:
[0055] (1) Pretreatment of Q235 carbon steel: same as in Example 1.
[0056] (2) Ti3C2T xPreparation of MXene nanosheets: 3.2 g LiF was dissolved in a polytetrafluoroethylene reactor containing 40 ml 9 M HCl and stirred for 10 min; then, 2 g 200 mesh Ti3AlC2 powder was slowly added and etched at 40 ° C for 60 h. After the reaction, the etching solution was acid-washed with 1 M HCl solution (3500 rpm, 1 min) 2-3 times; then, it was centrifuged and washed with water multiple times (5300 rpm, 1 min) until the precipitate showed obvious swelling and the upper liquid was dark green, and then ultrasonicated in an ice-water bath for 60 min (80 KHz) under Ar atmosphere; finally, the upper liquid was taken by centrifugation (5500 rpm, 10 min) and freeze-dried to obtain a single / few-layer Ti3C2T x MXene-based Ti3C2T x MXene nanosheets;
[0057] (3)VO2@Ti3C2T x Preparation of MXene nanosheets:
[0058] First, weigh 1.0 g Ti3C2T x MXene nanosheets and 2.0 g VO2 powder were dispersed in 500 mL Tris-HCl (15 mM, pH ≥ 8.5) buffer solution and ultrasonically stirred for 30 min in an ice-water bath;
[0059] Then, 1.0 g DA-HCl was slowly added within 10 min and stirred for 2 h to obtain a homogeneous solution. The reaction was continued at 30 °C for 24 h. The reaction product was repeatedly washed and centrifuged (6000 rpm, 1 min) with DI water to remove impurities such as unloaded VO2 nanoparticles. Finally, it was freeze-dried to constant weight to obtain VO@Ti3C2T x MXene nanosheets;
[0060] (4) Preparation of VO2@MXene / epoxy resin anti-corrosion composite coating:
[0061] Take 0.048g VO@Ti3C2T x MXene nanosheets were dispersed in 5 ml of anhydrous ethanol and ultrasonically dispersed for 10 min; then a mixture of 1.37 g of PAMMA and 3.40 g of DGEBA was added and stirred to make the mixture completely uniform, and then a sprayer was used to apply it to the surface of a pretreated Q235 steel plate (thickness of 100 μm), finally obtaining a VO2@MXene / epoxy resin anti-corrosion composite coating.
[0062] Example 4
[0063] A method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating comprises the following steps:
[0064] (1) Pretreatment of Q235 carbon steel: same as in Example 1.
[0065] (2) Ti3C2T x Preparation of MXene nanosheets: 3.2 g LiF was dissolved in a polytetrafluoroethylene reactor containing 35 ml 9 M HCl and stirred for 10 min; then, 1.5 g 200 mesh Ti3AlC2 powder was slowly added and etched at 60 ° C for 40 h. After the reaction, the etching solution was acid-washed with 1 M HCl solution (3500 rpm, 1 min) 2-3 times; then, it was centrifuged and washed with water multiple times (5300 rpm, 1 min) until the precipitate showed obvious swelling and the upper liquid was dark green, and then ultrasonicated in an ice-water bath for 60 min (80 KHz) under Ar atmosphere; finally, the upper liquid was taken by centrifugation (5500 rpm, 10 min) and freeze-dried to obtain a single / few-layer Ti3C2T x MXene-based Ti3C2T x MXene nanosheets;
[0066] (3)VO2@Ti3C2T x Preparation of MXene nanosheets:
[0067] First, weigh 2.0 g Ti3C2T x MXene nanosheets and 4.0 g VO2 powder were dispersed in 600 mL Tris-HCl (15 mM, pH ≥ 8.5) buffer solution and ultrasonically stirred for 30 min in an ice-water bath;
[0068] Then, 2.0 g DA-HCl was slowly added within 10 min and stirred for reaction for 3 h to obtain a homogeneous solution. The reaction was continued at 30 °C for 30 h. The reaction product was repeatedly washed and centrifuged (6000 rpm, 1 min) with DI water to remove impurities such as unloaded VO2 nanoparticles. Finally, it was freeze-dried to constant weight to obtain VO@Ti3C2T x MXene nanosheets;
[0069] (4) Preparation of VO2@MXene / epoxy resin anti-corrosion composite coating:
[0070] Take 0.060g VO@Ti3C2T xMXene nanosheets were dispersed in 6 ml of anhydrous ethanol and ultrasonically dispersed for 10 min; then a mixture of 2.0 g of PAMMA and 5.40 g of DGEBA was added and stirred to make the mixture completely uniform. Then, a sprayer was used to apply it on the surface of a pretreated Q235 steel plate (thickness of 100 μm), and finally a VO2@MXene / epoxy resin anti-corrosion composite coating was obtained.
[0071] Example 5
[0072] A method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating comprises the following steps:
[0073] (1) Pretreatment of Q235 carbon steel: same as in Example 1.
[0074] (2) Ti3C2T x Preparation of MXene nanosheets: 3.2 g LiF was dissolved in a polytetrafluoroethylene reactor containing 40 ml 9 M HCl and stirred for 10 min; then, 2 g 200 mesh Ti3AlC2 powder was slowly added and etched at 40 ° C for 48 h. After the reaction, the etching solution was acid-washed with 1 M HCl solution (3500 rpm, 1 min) 2-3 times; then, it was centrifuged and washed with water multiple times (5300 rpm, 1 min) until the precipitate showed obvious swelling and the upper liquid was dark green, and then ultrasonicated in an ice-water bath for 40 min (80 KHz) under Ar atmosphere; finally, the upper liquid was taken by centrifugation (5500 rpm, 10 min) and freeze-dried to obtain a single / few-layer Ti3C2T x MXene-based Ti3C2T x MXene nanosheets;
[0075] (3)VO2@Ti3C2T x Preparation of MXene nanosheets:
[0076] First, weigh 1.0 g Ti3C2T x MXene nanosheets and 2.0 g VO2 powder were dispersed in 500 mL Tris-HCl (15 mM, pH ≥ 8.5) buffer solution and ultrasonically stirred for 60 min in an ice-water bath;
[0077] Then, 1.0 g DA-HCl was slowly added within 10 min and stirred for 2 h to obtain a homogeneous solution. The reaction was continued at 40 °C for 24 h. The reaction product was repeatedly washed and centrifuged (6000 rpm, 1 min) with DI water to remove impurities such as unloaded VO2 nanoparticles. Finally, it was freeze-dried to constant weight to obtain VO@Ti3C2T x MXene nanosheets;
[0078] (4) Preparation of VO2@MXene / epoxy resin anti-corrosion composite coating:
[0079] Take 0.072g VO@Ti3C2T x MXene nanosheets were dispersed in 8 ml of anhydrous ethanol and ultrasonically dispersed for 10 min; then a mixture of 2.50 g of PAMMA and 7.5 g of DGEBA was added and stirred to make the mixture completely uniform. Then, a sprayer was used to apply it on the surface of a pretreated Q235 steel plate (thickness of 100 μm), and finally a VO2@MXene / epoxy resin anti-corrosion composite coating was obtained.
[0080] Comparative Example 1
[0081] It is basically the same as Example 1, except that VO2@Ti3C2T is not added x MXene nanosheets, specific steps:
[0082] (1) Pretreatment of Q235 carbon steel: same as in Example 1;
[0083] (2) Preparation of pure epoxy resin anti-corrosion coating: 1.37 g PAMMA and 3.40 g DGEBA were mixed evenly and then applied to the surface of the pretreated Q235 steel plate (thickness of 100 μm) using a sprayer to finally obtain a pure epoxy resin anti-corrosion coating, which was recorded as P-EP.
[0084] Comparative Example 2
[0085] The method is basically the same as Example 1, except that VO2 is not added. The specific steps are as follows:
[0086] (1) Pretreatment of Q235 carbon steel: same as in Example 1;
[0087] (2) Ti3C2T x Preparation of MXene nanosheets: same as in Example 1;
[0088] (3)PDA-Ti3C2T x Preparation of MXene materials: Weigh 1.0 g Ti3C2T x MXene nanosheets were dispersed in 500 mL Tris-HCl (15 mM, pH ≥ 8.5) buffer solution and ultrasonically stirred for 30 min in an ice-water bath. Then, 1.0 g DA-HCl was slowly added within 10 min and stirred for 2 h. The resulting homogeneous solution was reacted at 30 ° C for 24 h. The reaction product was repeatedly washed and centrifuged (6000 rpm, 1 min) with DI water. Finally, it was freeze-dried to constant weight to obtain PDA-Ti3C2T xMXene powder, denoted as PM;
[0089] (4)PDA-Ti3C2T x Preparation of MXene / epoxy resin anticorrosion composite coating: 0.048 g of PM was dispersed in 5 mL of anhydrous ethanol and ultrasonically dispersed for 10 min. Subsequently, a mixture consisting of 1.37 g of PAMMA and 3.40 g of DGEBA was added to the above dispersion. The resulting mixture was stirred to make it completely uniform, and then it was applied to the surface of the pretreated Q235 steel plate (thickness of 100 μm) using a sprayer to finally obtain PDA-Ti3C2T x MXene / epoxy resin anti-corrosion composite coating, denoted as PM-EP.
[0090] The Ti3C2T prepared in Example 1 x MXene nanosheets and Ti3AlC2 were characterized, and the results are shown in Figure 1 and Figure 2 shown.
[0091] Depend on Figure 1 The results show that 433cm -1 The broad absorption peak at is a typical hydroxyl absorption peak. Compared with Ti3AlC2, Ti3C2T x The MXene nanosheet material has a relatively wide and sharp peak here, which proves that during the etching process, x A large number of hydroxyl groups are introduced on the surface of MXene nanosheet materials. x MXene nanosheets at 1119 cm -1 The peak can also prove the introduction of alcohol hydroxyl groups. x The presence of hydroxyl groups on the surface of MXene nanosheets is beneficial to subsequent surface modification. x In the infrared absorption spectrum, at 2925cm -1 and 2853cm -1 There are two inconspicuous absorption peaks, which are caused by the symmetric stretching vibration and asymmetric stretching vibration of the C-H bond. In addition, it can be found that 1600cm -1 ~1650cm -1 Position Ti3AlC2 and Ti3C2T x MXene has a relatively sharp peak, which corresponds to the characteristic peak of CO bond. x In the infrared spectrum curve of MXene, 1480cm -1 、599cm -1 、545cm -1The characteristic peaks corresponding to Ti-OH, Ti-O and Ti-C bonds are shown at x MXene nanosheet materials were successfully prepared.
[0092] Depend on Figure 2 The results show that Ti3C2T x The Al 2p peak in the MXene nanosheets is significantly weakened or even disappears, while the F1s peak is significantly strengthened, proving that the Al layer is successfully etched away and new functional groups are introduced during the etching process, which indicates that the present invention successfully produces Ti3C2T x MXene nanosheets.
[0093] The VPM and PM prepared in Example 1 were characterized by infrared spectroscopy. Figure 3 .
[0094] Depend on Figure 3 The results show that in the infrared spectrum of PM, 3435cm -1 The broad absorption peak at is a typical hydroxyl absorption peak, indicating that PDA-Ti3C2T x There are hydroxyl groups on the surface of MXene materials. At the same time, the infrared spectrum of PM is at 1624cm -1 and 1071cm -1 There are peaks on the left and right, which are caused by the stretching vibration of CO bond and phenolic hydroxyl or aromatic benzene ring, indicating that dopamine is successfully coated on Ti3C2T x MXene surface. After loading VO2 on PM to form VPM material, we can observe 3435cm -1 The peak at position disappeared, and at 2918cm -1 and 2849cm -1 There are two obvious absorption peaks, which are caused by the symmetric stretching vibration and asymmetric stretching vibration of the CH bond in the structure of dopamine. -1 The infrared absorption of the latter is significantly enhanced, which is due to the loading of 1.0-VO2 on the PM surface. The above infrared spectrum test can prove that M-phase VO2 nanoparticles are successfully loaded on Ti3C2T x MXene surface, demonstrating VO2@Ti3C2T x Successful preparation of MXene materials.
[0095] The cross-sections of the coatings (VPM-EP, P-EP, PM-EP) obtained in Example 1 and Comparative Examples 1-2 were characterized. Figure 4 .
[0096] Depend on Figure 4The results show that the pure epoxy resin coating (P-EP) composed of bisphenol A diglycidyl ether DGEBA and hyperbranched amide compound PAMMA in Comparative Example 1 will produce defects such as microcracks and pores inside the epoxy resin due to the high crosslinking between PAMMA and DGEBA and the fast reaction rate during the curing process. The presence of these defects will cause corrosive media such as water, oxygen and ions to easily penetrate through the coating surface with the help of these microcracks and pores to reach the metal substrate, causing corrosion to the metal substrate. Compared with Comparative Example 1, PDA-Ti3C2T x The cross section of the PM-EP coating after MXene nanosheets is smoother and the defects are significantly reduced. The reduction of defects can effectively improve the barrier performance of the coating to the corrosive medium and prolong the time for the corrosive medium to reach the metal substrate. x The cross-section of the VPM-EP coating made with MXene as filler becomes smoother, without obvious defects such as microcracks and pores, which further enhances the anti-corrosion performance of the coating.
[0097] Based on the above SEM image results, it can be reasonably inferred that the reason for the reduction of microcracks and pores in the PM-EP coating prepared in Comparative Example 2 and the VPM-EP coating prepared in Example 1 may be that the presence of fillers can reduce the cross-linking density of the epoxy resin to a certain extent, while slowing down the internal stress generated by factors such as heat release during the curing process, thereby reducing or even eliminating the generation and growth of defects such as microcracks and pores.
[0098] For VO2, Ti3C2T x MXene, PDA-Ti3C2T x MXene and VO2@Ti3C2T x The photothermal properties of MXene were characterized at different temperatures (35°C, 55°C, 75°C). The results are shown in Figure 5 and Figure 6 .
[0099] Depend on Figure 5 The results show that Ti3C2T x The absorbance of MXene materials increases significantly with increasing temperature, especially at 55°C, where it nearly doubles, and at 75°C, where it increases by about three times. x After MXene was applied, the absorbance decreased significantly at 55°C. This is because the crystal structure of VO2 changed, which prevented light from penetrating VO2 and reaching Ti3C2T x MXene surface. This property makes the prepared VO2@Ti3C2T x MXene nanosheet materials can achieve controllable light absorption and light-to-heat conversion.
[0100] Depend on Figure 6 The results show that due to the dynamic thermal regulation mechanism of VO2, VO2@Ti3C2T loaded with VO2 particles x Under the irradiation of 2.80Sun xenon lamp, the average heating rate of MXene coating in the first 60s was about 0.5℃ / s, and the maximum temperature after 300s was 88.1℃, which was higher than that of Ti3C2T x MXene and PDA-Ti3C2T x The MXene coating reduced the temperature by about 27.3°C and reached the photothermal equilibrium state faster.
[0101] The three coating samples of VPM-EP, P-EP and PM-EP were immersed in 3.5wt% NaCl solution for 24 hours, and the polarization curves were measured. Figure 7 .
[0102] Depend on Figure 7 The results show that the i of the Bare sample corr The values are nearly three orders of magnitude higher than those of the P-EP coating, which are 4.80×10 -4 A.cm -2 and 2.01×10 -7 A.cm -2 . And the R of the Bare sample p It is also five orders of magnitude lower than that of the P-EP coating, which are 4.70×10 -2 kΩ·cm 2 and 2.21×10 2 kΩ·cm 2 , which shows that epoxy resin has a good protective effect on metal. After 1.0% PM material is doped in epoxy resin, the PM-EP coating corr (1.06×10 -8 A.cm -2 ) and v corr (2.43×10 -3 mm·y -1 ) is about one order of magnitude lower than that of EP coating, R p Also increased to 4.81×10 3 kΩ·cm 2 This is because the PM filler constructs a multi-level barrier system in the epoxy resin coating, which blocks the path of the corrosive medium that should diffuse evenly in the coating, causing the diffusion path and time path of the corrosive medium in the coating to become longer, and even difficult to penetrate into the metal surface.
[0103] Compared with PM-EP coating, VPM-EP coating has a higher E corr To be 3mV higher, i corr (1.85×10-9 A.cm -2 ) and v corr (4.23×10 -4 mm·y -1 ) is also nearly one order of magnitude lower. At the same time, the polarization resistance R p Increased to 2.83×10 4 kΩ·cm 2 The reason is that the surface of the VPM material is loaded with VO2 nanoparticles, which increases its specific surface area and forms a closer interface with the epoxy resin, thereby effectively curbing the penetration of the corrosive medium. In the inhibition efficiency IE, the IE of the P-EP coating is 99.95%, and the corrosion inhibition efficiency of PM-EP and VPM-EP both reach 99.99%. The Tafel polarization curve results show that after 24 hours of immersion, the VPM-EP coating has better corrosion resistance in the early stage.
[0104] The present invention is not limited to the above-mentioned specific implementation modes. Various changes made by ordinary technicians in this field based on the above-mentioned concepts without creative work are all within the protection scope of the present invention.
Claims
1. A method for preparing a controllable heat-absorbing VO2@MXene / epoxy resin anticorrosion composite coating, characterized in that: The following steps are involved: S1. Dissolve LiF in HCl, then add Ti3AlC2 and perform etching reaction to obtain Ti3C2T x MXene nanosheets; S2, Ti3C2T x MXene nanosheets and VO2 powder were dispersed in Tris-HCl buffer solution, ultrasonically treated in an ice-water bath, and then DA-HCl was added to react to obtain a homogeneous solution. The reaction was continued to obtain VO2@Ti3C2T x MXene nanosheets; S3. Preparation of VO2@MXene / epoxy resin anti-corrosion composite coating: VO2@Ti3C2T x MXene nanosheets were ultrasonically dispersed in anhydrous ethanol, and then PAMMA and DGEBA were added, mixed evenly, and sprayed onto the pretreated substrate to obtain the VO2@MXene / epoxy resin anti-corrosion composite coating.
2. The method for preparing the controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating according to claim 1, characterized in that: In step S1, the etching temperature is 40-60°C, and the etching time is 48-60h.
3. The method for preparing the controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating according to claim 1, characterized in that: In step S1, the dosage ratio of LiF, HCl and Ti3AlC2 is 3.0-3.2 g: 30-40 mL: 1-2 g.
4. The method for preparing the controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating according to claim 1, characterized in that: In step S2, the ultrasonic treatment time under the ice-water bath condition is 30-60 min.
5. The method for preparing the controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating according to claim 1, characterized in that: In step S2, the reaction time of adding DA-HCl is 30-40 minutes, and the reaction temperature is 30-40° C.; the continued reaction time is 24-32 hours.
6. The method for preparing the controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating according to claim 1, characterized in that: In step S2, the Ti3C2T x The dosage ratio of MXene nanosheets, VO2 powder, Tris-HCl buffer solution, and DA-HCl is 1.0-2.0g: 2.0-4.0g: 500-600mL: 1.0-2.0g.
7. The method for preparing the controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating according to claim 1, characterized in that: In step S3, the ultrasonic treatment time is 8-20 min.
8. The method for preparing the controllable heat-absorbing VO2@MXene / epoxy resin anticorrosive composite coating according to claim 1, characterized in that: In step S3, the VO2@Ti3C2T x The dosage ratio of MXene nanosheets, anhydrous ethanol, PAMMA, and DGEBA is 0.048-0.720 g: 5-8 mL: 1.37-2.50 g: 3.40-7.50 g.
9. A controllable heat-absorbing VO2@MXene / epoxy resin anti-corrosion composite coating prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
High-abrasion-resistance epoxy ceramic composite coating and preparation method thereof
CN109810616A
Polydopamine modified tungsten-doped vanadium dioxide nanoparticle composite intelligent temperature control coating and preparation method thereof
CN112341859A
Super-hydrophobic self-repairing SH / PDA-Ti3C2Tx / MXene / epoxy resin anti-corrosion composite coating and preparation method thereof
CN117384531A
Cited By
Waterborne epoxy zinc-rich coating as well as preparation method and application thereof
CN119799118A