Preparation method of poly (3, 4-ethylenedioxythiophene) doped vanadium pentoxide electrochromic film
By introducing poly3,4-ethylenedioxythiophene into V2O5 material to form a doped vanadium pentoxide electrochromic film, the problem of insufficient electrochemical and electrochromic properties of V2O5 material is solved, and the electrochemical activity and light are significantly improved Modulation performance, suitable for the preparation of high-performance zinc electrochromic devices.
Patent Information
- Application Number
- CN202411057089.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing V2O5 electrochromic materials have problems such as poor cycle performance, long response time and low transmittance in terms of electrochemical performance and electrochromic performance. Doping metal cations can only improve the electrochemical performance and rarely affect electrochemical performance. Color distortion performance.
The preparation method of poly3,4-ethylenedioxythiophene doped vanadium pentoxide electrochromic film is adopted, and the in-situ polymerization reaction is carried out by adding 3,4-ethylenedioxythiophene to the aqueous dispersion of vanadium pentoxide. The poly3,4-ethylenedioxythiophene interlayer V2O5 is formed to improve electrochemical activity, photomodulation range, response time and cyclic stability.
It realizes zinc-type electrochromic devices with high electrochemical activity, wide light modulation range, high color contrast, short response time, fast color change speed and good cycle stability, simplifying the preparation process of the material and suitable for industrial production.
Smart Images

Figure CN118956237A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of electrochromic materials and relates to a method for preparing a poly 3,4-ethylenedioxythiophene (PEDOT)-doped vanadium pentoxide electrochromic film. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Electrochromic (EC) materials are characterized by reversible and permanent changes in their optical properties when driven by an external voltage, which manifests itself in changes in color and transparency.
[0004] Electrochromic glass (smart window) is a new type of energy-saving building material. Its structure is generally composed of glass, transparent conductive layer, electrochromic layer, electrolyte layer, ion storage layer, transparent conductive layer and glass. V2O5 material is the only oxide material with bipolar electrochromic properties that can be used as both a color-changing material and an ion storage material. Its typical layered structure is conducive to the insertion and removal of metal ions during the redox process. V2O5 material is the most widely studied oxide among electrochromic materials. It can show a variety of color changes such as yellow, green, blue and intermediate states with voltage changes. Therefore, it has the characteristics of high color contrast and rich color change. However, as an electrode material, V2O5 also has many problems such as poor cycle performance, long response time and low transmittance. In order to improve the electrochemical performance of electrode materials, there are currently four typical methods to improve the electrochemical performance of electrode materials: (1) preparing nanostructured vanadium pentoxide electrode materials, which can significantly shorten the diffusion distance of lithium ions and increase the contact area between the electrode and the electrolyte; (2) improving the conductivity of vanadium pentoxide by adding carbon materials; (3) improving the electrochemical stability of vanadium pentoxide by surface coating; (4) doping with metal cations. Studies have shown that doping with metal cations is a very effective and promising method to improve the electrochemical performance of materials. However, doping with metal cations only improves the electrochemical performance of V2O5 materials and rarely changes the electrochromic properties of V2O5. Summary of the invention
[0005] In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a poly (3,4-ethylenedioxythiophene)-doped vanadium pentoxide electrochromic film, which can improve some electrochemical, optical and electrochromic properties of the film to varying degrees, such as electrochemical activity, light modulation range, response time or cycle stability, thereby obtaining a zinc-type electrochromic device with better performance.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, a method for preparing a poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide electrochromic film comprises the following steps:
[0008] Adding 3,4-ethylenedioxythiophene to the aqueous dispersion of vanadium pentoxide, stirring the reaction continuously, so that 3,4-ethylenedioxythiophene undergoes in-situ polymerization reaction, and poly-3,4-ethylenedioxythiophene is intercalated with V2O5;
[0009] The material after continuous stirring reaction is centrifuged and washed, and then the precipitate after centrifugal washing is added with water and ultrasonically treated to prepare a precursor solution;
[0010] The precursor solution is sprayed on the surface of the conductive substrate and then annealed to obtain the product.
[0011] The present invention utilizes the oxidizing property of vanadium pentoxide to make 3,4-ethylenedioxythiophene undergo in-situ polymerization reaction, and intercalates poly-3,4-ethylenedioxythiophene with V2O5 to obtain a poly-3,4-ethylenedioxythiophene doped with vanadium pentoxide composite, removes unreacted V2O5 and EDOT, sprays the composite onto the surface of a conductive substrate, and then anneals the composite. During the annealing process, not only is a film formed from the poly-3,4-ethylenedioxythiophene doped with vanadium pentoxide, but the film is also more firmly adhered to the conductive substrate.
[0012] On the other hand, a poly (3,4-ethylenedioxythiophene)-doped vanadium pentoxide film is obtained by the above preparation method.
[0013] In a third aspect, an electrochromic cathode includes a conductive substrate and the above-mentioned poly (3,4-ethylenedioxythiophene) doped with vanadium pentoxide film attached to the surface of the conductive substrate.
[0014] In a fourth aspect, an electrochromic device comprises an anode, a cathode, and an electrolyte, wherein the anode and the cathode are placed in the electrolyte, the anode is metallic zinc, the cathode is the electrochromic cathode described above, or the cathode contains a film of the poly 3,4-ethylenedioxythiophene doped with vanadium pentoxide described above.
[0015] The present invention has found that when the poly 3,4-ethylenedioxythiophene doped vanadium pentoxide film provided by the present invention is used as a zinc-type electrochromic cathode material, electrochromism can be achieved, wherein a coloring process can be achieved by applying a constant voltage of 0.1±0.02V, and a fading process can be achieved by applying a constant voltage of 2.2±0.02V.
[0016] A fifth aspect provides an application of the above-mentioned poly 3,4-ethylenedioxythiophene doped with vanadium pentoxide film, electrochromic cathode or electrochromic device in an electrochromic window.
[0017] The beneficial effects of the present invention are:
[0018] 1. The poly 3,4-ethylenedioxythiophene doped vanadium pentoxide thin film material provided by the present invention has the advantages of high electrochemical activity, wide light modulation range, high color contrast, short response time, fast color change speed, good cycle stability and long life compared with vanadium pentoxide thin film.
[0019] 2. The preparation method of the poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide thin film material provided by the present invention is simple and convenient for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0021] Figure 1 This is a photograph of the PEDOT@V2O5 film attached to the ITO glass when annealing is completed in Example 1 of the present invention.
[0022] Figure 2 These are photos of the PEDOT@V2O5 film of Example 1 of the present invention displaying different colors at different voltages, A is 0.1V, B is 1.2V, and C is 2.2V.
[0023] Figure 3 Scanning electron microscope photos of PEDOT@V2O5 and ITO / PEDOT@V2O5 of Example 1 of the present invention.
[0024] Figure 4 These are transmission electron microscope photos and element distribution images of PEDOT@V2O5 of Example 1 of the present invention, A is a bright field transmission electron microscope image, B is a dark field transmission electron microscope image, C is a sulfur element distribution map, D is an oxygen element distribution map, and E is a vanadium element distribution map.
[0025] Figure 5Cyclic voltammetry (CV) curve images of PEDOT@V2O5 (A) and V2O5 (B) prepared in Example 1 of the present invention and Comparative Example 1 in Zn(ClO4)2 (0.1M) and LiClO4 (0.8M)-PC solutions, respectively.
[0026] Figure 6 The visible light transmission spectrum images of PEDOT@V2O5 (A) and V2O5 (B) prepared in Example 1 of the present invention and Comparative Example 1 in different colors.
[0027] Figure 7 Response time images of PEDOT@V2O5 (A) and V2O5 (B) prepared in Example 1 of the present invention and Comparative Example 1 in Zn(ClO4)2 (0.1M) and LiClO4 (0.8M)-PC solutions (pH≈5), respectively.
[0028] Figure 8 These are the cyclic stability images of PEDOT@V2O5 (A) and V2O5 (B) prepared in Example 1 of the present invention and Comparative Example 1 in Zn(ClO4)2 (0.1M) and LiClO4 (0.8M)-PC solutions, respectively. DETAILED DESCRIPTION
[0029] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0030] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0031] In view of the fact that it is difficult to improve both the electrochemical properties and the electrochromic properties of V2O5 materials using existing modification methods, the present invention provides a method for preparing a poly-3,4-ethylenedioxythiophene doped vanadium pentoxide electrochromic film.
[0032] A typical embodiment of the present invention provides a method for preparing a poly-3,4-ethylenedioxythiophene doped vanadium pentoxide electrochromic film, comprising the following steps:
[0033] Adding 3,4-ethylenedioxythiophene to the aqueous dispersion of vanadium pentoxide, stirring the reaction continuously, so that 3,4-ethylenedioxythiophene undergoes in-situ polymerization reaction, and poly-3,4-ethylenedioxythiophene is intercalated with V2O5;
[0034] The material after continuous stirring reaction is centrifuged and washed, and then the precipitate after centrifugal washing is added with water and ultrasonically treated to prepare a precursor solution;
[0035] The precursor solution is sprayed on the surface of the conductive substrate and then annealed to obtain the product.
[0036] In some embodiments, the addition ratio of vanadium pentoxide to 3,4-ethylenedioxythiophene is 2.0-2.5 g:1 mL.
[0037] In some embodiments, the stirring reaction time is 115 to 125 hours.
[0038] In some embodiments, ethanol and water are used for centrifugal washing. Specifically, the centrifugal speed is 7000-9000 r / min, and the single centrifugal time is 2-4 min.
[0039] In some embodiments, the ultrasonic treatment time is 0.5 to 1 h.
[0040] In some embodiments, the concentration of the precursor solution is 8-15 mg / mL.
[0041] In some embodiments, the conductive substrate is conductive glass, and in particular, the conductive substrate is ITO glass.
[0042] In some embodiments, the annealing temperature is 140-190° C., and the annealing time is 15-25 hours.
[0043] Another embodiment of the present invention provides a poly (3,4-ethylenedioxythiophene)-doped vanadium pentoxide film obtained by the above preparation method.
[0044] A third embodiment of the present invention provides an electrochromic cathode, comprising a conductive substrate and the above-mentioned poly (3,4-ethylenedioxythiophene) doped with vanadium pentoxide film attached to the surface of the conductive substrate.
[0045] A fourth embodiment of the present invention provides an electrochromic device, comprising an anode, a cathode, and an electrolyte, wherein the anode and the cathode are placed in the electrolyte, the anode is metallic zinc, the cathode is the above-mentioned electrochromic cathode, or the cathode contains the above-mentioned poly 3,4-ethylenedioxythiophene doped vanadium pentoxide film.
[0046] In some embodiments, in the electrolyte, the electrolyte is Zn(ClO4)2 and LiClO4, and the solvent is propylene carbonate (PC). Specifically, in the electrolyte, the concentration of Zn(ClO4)2 is 0.05-0.15M, and the concentration of LiClO4 is 0.75-0.85M. The unit M refers to mol / L.
[0047] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0048] Example 1
[0049] A poly (3,4-ethylenedioxythiophene) (PEDOT)-doped vanadium pentoxide film, the preparation method of which comprises the following steps:
[0050] (1) 7 g of commercial vanadium pentoxide was added to 200 ml of deionized water solution and stirred for 30 min. Then 3 ml of 3,4-ethylenedioxythiophene was added and the mixture was stirred for 5 days to obtain a dark green solution.
[0051] (2) The dark green solution was washed twice by centrifugation with ethanol and deionized water respectively, the centrifugal speed was 8000 r / min, and the single centrifugation time was 3 min; the precipitate after centrifugal washing was added with deionized water, and then ultrasonically treated for 1 h to prepare a precursor solution (concentration of 10 mg / mL).
[0052] (3) 40 mL of the precursor solution of step (2) was evenly sprayed on an ITO glass (5 cm×5 cm) by a spraying method, and then annealed at 180° C. for 20 h to form a poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide (PEDOT@V2O5) film on the ITO glass.
[0053] The PEDOT@V2O5 film of Example 1 was characterized:
[0054] When annealing is completed, the PEDOT@V2O5 film attached to the ITO glass appears dark green, as shown in Figure 1 shown.
[0055] The power supply was connected to the cathode and anode through a wire, the film adhered to the ITO glass substrate was used as the cathode, and the metal zinc was used as the anode. The electrochemical workstation was used to detect the Zn(ClO4)2 (0.1M) and LiClO4 (0.8M) PC solutions. The PEDOT@V2O5 film was displayed as gray, olive, and dark green at voltages of 0.1V, 1.2V, and 2.2V, respectively. Figure 2As shown, the PEDOT@V2O5 film completes gray coloring at 0.1V, begins to fade to olive green at 1.2V, and completely fades to its original color, dark green, at 2.2V.
[0056] The morphology of PEDOT@V2O5 thin films was analyzed by scanning electron microscopy (SEM). Figure 3 As shown, PEDOT@V2O5 is a nanofiber (rod) structure.
[0057] Transmission electron microscopy (TEM) and elemental analysis images to analyze the microscopic morphology and whether the doping is uniform; Figure 4 As shown in A, a single rod-shaped structure of PEDOT@V2O5 was captured, which is consistent with the results captured by scanning electron microscopy; Figure 4 As shown in CE, PEDOT@V2O5 nanorods contain three elements, S, O, and V, and are evenly distributed.
[0058] Example 2
[0059] A poly (3,4-ethylenedioxythiophene) (PEDOT)-doped vanadium pentoxide film, the preparation method of which comprises the following steps:
[0060] (1) 7 g of commercial vanadium pentoxide was added to 200 ml of deionized water solution and stirred for 30 min. Then 3 ml of 3,4-ethylenedioxythiophene was added and the mixture was stirred for 5 days to obtain a dark green solution.
[0061] (2) The dark green solution was washed twice by centrifugation with ethanol and deionized water respectively, the centrifugal speed was 8000 r / min, and the single centrifugation time was 3 min; the precipitate after centrifugal washing was added with deionized water, and then ultrasonically treated for 0.5 h to prepare a precursor solution (concentration of 8 mg / mL).
[0062] (3) 40 mL of the precursor solution of step (2) was evenly sprayed on an ITO glass (5 cm×5 cm) by a spraying method, and then annealed at 150° C. for 20 h to form a poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide (PEDOT@V2O5) thin film on the ITO glass.
[0063] Example 3
[0064] A poly (3,4-ethylenedioxythiophene) (PEDOT)-doped vanadium pentoxide film, the preparation method of which comprises the following steps:
[0065] (1) 7 g of commercial vanadium pentoxide was added to 200 ml of deionized water solution and stirred for 30 min. Then 3 ml of 3,4-ethylenedioxythiophene was added and the mixture was stirred for 5 days to obtain a dark green solution.
[0066] (2) The dark green solution was washed twice by centrifugation with ethanol and deionized water respectively, the centrifugal speed was 8000 r / min, and the single centrifugation time was 3 min; the precipitate after centrifugal washing was added with deionized water, and then ultrasonically treated for 1 h to prepare a precursor solution (concentration of 15 mg / mL).
[0067] (3) 40 mL of the precursor solution of step (2) was evenly sprayed on an ITO glass (5 cm×5 cm) by a spraying method, and then annealed at 160° C. for 20 h to form a poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide (PEDOT@V2O5) film on the ITO glass.
[0068] Comparative Example 1
[0069] The method for preparing a vanadium pentoxide film comprises the following steps:
[0070] (1) Add 7 g of commercial vanadium pentoxide to 200 ml of deionized water solution, stir for 30 min, and continue mixing and stirring for 5 days;
[0071] (2) The dispersion obtained in step (1) was centrifuged twice with ethanol and deionized water respectively, at a centrifugal speed of 8000 r / min. The single centrifugation time was 3 min, and then ultrasonically treated for 1 h, and deionized water was added to prepare a precursor solution (concentration of 10 mg / mL).
[0072] (3) The precursor solution is evenly sprayed on the ITO glass, and then annealed at 180°C for 20 hours to form a vanadium pentoxide film on the ITO glass.
[0073] Electrochemical and optical tests (Example 1 and Comparative Example 1)
[0074] (1) A power source was connected to the cathode and the anode through a wire, the film adhered to the ITO glass substrate was used as the cathode, and metal zinc was used as the anode. Cyclic voltammetry (CV) measurements were performed on PEDOT@V2O5 (Example 1) and V2O5 (Comparative Example 1) in Zn(ClO4)2 (0.1 M) and LiClO4 (0.8 M)-PC solutions, respectively, using an electrochemical workstation, where the scan rate was 50 mV / s.
[0075] like Figure 5 As shown, compared with V2O5 (Comparative Example 1), the current density in the CV curve of the PEDOT-doped film is larger, indicating that PEDOT@V2O5 (Example 1) has higher electrochemical activity.
[0076] (2) Use a visible light spectrophotometer to measure the visible light transmission spectra of PEDOT@V2O5 films at constant voltages of 0.2 V, 1.2 V, and 2.2 V (different colors);
[0077] like Figure 6 As shown, the colors of PEDOT@V2O5 (Example 1) and V2O5 (Comparative Example 1) are the same at constant voltages of 0.2 V, 1.2 V, and 2.2 V, which are gray and olive respectively. The results show that the lower the PEDOT element doping content, the lower the light modulation range of the film.
[0078] Among them, the light modulation range of PEDOT@V2O5 (Example 1) at 400nm is the largest, about 27.1%; the light modulation range of V2O5 (Comparative Example 1) at 400nm is about 13.3%. The above measurement results show that the maximum light modulation range of the film doped with PEDOT is significantly larger than that of the film doped with PEDOT.
[0079] (3) The response time and cycle stability of PEDOT@V2O5 (Example 1) and V2O5 (Comparative Example 1) were measured using an electrochemical workstation in combination with a visible light spectrophotometer in Zn(ClO4)2 (0.1 M) and LiClO4 (0.8 M)-PC solutions, respectively.
[0080] like Figure 7 As shown, the response time of PEDOT@V2O5 (Example 1) and V2O5 (Comparative Example 1) was measured for multiple cycles in Zn(ClO4)2 (0.1M) and LiClO4 (0.8M)-PC solutions, respectively. Each cycle was 120 seconds, that is, a constant voltage of 0.1V for 60 seconds and a constant voltage of 2.2V for 60 seconds were applied, respectively. The response time is defined as the time required to reach a final transmittance of 90%. The coloring time of the PEDOT@V2O5 film (Example 1) at 400nm is 9.2s, and the fading time is 9.6s, which is the fastest of the two; the coloring time of the V2O5 film (Comparative Example 1) at 524nm is 16.2s, and the fading time is 31.7s.
[0081] like Figure 8 As shown, PEDOT@V2O5 (Example 1) and V2O5 (Comparative Example 1) were subjected to 1000 CV cycles in Zn(ClO4)2 (0.1M) and LiClO4 (0.8M)-PC solutions, respectively, with a scan rate of 50mV / s. The ratio of the areas enclosed by the CV curves is the ratio of the capacity of the electrodes. The measurement results show that PEDOT@V2O5 (Example 1) has the smallest attenuation after 1000 CV cycles and the highest capacity retention rate; while the attenuation of V2O5 (Comparative Example 1) is significantly larger and the capacity retention rate is lower.
[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide electrochromic film, characterized in that: The process includes the following: Adding 3,4-ethylenedioxythiophene to the aqueous dispersion of vanadium pentoxide, stirring the reaction continuously, so that 3,4-ethylenedioxythiophene undergoes in-situ polymerization reaction, and poly-3,4-ethylenedioxythiophene is intercalated with V2O5; The material after continuous stirring reaction is centrifuged and washed, and then the precipitate after centrifugal washing is added with water and ultrasonically treated to prepare a precursor solution; The precursor solution is sprayed on the surface of the conductive substrate and then annealed to obtain the product.
2. The method for preparing the poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide electrochromic film as claimed in claim 1, characterized in that: The addition ratio of vanadium pentoxide to 3,4-ethylenedioxythiophene is 2.0-2.5 g:1 mL; the stirring reaction time is 115-125 h.
3. The method for preparing the poly-3,4-ethylenedioxythiophene doped vanadium pentoxide electrochromic film according to claim 1, characterized in that: Wash by centrifugation with ethanol and water.
4. The method for preparing the poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide electrochromic film as claimed in claim 1, characterized in that: The ultrasonic treatment time is 0.5 to 1 h.
5. The method for preparing the poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide electrochromic film as claimed in claim 1, characterized in that: The concentration of the precursor solution is 8-15 mg / mL; the conductive substrate is conductive glass; or the conductive substrate is ITO glass; the annealing temperature is 140-190° C., and the annealing time is 15-25 hours.
6. A poly (3,4-ethylenedioxythiophene) doped vanadium pentoxide film, characterized in that: Obtained by the preparation method according to any one of claims 1 to 5.
7. An electrochromic cathode, characterized in that: The invention comprises a conductive substrate and a film of poly 3,4-ethylenedioxythiophene doped with vanadium pentoxide attached to the surface of the conductive substrate.
8. An electrochromic device, characterized in that: The invention comprises an anode, a cathode and an electrolyte. The anode and the cathode are placed in the electrolyte. The anode is metal zinc, the cathode is the electrochromic cathode, or the cathode contains a film of poly 3,4-ethylenedioxythiophene doped with vanadium pentoxide.
9. In some embodiments as described in claim 8, in the electrolyte, the electrolyte is Zn(ClO4)2 and LiClO4, and the solvent is propylene carbonate; or, in the electrolyte, the concentration of Zn(ClO4)2 is 0.05-0.15M, and the concentration of LiClO4 is 0.75-0.85M.
10. Use of the above-mentioned poly 3,4-ethylenedioxythiophene doped with vanadium pentoxide film, electrochromic cathode or electrochromic device in electrochromic glass.
Citation Information
Patent Citations
Oxidizability and reducibility conducting polymer flow anode used for flow battery
CN102646835A
Electrochromic device (ECD) taking poly 3, 4-ethylenedioxy thiophene and vanadium pentoxide as electrochromism electrode materials and application thereof
CN104199228A
Preparation method for PEDOT: PSS solution and film based on molecule template principle
CN106928480A
Multicolor electrochromic composite film and preparation method and application thereof
CN113979646A
Alcohol dispersion liquid of conductive polyethylene dioxythiophene as well as preparation method and application of alcohol dispersion liquid
CN114316223A