Functional acrylic acid modified polysiloxane heavy anti-corrosion coating and preparation method thereof

By introducing ZIF-8 nanoparticles into acrylic modified polysiloxane coatings, the problem of poor adhesion of the coating is solved, the adhesion and weatherability of the coating is improved, the chemical stability and antibacterial properties are enhanced, and the coating is improved. Overall strength and environmental friendliness.

CN118956263AInactive Publication Date: 2024-11-15SHENGHONG COATINGS (DALIAN) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411419310.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Acrylic modified polysiloxane coatings have poor adhesion to primer/intermediate paints in construction applications, are prone to falling off, and have strict requirements on ambient temperature and humidity and coating intervals, which affects their construction and weather resistance.

Method used

By introducing ZIF-8 nanoparticles and reacting with acrylic resin under the action of a catalyst, good compatibility and dispersion are formed, the adhesion between the coating and the substrate is improved, and the mechanical strength and chemical stability of the coating are enhanced. Increase antibacterial properties.

Benefits of technology

It improves the adhesion, chemical resistance, thermal stability and corrosion resistance of the coating, reduces the organic volatiles in the solid content, and improves the overall strength and environmental friendliness of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118956263A_ABST
    Figure CN118956263A_ABST
Patent Text Reader

Abstract

The invention provides a functional acrylic acid modified polysiloxane heavy anti-corrosion coating and a preparation method thereof, and belongs to the technical field of coating preparation, and the preparation method comprises the following steps: reacting acrylic resin, an organic environment-friendly solvent, amino-modified ZIF-8 nanoparticle dispersion liquid, a catalyst and functional modified polysiloxane to prepare a mixture I; uniformly stirring acrylic acid modified polysiloxane resin, calcium carbonate, polyvinylpyrrolidone, polyether modified siloxane, organic silicon, an ultraviolet light absorber triazine-5, a histamine light stabilizer, amino silane and an organic environment-friendly solvent, and filtering to obtain a mixture II; adding functional modified polysiloxane, methyl methacrylate and epoxy resin into the mixture II, reacting and filtering to obtain a mixture III; and mixing the mixture I with the mixture III, fully reacting, and filtering to obtain the functional acrylic acid modified polysiloxane heavy anti-corrosion coating. The adhesive force, the corrosion resistance, the chemical resistance and the antibacterial property of the coating are improved, and the coating is environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating preparation, and in particular to a functionalized acrylic acid-modified polysiloxane heavy-duty anticorrosive coating and a preparation method thereof. Background Art

[0002] In recent years, my country's anti-corrosion coatings have made great achievements, and the production, sales and technical performance of coatings have been greatly improved. In the development of anti-corrosion coatings, the country has played a great role in promoting the healthy development of the coatings industry in terms of energy conservation and emission reduction, environmental protection, and low-carbon construction. At the same time, it has also put forward higher requirements for the anti-corrosion coatings industry. With the continuous improvement of environmental awareness, coating companies are encouraged to develop alternatives to traditional solvent-based coatings (high solids, solvent-free and water-based anti-corrosion coatings); develop alternatives to traditional heavily polluting and toxic anti-corrosion primers containing heavy metal pigments; develop environmentally friendly long-lasting anti-fouling coatings; develop low surface treatment technology; develop new energy-saving and emission-reducing coating processes and technologies, and limit high-energy-consuming coating equipment and processes.

[0003] Acrylic modified polysiloxane coatings have inorganic-organic hybrid properties that are far greater than ultraviolet radiation, Si-O-Si bond energy (446 kJ / mol), excellent weather resistance and corrosion resistance, and the abundant silanol groups in the film-forming material can condense with the hydroxyl groups on the metal surface to form covalent bonds, resulting in high adhesion between the coating and the substrate. However, compared with traditional polyurethane and fluorocarbon topcoats, acrylic modified polysiloxane coatings are not ideal for matching with primers / intermediate paints during construction and application, mainly manifested in: (1) poor adhesion between the primer / intermediate paint layer and easy to fall off; (2) strict requirements on environmental temperature and humidity, coating interval, and coating thickness, and easy to peel off from the primer and intermediate paint.

[0004] However, acrylic modified polysiloxane coatings are still an ideal substitute for traditional topcoats due to their low volatile organic matter content, environmental protection, no isocyanate group, and low toxicity. Therefore, solving the poor adhesion, weather resistance and construction performance of acrylic modified polysiloxane coatings has become a research focus. Summary of the invention

[0005] The purpose of the present invention is to provide a functionalized acrylic modified polysiloxane heavy-duty anticorrosion coating and a preparation method thereof. The preparation method improves the adhesion of the coating to a primer and an intermediate paint due to the introduction of ZIF-8 nanoparticles, improves the anticorrosion performance, improves the chemical resistance, improves the thermal stability, provides antibacterial properties, and improves the mechanical strength of the coating. The coating also has low solid content, low organic volatiles, and is environmentally friendly.

[0006] In order to solve the above technical problems, the present invention provides a functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating and a preparation method thereof.

[0007] To achieve the above object, the present invention provides the following technical solution: a functional acrylic modified polysiloxane heavy anticorrosive coating, characterized in that it comprises mixture one, mixture two and mixture three, The raw materials in the mixture 1 are calculated by mass ratio, wherein the mass ratio of acrylic resin to organic environmentally friendly solvent is 1:0.5-4, the mass ratio of amino-modified ZIF-8 nanoparticle dispersion to acrylic resin is 1:10-50, and the mass ratio of acrylic resin to functionalized modified polysiloxane to catalyst is 1:0.5-1.2:0.005-0.02; The raw materials in the second mixture are calculated by mass ratio, wherein acrylic modified polysiloxane resin: calcium carbonate: polyvinyl pyrrolidone: polyether modified siloxane: silicone: ultraviolet absorber triazine-5: histamine light stabilizer: aminosilane: organic environmentally friendly solvent = 1: 0.01~0.08: 0.005~0.025: 0.005~0.025: 0.005~0.025: 0~0.08: 0~0.08: 0.12~0.2: 0.7~1.5; The raw materials in the mixture three are added to the mixture two in a mass ratio of functionalized modified polysiloxane, methyl methacrylate, and epoxy resin, wherein the acrylic modified polysiloxane resin from the mixture two: functionalized modified polysiloxane: methyl methacrylate: epoxy resin = 1:0~0.25: 0.02~0.3: 0.08~0.15; Furthermore, the method for preparing the amino-modified ZIF-8 nanoparticle dispersion comprises the following steps: Step 1: adding ZIF-8 nanoparticles to an organic solvent containing an organic amine at a mass ratio of 1:50-100, stirring at 40-80°C for 2-4 hours, filtering, washing, and drying to obtain amino-modified ZIF-8 nanoparticles; Step 2: Add the amino-modified ZIF-8 nanoparticles into an organic environmentally friendly solvent at a mass ratio of 1:10-50, stir for 1-3 hours, and ultrasonicate for 30-120 minutes to obtain an amino-modified ZIF-8 nanoparticle dispersion.

[0008] Furthermore, the organic environmentally friendly solvent is one or more of ethyl acetate, propylene glycol methyl ether acetate, diethylene glycol butyl ether, and xylene; Furthermore, the functionalized modified polysiloxane is a polysiloxane modified to introduce a nucleophilic functional group, an amino group (-NH 2 ), hydroxyl (-OH) and thiol (-SH) groups; Furthermore, the catalyst is one or more of dibutyltin dilaurate, dibutyltin acetate and tetrabutyl titanate.

[0009] Furthermore, the organic solvent containing organic amine is prepared by dissolving the organic amine in an organic solvent at a mass ratio of 1:2 to 10. The organic amine is aqueous ammonia, ethylenediamine, diethylenetriamine, or aminopropyltriethoxysilane; and the organic solvent is one or more of dimethylformamide, dimethyl sulfoxide, xylene, ethanol, tetrahydrofuran, and ethyl acetate.

[0010] A method for preparing a functionalized acrylic acid-modified polysiloxane heavy-duty anticorrosive coating comprises the following steps: Step 1: Add acrylic resin and organic environmentally friendly solvent to a stirrer, mix well, add amino-modified ZIF-8 nanoparticle dispersion, continue stirring for 15 to 30 minutes, add catalyst, continue stirring for 30 minutes, add functionalized modified polysiloxane, continue mixing and stirring, continue to add catalyst during this stirring process, fully react and mix well to obtain mixture 1; Step 2: Add acrylic modified polysiloxane resin, calcium carbonate, polyvinyl pyrrolidone, polyether modified siloxane, silicone, ultraviolet absorber triazine-5, histamine light stabilizer, and aminosilane into a stirrer at a speed of 500-1000 r / min and stir for 30 min, then add pigments and fillers, continue stirring at 1500-2000 r / min for 1-2 hours until the fineness is ≤30 μm, add an organic environmentally friendly solvent into the system, stir evenly at 1000 r / min, and filter to obtain a mixture II; Step 3: Add functionalized modified polysiloxane, methyl methacrylate and epoxy resin to mixture 2, stir at 500-1000 r / min for 15 min, and filter again to obtain mixture 3; Step 4: Mix mixture 1 and mixture 3, stir at 500-1000 r / min for 30-90 min, mix evenly and filter after sufficient reaction to obtain a functionalized acrylic modified polysiloxane heavy anti-corrosion coating, wherein the ratio of acrylic resin to acrylic modified polysiloxane resin is 1:0.5-2.5.

[0011] The present invention provides a functionalized acrylic modified polysiloxane heavy anticorrosion coating and a preparation method thereof. ZIF-8 nanoparticles are introduced during the synthesis process, reacted with acrylic acid under the action of a catalyst, and introduced into an acrylic modified polysiloxane coating. The method allows the introduced ZIF-8 nanoparticles to have good compatibility, dispersibility and stability with the acrylic polysiloxane coating. The nanoparticles of ZIF-8 can increase the adhesion between the coating and the substrate, and improve the adhesion of the coating by forming more mechanical anchoring points. It has high chemical stability and good pore structure, and can be used as a physical barrier to block the penetration of corrosive media such as moisture, oxygen and corrosive chemicals, thereby improving the anticorrosion performance of the coating. The coating can be improved in terms of tolerance to chemicals, including acids, alkalis and solvents, and the overall strength of the coating can be improved, which is particularly important for coatings used in harsh environments. The functionalized acrylic modified polysiloxane heavy anticorrosion coating prepared by the present invention can well solve the existing technical problems and can make the coating have antibacterial properties through the release of zinc ions, so that it has more competitive advantages in the heavy anticorrosion coating market. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 The present invention provides a functionalized acrylic modified polysiloxane heavy-duty anti-corrosion coating and a flow chart of its preparation method. DETAILED DESCRIPTION

[0013] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0014] See also Figure 1 , an embodiment of the present invention provides a functionalized acrylic modified polysiloxane heavy-duty anti-corrosion coating and a preparation method thereof.

[0015] A functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating, characterized in that it comprises a mixture 1, a mixture 2 and a mixture 3, The raw materials in the mixture 1 are calculated by mass ratio, wherein the mass ratio of acrylic resin to organic environmentally friendly solvent is 1:0.5-4, the mass ratio of amino-modified ZIF-8 nanoparticle dispersion to acrylic resin is 1:10-50, and the mass ratio of acrylic resin to functionalized modified polysiloxane to catalyst is 1:0.5-1.2:0.005-0.02; The raw materials in the second mixture are calculated by mass ratio, wherein acrylic modified polysiloxane resin: calcium carbonate: polyvinyl pyrrolidone: polyether modified siloxane: silicone: ultraviolet absorber triazine-5: histamine light stabilizer: aminosilane: organic environmentally friendly solvent = 1: 0.01~0.08: 0.005~0.025: 0.005~0.025: 0.005~0.025: 0~0.08: 0~0.08: 0.12~0.2: 0.7~1.5; The raw materials in the mixture three are added to the mixture two in a mass ratio of functionalized modified polysiloxane, methyl methacrylate, and epoxy resin, wherein the acrylic modified polysiloxane resin from the mixture two: functionalized modified polysiloxane: methyl methacrylate: epoxy resin = 1:0~0.25: 0.02~0.3: 0.08~0.15; The method for preparing the amino-modified ZIF-8 nanoparticle dispersion comprises the following steps: Step 1: adding ZIF-8 nanoparticles to an organic solvent containing an organic amine at a mass ratio of 1:50-100, stirring at 40-80°C for 2-4 hours, filtering, washing, and drying to obtain amino-modified ZIF-8 nanoparticles; Step 2: Add the amino-modified ZIF-8 nanoparticles into an organic environmentally friendly solvent at a mass ratio of 1:10-50, stir for 1-3 hours, and ultrasonicate for 30-120 minutes to obtain an amino-modified ZIF-8 nanoparticle dispersion.

[0016] Wherein, the organic environmentally friendly solvent is one or more of ethyl acetate, propylene glycol methyl ether acetate, diethylene glycol butyl ether, and xylene.

[0017] The functionalized modified polysiloxane is a polysiloxane that has been modified to introduce nucleophilic functional groups, amino groups (-NH 2 ), hydroxyl (-OH) and thiol (-SH) groups; Furthermore, the catalyst is one or more of dibutyltin dilaurate, dibutyltin acetate and tetrabutyl titanate.

[0018] Furthermore, the organic solvent containing organic amine is prepared by dissolving the organic amine in an organic solvent at a mass ratio of 1:2 to 10. The organic amine is aqueous ammonia, ethylenediamine, diethylenetriamine, or aminopropyltriethoxysilane; and the organic solvent is one or more of dimethylformamide, dimethyl sulfoxide, xylene, ethanol, tetrahydrofuran, and ethyl acetate.

[0019] A method for preparing a functionalized acrylic acid-modified polysiloxane heavy-duty anticorrosive coating comprises the following steps: Step 1: Add acrylic resin and organic environmentally friendly solvent to a stirrer, mix well, add amino-modified ZIF-8 nanoparticle dispersion, continue stirring for 15 to 30 minutes, add catalyst, continue stirring for 30 minutes, add functionalized modified polysiloxane, continue mixing and stirring, continue to add catalyst during this stirring process, fully react and mix well to obtain mixture 1; Step 2: Add acrylic modified polysiloxane resin, calcium carbonate, polyvinyl pyrrolidone, polyether modified siloxane, silicone, ultraviolet absorber triazine-5, histamine light stabilizer, and aminosilane into a stirrer at a speed of 500-1000 r / min and stir for 30 min, then add pigments and fillers, continue stirring at 1500-2000 r / min for 1-2 hours until the fineness is ≤30 μm, add an organic environmentally friendly solvent into the system, stir evenly at 1000 r / min, and filter to obtain a mixture II; Step 3: Add functionalized modified polysiloxane, methyl methacrylate and epoxy resin to mixture 2, stir at 500-1000 r / min for 15 min, and filter again to obtain mixture 3; Step 4: Mix mixture 1 and mixture 3, stir at 500-1000 r / min for 30-90 min, mix evenly and filter after sufficient reaction to obtain a functionalized acrylic modified polysiloxane heavy anti-corrosion coating, wherein the ratio of acrylic resin to acrylic modified polysiloxane resin is 1:0.5-2.5.

[0020] The functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating and its preparation method provided by the present invention are specifically described below through examples.

[0021] Embodiment 1: Step 1: Add acrylic resin and xylene in a stirrer at a mass ratio of 1:1, mix well, add amino-modified ZIF-8 nanoparticle dispersion, wherein the mass ratio of amino-modified ZIF-8 nanoparticle dispersion to acrylic resin is 1:20, stir for 30 minutes, add tetrabutyl titanate, continue stirring for 30 minutes, add polysiloxane containing amino groups, continue mixing and stirring, continue to add catalyst during this stirring process, fully react, mix well to obtain mixture 1, wherein acrylic resin: polysiloxane containing amino groups: tetrabutyl titanate = 1:1:0.009; Step 2: Add acrylic modified polysiloxane resin, calcium carbonate, polyvinyl pyrrolidone, polyether modified siloxane, silicone, ultraviolet absorber triazine-5, histamine-sensitive light stabilizer, and aminosilane into a stirrer, stir at a speed of 800 r / min for 30 min, then add pigments and fillers, continue stirring at 1500 r / min for 1 hour until the fineness is ≤30 μm, add xylene into the system, stir evenly at 1000 r / min, and filter to obtain a mixture 2, wherein the mass ratio of the raw materials is acrylic modified polysiloxane resin: calcium carbonate: polyvinyl pyrrolidone: polyether modified siloxane: silicone: ultraviolet absorber triazine-5: histamine-sensitive light stabilizer: aminosilane: xylene = 1: 0.02: 0.01: 0.01: 0.01: 0.02: 0.02: 0.15: 0.8; Step 3: Add amino-containing polysiloxane, methyl methacrylate and epoxy resin to mixture 2, stir at 800 r / min for 15 min, and filter again to obtain mixture 3, wherein the raw material mass ratio of acrylic modified polysiloxane resin: amino-containing polysiloxane: methyl methacrylate: epoxy resin is 1:0.1:0.2:0.12; Step 4: Mix mixture 1 and mixture 3, stir at 800 r / min for 60 min, and filter after mixing evenly and fully reacting to obtain a functionalized acrylic modified polysiloxane heavy anti-corrosion coating, wherein the ratio of acrylic resin to acrylic modified polysiloxane resin is 1:1.2.

[0022] The method for preparing the amino-modified ZIF-8 nanoparticle dispersion comprises the following steps: Step 1: adding ZIF-8 nanoparticles to an organic solvent of ammonia water: ethanol = 1:10, wherein the mass ratio of ZIF-8 nanoparticles to the organic solvent is 1:50, stirring at 60°C for 2 to 4 hours, filtering, washing, and drying to obtain amino-modified ZIF-8 nanoparticles; Step 2: Add amino-modified ZIF-8 nanoparticles into xylene at a mass ratio of 1:50, stir for 2 hours, and perform ultrasonic treatment for 60 minutes to obtain an amino-modified ZIF-8 nanoparticle dispersion.

[0023] Example 2: Step 1: Add acrylic resin and diethylene glycol butyl ether to a stirrer in a mass ratio of 1:1.1, mix well, add amino-modified ZIF-8 nanoparticle dispersion, wherein the mass ratio of amino-modified ZIF-8 nanoparticle dispersion to acrylic resin is 1:30, continue stirring for 30 minutes, add tetrabutyl titanate, continue stirring for 30 minutes, add hydroxyl-containing polysiloxane, continue mixing and stirring, continue to add tetrabutyl titanate during this stirring process, fully react, mix well to obtain a mixture 1, wherein acrylic resin: hydroxyl-containing polysiloxane: tetrabutyl titanate = 1:1.1:0.01; Step 2: Add acrylic modified polysiloxane resin, calcium carbonate, polyvinyl pyrrolidone, polyether modified siloxane, silicone, ultraviolet absorber triazine-5, histamine-sensitive light stabilizer, and aminosilane into a stirrer, stir at a speed of 800 r / min for 30 min, then add pigments and fillers, continue stirring at 1500 r / min for 1 hour until the fineness is ≤30 μm, add diethylene glycol butyl ether into the system, stir evenly at 1000 r / min, and filter to obtain a mixture 2, wherein the mass ratio of the raw materials is acrylic modified polysiloxane resin: calcium carbonate: polyvinyl pyrrolidone: polyether modified siloxane: silicone: ultraviolet absorber triazine-5: histamine-sensitive light stabilizer: aminosilane: diethylene glycol butyl ether = 1: 0.02: 0.008: 0.009: 0.01: 0.02: 0.02: 0.15: 0.8; Step 3: Add hydroxyl-containing polysiloxane, methyl methacrylate and epoxy resin to mixture 2, stir at 800 r / min for 15 min, and filter again to obtain mixture 3, wherein the mass ratio of the raw materials is acrylic modified polysiloxane resin: methyl methacrylate: epoxy resin = 1:0.2:0.12; Step 4: Mix mixture 1 and mixture 3, stir at 800 r / min for 60 min, and filter after mixing evenly and fully reacting to obtain a functionalized acrylic modified polysiloxane heavy anti-corrosion coating, wherein the ratio of acrylic resin to acrylic modified polysiloxane resin is 1:1.3.

[0024] The method for preparing the amino-modified ZIF-8 nanoparticle dispersion comprises the following steps: Step 1: adding ZIF-8 nanoparticles to an organic solvent of ethylenediamine:ethanol=1:10, wherein the mass ratio of ZIF-8 nanoparticles to the organic solvent is 1:50, stirring at 60°C for 2-4 hours, filtering, washing, and drying to obtain amino-modified ZIF-8 nanoparticles; Step 2: Add amino-modified ZIF-8 nanoparticles into diethylene glycol butyl ether at a mass ratio of 1:40, stir for 2 hours, and perform ultrasonic treatment for 60 minutes to obtain an amino-modified ZIF-8 nanoparticle dispersion.

[0025] Example 3: Step 1: Add acrylic resin and propylene glycol methyl ether acetate in a stirrer at a mass ratio of 1:1.1. After mixing evenly, add amino-modified ZIF-8 nanoparticle dispersion, wherein the mass ratio of amino-modified ZIF-8 nanoparticle dispersion to acrylic resin is 1:40. After continuous stirring for 30 minutes, add tetrabutyl titanate. After continuing stirring for 30 minutes, add polysiloxane containing amino groups, continue mixing and stirring, and continue to add tetrabutyl titanate during this stirring process. After sufficient reaction and mixing evenly, a mixture 1 is obtained, wherein the ratio of acrylic resin: polysiloxane containing amino groups: catalyst = 1:0.8:0.007; Step 2: Add acrylic modified polysiloxane resin, calcium carbonate, polyvinyl pyrrolidone, polyether modified siloxane, silicone, ultraviolet absorber triazine-5, histamine-sensitive light stabilizer, and aminosilane into a stirrer, stir at a speed of 800 r / min for 30 min, then add pigments and fillers, continue stirring at 1500 r / min for 1 hour until the fineness is ≤30 μm, add propylene glycol methyl ether acetate into the system, stir evenly at 1000 r / min, and filter to obtain a mixture 2, wherein the mass ratio of the raw materials is acrylic modified polysiloxane resin: calcium carbonate: polyvinyl pyrrolidone: polyether modified siloxane: silicone: ultraviolet absorber triazine-5: histamine-sensitive light stabilizer: aminosilane: propylene glycol methyl ether acetate = 1: 0.01: 0.007: 0.007: 0.007: 0.03: 0.03: 0.15: 0.7; Step 3: Add amino-containing polysiloxane, methyl methacrylate and epoxy resin to mixture 2, stir at 800 r / min for 15 min, and filter again to obtain mixture 3, wherein the raw material mass ratio of acrylic modified polysiloxane resin: amino-containing polysiloxane: methyl methacrylate: epoxy resin is 1:0.1:0.02:0.1; Step 4: Mix mixture 1 and mixture 3, stir at 800 r / min for 60 min, and filter after mixing evenly and fully reacting to obtain a functionalized acrylic modified polysiloxane heavy anti-corrosion coating, wherein the ratio of acrylic resin to acrylic modified polysiloxane resin is 1:1.5.

[0026] The method for preparing the amino-modified ZIF-8 nanoparticle dispersion comprises the following steps: Step 1: adding ZIF-8 nanoparticles to an organic solvent of ethylenediamine:ethanol=1:10, wherein the mass ratio of ZIF-8 nanoparticles to the organic solvent is 1:50, stirring at 60°C for 2-4 hours, filtering, washing, and drying to obtain amino-modified ZIF-8 nanoparticles; Step 2: Add amino-modified ZIF-8 nanoparticles into propylene glycol methyl ether acetate at a mass ratio of 1:40, stir for 2 hours, and perform ultrasonic treatment for 60 minutes to obtain an amino-modified ZIF-8 nanoparticle dispersion.

[0027] Experiments have shown that the functionalized acrylic polysilicone heavy-duty anticorrosive coatings obtained in Examples 1 to 3 of the present invention have high stability, good adhesion and antibacterial properties, and good weather resistance and anticorrosion properties.

[0028] The functionalized acrylic polysilicone coating obtained in Example 1 was tested and the data shown in Table 1 were obtained. Table 1 Test of functionalized acrylic polysilicone coating prepared in Example 1

[0029] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating, characterized in that: Comprising mixture 1, mixture 2 and mixture 3, The raw materials in the mixture 1 are calculated by mass ratio, wherein the mass ratio of acrylic resin to organic environmentally friendly solvent is 1:0.5-4, the mass ratio of amino-modified ZIF-8 nanoparticle dispersion to acrylic resin is 1:10-50, and the mass ratio of acrylic resin to functionalized modified polysiloxane to catalyst is 1:0.5-1.2:0.005-0.02; The raw materials in the second mixture are calculated by mass ratio, wherein acrylic modified polysiloxane resin: calcium carbonate: polyvinyl pyrrolidone: polyether modified siloxane: silicone: ultraviolet absorber triazine-5: histamine light stabilizer: aminosilane: organic environmentally friendly solvent = 1: 0.01~0.08: 0.005~0.025: 0.005~0.025: 0.005~0.025: 0~0.08: 0~0.08: 0.12~0.2: 0.7~1.5; The raw materials in the mixture three are calculated by mass ratio, and functionalized modified polysiloxane, methyl methacrylate, and epoxy resin are added to the mixture two, wherein the acrylic modified polysiloxane resin from the mixture two: functionalized modified polysiloxane: methyl methacrylate: epoxy resin = 1:0~0.25: 0.02~0.3: 0.08~0.

15.

2. The functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating according to claim 1, characterized in that: The method for preparing the amino-modified ZIF-8 nanoparticle dispersion comprises the following steps: Step 1: adding ZIF-8 nanoparticles to an organic solvent containing an organic amine at a mass ratio of 1:50-100, stirring at 40-80°C for 2-4 hours, filtering, washing, and drying to obtain amino-modified ZIF-8 nanoparticles; Step 2: Add the amino-modified ZIF-8 nanoparticles into an organic environmentally friendly solvent at a mass ratio of 1:10-50, stir for 1-3 hours, and ultrasonicate for 30-120 minutes to obtain an amino-modified ZIF-8 nanoparticle dispersion.

3. The functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating according to claim 1, characterized in that: The organic environmentally friendly solvent is one or more of ethyl acetate, propylene glycol methyl ether acetate, diethylene glycol butyl ether, and xylene.

4. The functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating according to claim 1, characterized in that: The functionally modified polysiloxane is a polysiloxane that has been modified to introduce a nucleophilic functional group, one or more of an amino group (-NH2), a hydroxyl group (-OH) and a thiol group (-SH).

5. The functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating according to claim 1, characterized in that: The catalyst is one or more of dibutyltin dilaurate, dibutyltin acetate and tetrabutyl titanate.

6. The functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating according to claim 2, characterized in that: The organic solvent containing organic amine is prepared by dissolving the organic amine in an organic solvent at a mass ratio of 1:2-10. The organic amine is aqueous ammonia, ethylenediamine, diethylenetriamine, or aminopropyltriethoxysilane; and the organic solvent is one or more of dimethylformamide, dimethyl sulfoxide, xylene, ethanol, tetrahydrofuran, and ethyl acetate.

7. A method for preparing a functionalized acrylic modified polysiloxane heavy-duty anticorrosive coating according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1: Add acrylic resin and organic environmentally friendly solvent to a stirrer, mix well, add amino-modified ZIF-8 nanoparticle dispersion, continue stirring for 15 to 30 minutes, add catalyst, continue stirring for 30 minutes, add functionalized modified polysiloxane, continue mixing and stirring, continue to add catalyst during this stirring process, fully react and mix well to obtain mixture 1; Step 2: Add acrylic modified polysiloxane resin, calcium carbonate, polyvinyl pyrrolidone, polyether modified siloxane, silicone, ultraviolet absorber triazine-5, histamine light stabilizer, and aminosilane into a stirrer at a speed of 500-1000 r / min and stir for 30 min, then add pigments and fillers, continue stirring at 1500-2000 r / min for 1-2 hours until the fineness is ≤30 μm, add an organic environmentally friendly solvent into the system, stir evenly at 1000 r / min, and filter to obtain a mixture II; Step 3: Add functionalized modified polysiloxane, methyl methacrylate and epoxy resin to mixture 2, stir at 500-1000 r / min for 15 min, and filter again to obtain mixture 3; Step 4: Mix mixture 1 and mixture 3, stir at 500-1000 r / min for 30-90 min, mix evenly and filter after sufficient reaction to obtain a functionalized acrylic modified polysiloxane heavy anti-corrosion coating, wherein the ratio of acrylic resin to acrylic modified polysiloxane resin is 1:0.5-2.5.

Citation Information

Patent Citations

  • Filling modification polyurethane membrane and preparation method thereof

    CN109126485A

  • Preparation method of high-corrosion-resistance modified epoxy resin composite coating

    CN112341900A

  • Acrylic acid modified polysiloxane coating and preparation method thereof

    CN113817349A