Wax crystal inhibitor as well as preparation method and application thereof
The existing wax crystal inhibitor was solved by combining octadecyl acrylate, maleic anhydride, vinyl ester and 1-amino-10-undecene with styrene-ethylene-butene block copolymers. The problem of low agent performance significantly improves the dispersion and fluidity of wax crystals, prevents wax crystals from aggregating and precipitating, and improves the efficiency of crude oil transportation and equipment stability.
Patent Information
- Application Number
- CN202411153604.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-15
AI Technical Summary
The existing wax crystal inhibitors have low efficacy, resulting in the precipitation of wax during crude oil transportation seriously affecting liquidity and equipment transportation efficiency.
The wax crystal inhibitor is prepared by condensation reaction by combining octadecyl acrylate, maleic anhydride, vinyl ester and 1-amino-10-undecene with styrene-ethylene-butene block copolymer. -10-undecene reduces interfacial tension, and styrene-ethylene-butene block copolymer improves fluidity and stability.
It significantly improves the dispersion and fluidity of wax crystals, reduces the aggregation and precipitation of wax crystals, prevents blockage, and improves the efficiency of crude oil transportation and the stability of equipment.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of wax crystal inhibitors, and in particular to a wax crystal inhibitor and a preparation method and application thereof. Background Art
[0002] Wax crystal inhibitors are a class of chemicals used to prevent wax precipitation in crude oil and are widely used in the oil and gas industry. Crude oil transportation refers to the process of transporting crude oil from production sites (such as oil fields) to refineries, storage facilities or consumer markets through pipelines, ships, railways or roads. During transportation, wax in crude oil is prone to precipitate to form wax crystals, causing pipeline blockage or equipment failure, thereby affecting the fluidity and transportation efficiency of crude oil. However, the wax crystal inhibitors currently used are generally less effective, wax crystals are not effectively inhibited, and the deposition and aggregation of wax crystals seriously affect the crude oil transportation process. Therefore, the development of a high-efficiency wax crystal inhibitor is an urgent problem that needs to be solved. Summary of the invention
[0003] The invention provides a wax crystal inhibitor and a preparation method and application thereof, which solves the problem of low efficiency of the wax crystal inhibitor in the related art.
[0004] The technical scheme of the present invention is as follows: The present invention proposes a wax crystal inhibitor and a preparation method and application thereof, a wax crystal inhibitor comprising the following component raw materials in parts by weight: 30-35 parts of octadecyl acrylate, 20-22 parts of maleic anhydride, 5-10 parts of vinyl ester, 15-25 parts of 1-amino-10-undecene, 12-15 parts of styrene-ethylene-butylene block copolymer, 2-4 parts of initiator, and 120-160 parts of solvent.
[0005] As a further technical solution, the styrene-ethylene-butylene block copolymer consists of a first styrene-ethylene-butylene block copolymer and a second styrene-ethylene-butylene block copolymer, and the first styrene-ethylene-butylene block copolymer and the second styrene-ethylene-butylene block copolymer have different Shore hardnesses.
[0006] As a further technical solution, the Shore hardness of the first styrene-ethylene-butylene block copolymer is 50, and the Shore hardness of the second styrene-ethylene-butylene block copolymer is 69.
[0007] As a further technical solution, the mass ratio of the first styrene-ethylene-butylene block copolymer to the second styrene-ethylene-butylene block copolymer is 1:2-4.
[0008] As a further technical solution, the mass ratio of the first styrene-ethylene-butylene block copolymer to the second styrene-ethylene-butylene block copolymer is 1:3.
[0009] As a thermoplastic elastomer, styrene-ethylene-butylene block copolymer has good elasticity and can maintain performance under low temperature conditions, effectively improving the stability of wax crystal inhibitors under low temperature environments. By limiting the Shore hardness of styrene-ethylene-butylene block copolymers, the balance between fluidity and inhibitory effect is sought to obtain the best wax crystal inhibitor.
[0010] As a further technical solution, the mass ratio of octadecyl acrylate, maleic anhydride, vinyl ester, and 1-amino-10-undecene is 6:4:1:3-5.
[0011] As a further technical solution, the mass ratio of octadecyl acrylate, maleic anhydride, vinyl ester, and 1-amino-10-undecene is 6:4:1:4.
[0012] As a further technical solution, the initiator includes one or more of tert-butyl perbenzoate, azobisisobutylcyanide, and benzoyl peroxide.
[0013] As a further technical solution, the solvent includes one or more of toluene, xylene, and trimethylbenzene.
[0014] The present invention also provides a method for preparing a wax crystal inhibitor, comprising the following steps: S1, dissolving octadecyl acrylate, maleic anhydride, vinyl ester, and 1-amino-10-undecene in a solvent, adding an initiator and stirring evenly, and condensing the reaction to obtain a copolymer I; S2. Fully mix the copolymer I and the styrene-ethylene-butylene block copolymer to obtain a wax crystal inhibitor.
[0015] As a further technical solution, the stirring temperature is 70-90°C.
[0016] As a further technical solution, the stirring time is 1.5 to 2.5 hours.
[0017] The invention also provides application of the wax crystal inhibitor or the wax crystal inhibitor obtained by the preparation method in the petroleum industry.
[0018] The working principle and beneficial effects of the present invention are: In the present invention, octadecyl acrylate, maleic anhydride, vinyl ester, and 1-amino-10-undecene are selected as monomers, which are polymerized and mixed with styrene-ethylene-butylene block copolymer to form a polymer wax crystal inhibitor. 1-amino-10-undecene can effectively reduce the interfacial tension between the liquid and the wax crystal, improve the dispersibility of the wax crystal, reduce aggregation and precipitation, and the amino group enables the substance to form a strong chemical bond with the surface of the wax crystal to prevent the growth of the wax crystal; the styrene-ethylene-butylene block copolymer has good elasticity and flexibility, so that it can adapt to different flow conditions, effectively improve the fluidity of the fluid, and prevent blockage caused by the deposition of wax crystals. DETAILED DESCRIPTION
[0019] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] In the following examples and comparative examples: The first styrene-ethylene-butylene block copolymer: Shore hardness is 50, model is G2832 GS-N, manufacturer is Kraton Performance Polymers; The first styrene-ethylene-butylene block copolymer: Shore hardness is 69, model is G1652 MU, and the manufacturer is Kraton High Performance Polymers.
[0021] Example 1 S1, weigh 30 parts of octadecyl acrylate, 20 parts of maleic anhydride, 5 parts of vinyl ester, 12 parts of 1-amino-10-undecene, add 120 parts of toluene, stir until fully dissolved, heat to 70°C, add 2 parts of tert-butyl oxybenzoate, condense and reflux for 2.5 hours to obtain copolymer I; S2. The copolymer I and 12 parts of styrene-ethylene-butylene block copolymer (model G1645 VO, Shore strength 35, manufactured by Kraton High Performance Polymers) are mixed thoroughly to obtain a wax crystal inhibitor.
[0022] Example 2 S1, weigh 32 parts of octadecyl acrylate, 21 parts of maleic anhydride, 8 parts of vinyl ester, 12 parts of 1-amino-10-undecene, add 140 parts of xylene, stir until fully dissolved, heat to 80°C, add 3 parts of azobisisobutyl cyanide, condense and reflux for 2h to obtain copolymer I; S2. The copolymer I and 13 parts of styrene-ethylene-butylene block copolymer (model G1645 VO, Shore strength 35, manufactured by Kraton High Performance Polymers) are fully mixed to obtain a wax crystal inhibitor.
[0023] Example 3 S1, weigh 35 parts of octadecyl acrylate, 22 parts of maleic anhydride, 10 parts of vinyl ester, 12 parts of 1-amino-10-undecene, add 160 parts of trimethylbenzene, stir until fully dissolved, heat to 90°C, add 4 parts of benzoyl peroxide, condense and reflux for 1.5 hours to obtain copolymer I; S2. The copolymer I and 15 parts of styrene-ethylene-butylene block copolymer (model G1645 VO, Shore strength 35, manufactured by Kraton High Performance Polymers) are fully mixed to obtain a wax crystal inhibitor.
[0024] Example 4 Compared with Example 1, the difference in Example 4 is that the added amount of 1-amino-10-undecene is 15 parts.
[0025] Example 5 Compared with Example 1, the difference in Example 5 is that the added amount of 1-amino-10-undecene is 20 parts.
[0026] Example 6 Compared with Example 1, the difference in Example 6 is that the added amount of 1-amino-10-undecene is 25 parts.
[0027] Example 7 Compared with Example 1, the difference in Example 7 is that the added amount of 1-amino-10-undecene is 30 parts.
[0028] Example 8 Compared with Example 5, Example 8 is different in that 12 parts of styrene-ethylene-butylene block copolymer (model G1645 VO, Shore strength 35, manufactured by Kraton High Performance Polymers) are replaced by an equal amount of the first styrene-ethylene-butylene block copolymer.
[0029] Example 9 Compared with Example 5, Example 9 is different in that 12 parts of styrene-ethylene-butylene block copolymer (model G1645 VO, Shore strength 35, manufactured by Kraton High Performance Polymers) are replaced with an equal amount of a second styrene-ethylene-butylene block copolymer.
[0030] Example 10 Compared with Example 5, the difference of Example 10 is that 12 parts of styrene-ethylene-butylene block copolymer (model G1645 VO, Shore strength of 35, manufactured by Kraton High Performance Polymers) are replaced by an equal amount of styrene-ethylene-butylene block copolymer (model G1650 M, Shore strength of 72, manufactured by Kraton High Performance Polymers).
[0031] Embodiment 11 Compared with Example 8, Example 11 is different in that 12 parts of the first styrene-ethylene-butylene block copolymer are replaced by 6 parts of the first styrene-ethylene-butylene block copolymer and 6 parts of the second styrene-ethylene-butylene block copolymer.
[0032] Example 12 Compared with Example 8, Example 12 is different in that 12 parts of the first styrene-ethylene-butylene block copolymer are replaced by 4 parts of the first styrene-ethylene-butylene block copolymer and 8 parts of the second styrene-ethylene-butylene block copolymer.
[0033] Example 13 Compared with Example 8, Example 13 is different in that 12 parts of the first styrene-ethylene-butylene block copolymer are replaced by 3 parts of the first styrene-ethylene-butylene block copolymer and 9 parts of the second styrene-ethylene-butylene block copolymer.
[0034] Embodiment 14 Compared with Example 8, Example 14 is different in that 12 parts of the first styrene-ethylene-butylene block copolymer are replaced by 2.4 parts of the first styrene-ethylene-butylene block copolymer and 9.6 parts of the second styrene-ethylene-butylene block copolymer.
[0035] Embodiment 15 Compared with Example 8, Example 15 is different in that 12 parts of the first styrene-ethylene-butylene block copolymer are replaced by 2 parts of the first styrene-ethylene-butylene block copolymer and 10 parts of the second styrene-ethylene-butylene block copolymer.
[0036] Comparative Example 1 Compared with Example 1, Comparative Example 1 is different in that 1-amino-10-undecene is not added.
[0037] The samples prepared in Examples 1 to 15 and Comparative Example 1 were tested as follows: 1. Wax prevention rate: According to the test method specified in A.6.1 of SY / T 6300-2009 "Technical Requirements for Cleaners and Wax Inhibitors for Oil Production", the wax prevention rate of the samples was tested. The test results are shown in Table 1.
[0038] 2. Fluidity: The natural gas condensate sample was cooled to -18°C in a stainless steel cup and kept for 2 hours. The flow state of the condensate was observed. The amount of paraffin inhibitor added was 0 ppm, 100 ppm, and 300 ppm, respectively. The test results are shown in Table 2.
[0039] Table 1 Wax prevention rate test results of wax crystal inhibitors prepared in Examples 1 to 15 and Comparative Example 1
[0040] Table 2 Fluidity test results of wax crystal inhibitors prepared in Example 1, Example 13 and Comparative Example 1
[0041] Compared with Comparative Example 1, Example 1 adds 1-amino-10-undecene. As a result, the anti-wax rate and fluidity of Example 1 are better than those of Comparative Example 1, indicating that the addition of 1-amino-10-undecene can enhance the anti-wax effect and fluidity of the wax crystal inhibitor.
[0042] Compared with Example 1, Examples 4 to 7 added different amounts of 1-amino-10-undecene, and the wax resistance rates of Examples 4 to 6 were better than those of Example 1, indicating that when the mass ratio of octadecyl acrylate, maleic anhydride, vinyl ester, and 1-amino-10-undecene was 6:4:1:3 to 5, and the preferred ratio was 6:4:1:4, the wax resistance rate of the obtained wax crystal inhibitor was higher.
[0043] Compared with Example 5, Examples 8 to 10 added styrene-ethylene-butylene block copolymers with different Shore strengths. As a result, the wax resistance rates of Examples 8 and 9 were higher than those of Examples 5 and 10, indicating that when the Shore strength of the styrene-ethylene-butylene block copolymer was 50 to 69, the wax crystal inhibitor had a better wax resistance effect.
[0044] Compared with Example 8, Examples 11 to 15 simultaneously added the first styrene-ethylene-butylene block copolymer and the second styrene-ethylene-butylene block copolymer. As a result, the anti-wax rate of Examples 11 to 15 was better than that of Example 8, indicating that the first styrene-ethylene-butylene block copolymer and the second styrene-ethylene-butylene block copolymer played a synergistic role and could further enhance the anti-wax effect of the wax crystal inhibitor.
[0045] Compared with Example 11, Examples 12 to 15 added the first styrene-ethylene-butylene block copolymer and the second styrene-ethylene-butylene block copolymer in different mass ratios. As a result, the anti-wax rates of Examples 12 to 14 were better than those of Examples 11 and 15, indicating that when the mass ratio of the first styrene-ethylene-butylene block copolymer and the second styrene-ethylene-butylene block copolymer is 1:2 to 4, and the preferred ratio is 1:3, the anti-wax effect of the obtained wax crystal inhibitor is the best.
[0046] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A wax crystal inhibitor, It is characterized in that The invention comprises the following raw materials in parts by weight: 30-35 parts of octadecyl acrylate, 20-22 parts of maleic anhydride, 5-10 parts of vinyl ester, 15-25 parts of 1-amino-10-undecene, 12-15 parts of styrene-ethylene-butylene block copolymer, 2-4 parts of initiator and 120-160 parts of solvent.
2. A wax crystal inhibitor according to claim 1, It is characterized in that The styrene-ethylene-butylene block copolymer consists of a first styrene-ethylene-butylene block copolymer and a second styrene-ethylene-butylene block copolymer, and the first styrene-ethylene-butylene block copolymer and the second styrene-ethylene-butylene block copolymer have different Shore hardnesses.
3. A wax crystal inhibitor according to claim 2, It is characterized in that The first styrene-ethylene-butylene block copolymer has a Shore hardness of 50, and the second styrene-ethylene-butylene block copolymer has a Shore hardness of 69.
4. A wax crystal inhibitor according to claim 2, It is characterized in that The mass ratio of the first styrene-ethylene-butylene block copolymer to the second styrene-ethylene-butylene block copolymer is 1:2-4.
5. A wax crystal inhibitor according to claim 1, It is characterized in that The initiator includes one or more of tert-butyl perbenzoate, azobisisobutyl cyanide, and benzoyl peroxide.
6. A wax crystal inhibitor according to claim 1, It is characterized in that The solvent includes one or more of toluene, xylene and trimethylbenzene.
7. A method for preparing a wax crystal inhibitor according to any one of claims 1 to 6, It is characterized in that The following steps are involved: S1, dissolving octadecyl acrylate, maleic anhydride, vinyl ester, and 1-amino-10-undecene in a solvent, adding an initiator and stirring evenly, and condensing the reaction to obtain a copolymer I; S2. Fully mix the copolymer I and the styrene-ethylene-butylene block copolymer to obtain a wax crystal inhibitor.
8. The method for preparing a wax crystal inhibitor according to claim 7, It is characterized in that The stirring temperature is 70-90°C.
9. The method for preparing a wax crystal inhibitor according to claim 7, It is characterized in that The stirring time is 1.5 to 2.5 hours.
10. Use of the wax crystal inhibitor according to any one of claims 1 to 6 or the wax crystal inhibitor obtained by the preparation method according to any one of claims 7 to 9 in the petroleum industry.