Operation method of blast furnace after using high-aluminum material

By adjusting the permeability of the column, the heat of the furnace cylinder and the composition of the slag, the problems of increasing the viscosity of the slag and reducing the grade of the furnace after using high-aluminum materials in the blast furnace are solved, and the stability and cost of the smelting process are reduced, ensuring the production of the blast furnace Efficiency and quality.

CN118957185APending Publication Date: 2024-11-15山西建龙实业有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411037966.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

After using high aluminum material in the blast furnace, the slag viscosity increases, the grade of the furnace is reduced, the drum index and low-temperature reduction powdering rate decrease, affecting the smelting quality and the stability of the furnace.

Method used

By adjusting the air permeability of the material column, ensuring sufficient heat in the furnace cylinder and reasonably adjusting the slag composition, including optimizing the complementarity of raw materials and fuel, giving full play to the role of block ore drying and screening, strengthening screening under the tank, stabilizing the air volume into the furnace, and improving gas utilization and furnace temperature control, and reasonably adjust the dolomite powder ratio in sintered ore to ensure that the R4 alkalinity and R2 alkalinity of the slag are within the appropriate range.

Benefits of technology

The stability and cost reduction of the blast furnace smelting process are achieved, the furnace condition is continuously stable, the cost of molten iron is reduced, and the viscosity and magnesium-aluminum ratio of the slag are within the appropriate range, ensuring the production efficiency and quality of the blast furnace.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957185A_ABST
    Figure CN118957185A_ABST
Patent Text Reader

Abstract

The invention relates to the field of blast furnace smelting, in particular to the field of high-aluminum material smelting. The invention relates to an operation method for a blast furnace after using a high-aluminum material, which adopts adjustment measures and stabilizes the furnace condition from three aspects of material column air permeability, ensuring sufficient heat of a hearth and reasonably adjusting slag components, and specifically comprises the following contents: in the aspect of material column air permeability, keeping complementation of raw materials and fuel, fully playing roles of lump ore drying and screening and strengthening screening under a tank; the furnace inlet air volume is stabilized, and the furnace front ditch repairing period is adjusted to enhance the material column air permeability; in the aspect of ensuring sufficient heat of the hearth, sufficient heat of the hearth is ensured from improvement of coal gas utilization and reasonable control of the furnace temperature; in the aspect of reasonable adjustment of slag components, when high-aluminum powder is matched and used for sintering to form a high-aluminum material, the proportion of dolomite powder in sintered ore is synchronously increased, the alkalinity of R4 is ensured to be 1.02 + / -0.02, the alkalinity of slag R2 is ensured to be 1.22 + / -0.02, and the viscosity of the slag at 1500 DEG C is smaller than or equal to 0.400 Pa.s.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of blast furnace smelting, in particular to the field of high-aluminum material smelting. Background Art

[0002] There is room for cost reduction when a certain proportion of high-aluminum materials are added to the blast furnace. For example, adding Sierra Leone powder and / or laterite nickel ore to the sintered ore can reduce the cost of ore materials. Too low a magnesium-aluminum ratio will cause the slag to be too viscous and difficult to remove, which will seriously affect the quality of steel. In addition, the ratio of magnesium oxide to aluminum oxide in the sintered ore will also directly affect the smelting temperature of the blast furnace. Therefore, in order to ensure the smelting quality, when the mass percentage of alumina in the sintered ore increases, the mass percentage of magnesium oxide also needs to be provided.

[0003] As the mass percentage of alumina and magnesia in sintered ore increases, the drum index of the blast furnace will decrease, and the low-temperature reduction powder rate RDI +3.15 The 500℃ low-temperature reducibility index will be reduced, which will affect the permeability of the upper part of the blast furnace. At the same time, the increase in the mass percentage of aluminum oxide in the slag is not conducive to desulfurization, and the viscosity increases, and the slag-iron ratio is significantly improved.

[0004] In summary, after using high-aluminum materials in the blast furnace, the grade entering the furnace decreases, the slag viscosity increases, and the rising resistance of the coal gas flow in the middle and lower parts of the blast furnace increases, affecting the stability of the furnace condition. Summary of the invention

[0005] The technical problem to be solved by the present invention is: how to ensure stable smelting of the blast furnace after using high-aluminum materials (the mass percentage of alumina in the sintered ore is greater than 2.4%), and solve various drawbacks produced after using high-aluminum materials in the blast furnace.

[0006] The technical solution adopted by the present invention is: an operating method for a blast furnace using high-aluminum materials, taking adjustment measures from three aspects: material column permeability, ensuring sufficient heat in the furnace, and reasonably adjusting the slag composition to stabilize the furnace condition, specifically including the following contents:

[0007] In terms of the air permeability of the material column: maintain the complementarity between raw materials and fuel, give full play to the role of lump ore drying and screening, strengthen the screening under the trough, stabilize the air volume entering the furnace, and adjust the cycle of repairing trenches in front of the furnace to enhance the air permeability of the material column;

[0008] To ensure sufficient heat in the furnace: improve gas utilization and reasonably control furnace temperature to ensure sufficient heat in the furnace; to reasonably adjust slag composition: when using high-aluminum powder to form high-aluminum material during sintering, increase the proportion of dolomite powder in the sintered ore simultaneously to ensure that the R4 basicity is 1.02±0.02, the slag R2 basicity is 1.22±0.02, and the slag viscosity is ≤0.400Pa.s at 1500℃.

[0009] Maintaining the complementarity between raw materials and fuel refers to optimizing and improving the quality of pulverized coal while stabilizing the mainstream coke structure. The stabilizing the mainstream coke structure refers to adopting a 25% water quenching + 75% dry quenching structure. The optimizing and improving the quality of pulverized coal refers to ensuring that the high calorific value of the injected coal is maintained above 7500kCal / kg, and that the pulverized coal equal to 200 mesh accounts for more than 70% of the total pulverized coal in terms of mass percentage.

[0010] The said giving full play to the role of lump ore drying and screening means that the moisture content of the lump ore drying is ≤2.00% by mass, the powder entering the furnace is ≤3.0% by mass, the lump ore drying furnace temperature is 650-700° C., and the roller screen is a square hole screen with an aperture of 5 mm×10 mm.

[0011] The enhanced under-trough screening refers to adjusting the opening of the under-trough material flow gate and the amplitude of the vibrator, so that, by mass percentage, the coke is less than 15kg / s, the pellets are less than 20kg / s, the sintered ore is less than 30kg / s, and the powder entering the furnace is ≤3.0%, where the powder entering the furnace refers to the particle size of the material entering the furnace being less than 5mm.

[0012] The stable air volume entering the furnace refers to reducing the blast furnace coal ratio, reducing the coke load, and reducing the wind pressure, so that the average air volume entering the furnace is 3101±110m3 / min and the actual average wind speed is 258.4±10m / s.

[0013] The improved coal gas utilization refers to improving coal gas utilization from two aspects: ore batch adjustment and charging matrix adjustment. The ore batch adjustment refers to the ore batch being increased to: 45.0-48.0t / batch, and the ore batch size being adjusted according to the number of charging cars 32±1 cars / h; the charging matrix adjustment refers to changing the blast furnace charging method from A+B to A+2B, reducing the ore platform width from 8° to 6°, keeping the coke platform width unchanged, and adjusting the ore-coke angle difference from 1.34° to 1.31°, wherein A represents CC↓00↓, B represents CC↓00↓00↓, CC↓ represents 2 cars of coke, 00↓ represents 2 cars of ore, and 2B represents that the B charging sequence is executed twice per cycle.

[0014] The reasonable control of the furnace temperature means that the physical heat of the molten iron is not lower than 1490°C.

[0015] The beneficial effect of the present invention is that the sintered ore of the present invention is matched with high-aluminum ore (such as Sierra Leone powder and laterite nickel ore), thereby reducing the cost of iron ore. After the blast furnace uses high-aluminum materials, although the grade of the blast furnace is reduced by the present invention, resulting in a decrease in the blast furnace output, the furnace condition remains stable, and the cost is reduced while the smelting is completed. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a graph showing the changes in ω(Al2O3) in sintered ore after sintering with Sierra Leone powder and laterite nickel ore;

[0017] Figure 2 This is the change of slag ω(Al2O3) after using high aluminum material in blast furnace;

[0018] Figure 3 This is the change diagram of ω(TFe) entering the blast furnace after sintering with high-alumina ore powder;

[0019] Figure 4 This is the change chart of high calorific value of PCI coal;

[0020] Figure 5 It is the graph of the change of the air volume entering the furnace and the actual wind speed;

[0021] Figure 6 It is a graph showing the relationship between batch weight and pressure drop;

[0022] Figure 7 It is the graph of the physical heat of molten iron and the change of ω[Si] content;

[0023] Figure 8 It is the variation diagram of ω(Al2O3) and ω(MgO) in slag;

[0024] Fig. 9 It is the variation diagram of slag R2, R4 and magnesium-aluminum ratio;

[0025] Fig.10 This is a comparison chart of changes in fuel ratio and coal ratio. DETAILED DESCRIPTION

[0026] Shanxi Jianlong 5 # Furnace capacity 1080m 3 , adopting a bell-less furnace top, material loading by material car, and configuring north and south iron-making yards. In September 2023, through the industry's advanced cost benchmarking, the blast furnace has room for cost reduction by matching a certain proportion of high-aluminum materials. In view of the drawbacks of high-aluminum slag, the blast furnace has been optimized and adjusted through operating measures, the furnace condition has been stabilized, the coal ratio has reached 172.4kg / t, the fuel ratio is 515.6kg / t, and the molten iron cost has been reduced by 36.46 yuan / t, achieving the goal of cost reduction.

[0027] 1. The impact of high aluminum material use on blast furnace operation

[0028] 1.1 High-aluminum materials used in blast furnaces from October to November 2023

[0029] 1) On October 18, the sintering reduced the refined powder by 9.0%, and replaced it all with Sierra Leone powder with ω(Al2O3)=7.68%. The chemical composition of Sierra Leone powder is shown in Table 1, where ω refers to the mass percentage.

[0030] Table 1 Chemical composition of Sierra Leone powder (mass fraction) %

[0031]

[0032] 2) On November 15, the blast furnace was changed to 8% ω(Al2O3)=7.37% Sierra Leone block. The chemical composition of Sierra Leone block is shown in Table 2.

[0033] Table 2 Chemical composition of Sierra Leone block (mass fraction) %

[0034]

[0035] 3) On November 22, the sintering reduced the fine powder by 3.0%, and all of it was replaced by laterite nickel ore with ω(Al2O3)=9.01%. The chemical composition of the laterite nickel ore is shown in Table 3.

[0036] Table 3 Chemical composition of laterite nickel ore (mass fraction) %

[0037]

[0038] 1.2 Disadvantages of using high-alumina ore in blast furnaces

[0039] 1.2.1 Decrease in sinter quality

[0040] After sintering with Sierra Leone powder and laterite nickel ore, the ω(Al203) of the sintered ore increased to an average of 2.47% and a maximum of 2.73%. Figure 1 .

[0041] In view of the increase of ω(Al203) in the slag, the magnesium-aluminum ratio was increased, and the ω(Mg0) of the sintered ore was increased from 2.20% to 2.40%~2.50%, and the highest was 2.70%~2.80%; the ω(Al2O3) and ω(MgO) in the sintered ore increased, and its drum index dropped from 76.75% to 75.68%, and the low-temperature reduction powder rate RDI +3.15 From 70.77% to 70.40%. The sinter drum index and 500℃ low-temperature reducibility index decreased, affecting the permeability of the upper part of the blast furnace.

[0042] 1.2.2 Increased slag viscosity

[0043] After using high aluminum materials in blast furnace, the slag ω(Al2O3) increased, with an average of 16.0% and a maximum of 17.04%. The changes in slag ω(Al2O3) are shown in Figure 2 .

[0044] The increase of ω(Al2O3) in slag is not conducive to desulfurization and the viscosity increases; at 1500℃, the slag viscosity increases from 0.209Pa.s to 0.460Pa.s; both the slag viscosity mutation point temperature and viscosity increase. The changes in slag mutation point temperature and viscosity are shown in Table 4.

[0045] Table 4 Changes in slag mutation point temperature and viscosity

[0046] <![CDATA[ω(A12O3) / %]]> Temperature / ℃ Viscosity / Pa·s 15.34 1334 0.461 16.62 1341 0.757 17.02 1371 0.805

[0047] 1.2.3 Reduced furnace quality

[0048] After sintering with high-alumina ore powder, the ω(TFe) of sintered ore dropped from 56.64% to 55.87%, and the ω(TFe) of blast furnace dropped from 57.56% to 56.66%. On November 15, Sierra Leone blocks were used in the blast furnace, and the ω(TFe) of blast furnace dropped more significantly, to 56.20%. For details, see Figure 3 ; The slag-iron ratio increased from 351.50kg / t to 370.20kg / t; After the blast furnace uses aluminum material, the furnace grade is reduced, the slag viscosity increases, the upward resistance of the coal gas flow in the middle and lower parts of the blast furnace increases, affecting the stability of the furnace condition, and the coke ratio of the blast furnace increases. Among them, the resistance loss of the softening zone in the lower part of the furnace body and the waist part accounts for about 25% of the total resistance loss; the resistance loss in the lower part of the blast furnace that affects the molten dripping performance accounts for about 60% of the total resistance loss.

[0049] Improvement measures of the present invention

[0050] The effects of high aluminum materials on blast furnace operation can be summarized as follows: 1) The ω(Al2O3) in the slag is high, and the slag viscosity increases; 2) The furnace grade is reduced, affecting the permeability of the charge in the middle and lower parts of the blast furnace and the permeability of the liquid slag; 3) The sintering ω(Al2O3) and ω(Mg0) increase, and the sintering drum index and low-temperature reduction powder rate RDI+ 3.1 5 decreases, affecting the permeability of the upper charge of the blast furnace; 4) When the slag ω(Al2O3) ≥14.0%, the sensitivity of the slag to temperature and the viscosity of the slag decrease with increasing temperature, and the fluidity increases with decreasing viscosity. The relationship is in the form of Arrhenius law as shown in formula (1).

[0051]

[0052] Where: 1) η--viscosity, Pa.s; 2) A η -- coefficient, depending on the composition of the slag; 3) E η --Activation energy of viscous flow, J / mol; 4) R--molar constant, J / mol.K; 5) T--temperature, ℃.

[0053] To address the above-mentioned drawbacks of high-aluminum slag, optimization and adjustment measures are taken from three aspects: physical heat of molten iron, slag composition, and permeability of the material column to stabilize the furnace conditions and achieve the goal of orderly reducing costs.

[0054] 2.1 Improve the air permeability of the column

[0055] 2.1.1 Maintaining complementarity between raw materials and fuel

[0056] Blast furnace operation is "70% raw materials and 30% operation", so improving raw materials is a prerequisite for ensuring stable blast furnace production and improving technical indicators; ensuring the coke skeleton is the basis for stable furnace conditions.

[0057] 2.1.1.1 Stable mainstream focal structure

[0058] 1) All coke in our factory is purchased from outside, which is greatly affected by the market. We give full play to the advantages of customized coke and long-term contract coke to meet the 25% water-quenched coke + 75% dry-quenched coke structure; the integration and optimization of coke resources, blast furnace coke is stabilized at 4 companies, with a reasonable structure. The blast furnace coke matching situation is shown in Table 5.

[0059] Table 5 Blast furnace coke matching

[0060] name Ratio / % Ad / % St.d / % Moisture / % Reactivity / % Strength after reaction / % M10 / % M25 / % Remark A 25 12.23 0.66 0.2 20.00 70.75 5.1 92.70 Dry quenching (top installation) B 25 12.56 0.71 0.2 21.96 67.74 5.48 92.29 Dry quenching (top installation) C 25 12.71 0.66 0.2 25.51 65.35 5.42 92.12 Dry quenching (ramming) D 25 12.3 0.72 8.5 24.94 66.04 5.92 92.10 Water quenching (tamping)

[0061] 2) The blast furnace is loaded with material cars, and the order of coke entering the furnace is optimized: coke (C+D) is the first car, and coke (A+B) is the second car, which are placed in a relatively central position to ensure the quality of the central coke and stabilize the central airflow.

[0062] 2.1.1.2 Optimizing and improving coal powder quality

[0063] The quality of pulverized coal for blast furnace injection fluctuated (the high calorific value of coal was 7472 kCal / kg on October 24, 7484 kCal / kg on November 6, and 7492 kCal / kg on November 19). On the one hand, we continued to pay attention to the quality of pulverized coal entering the factory, and on the other hand, we adjusted the ratio of bituminous coal to anthracite to 55:45 to ensure that the high calorific value of pulverized coal for blast furnace injection remained above 7500 kCal / kg. The changes in the high calorific value of pulverized coal for blast furnace injection can be seen in Figure 2. Figure 4 ; Coal powder ω (-200 mesh) is maintained above 70%.

[0064] 2.1.2 Give full play to the role of lump ore drying and screening

[0065] Our factory has established and put into use a lump ore drying and screening system in the raw material yard, with the following parameters: 1) The furnace temperature is controlled at 650~700℃, and the exhaust gas temperature is controlled at 80~110℃; 2) The feed rate is controlled at 350~400t / h, and the moisture content after drying is controlled at ≤2.00%; 3) The roller screen is a square hole screen with a length of 1.5m and an aperture of 5mm×10mm.

[0066] Lump ore drying and screening have the following effects on furnace condition stability: 1) The moisture content of lump ore during drying is ≤2.00%, which is conducive to the screening and removal of lump ore powder and reduces the amount of powder entering the furnace; 2) When the lump ore drying furnace temperature is between 650 and 700°C, the crystal water of the lump ore evaporates, causing cracks and powderization. The lump ore is screened before entering the blast furnace, which can reduce the impact on the permeability of the upper material column of the blast furnace.

[0067] The lump ore drying and screening system was put into use, and the lump ore ratio of blast furnace increased from 10% to 15.5%, with obvious improvement effect. Especially when using high-moisture Sierra Leone lump, the lump ore drying and screening system is more important. The comparison of different lump ore compositions used in blast furnace is shown in Table 6.

[0068] Table 6 Comparison of different lump ore compositions used in blast furnaces

[0069]

[0070] Table 6 shows that among the lump ores used in blast furnaces, the moisture content of Sierra Leone lump is 11.02%, which is relatively high and contains a lot of powder, affecting the blast furnace powder screening.

[0071] Improvement measures: 1) First ensure that the moisture content of the lump ore is ≤2.0% after drying, and adjust the rolling screen speed simultaneously to screen out the maximum amount of powder in the lump ore; 2) Simultaneously control the flow rate and layer thickness of the lump ore screening under the trough of the blast furnace, clean the screen frequently to keep the lump screen clean, and ensure that the powder entering the furnace is ≤3.0%.

[0072] From the perspective of blast furnace use effect: 1) PB blocks, Peruvian blocks, and South African blocks have relatively good use effects, but the relatively high K20 of South African blocks has a certain impact on the use effect; 2) Brazilian blocks and Sierra Leone blocks have poor use effects, and their proportions need to be reasonably controlled. In the future, it is necessary to optimize the existing block ore resources, stabilize the mainstream blocks, and reasonably match them, which will help the blast furnace to steadily increase the block ore proportion, stabilize the furnace conditions, and reduce costs.

[0073] 2.1.3 Enhanced under-tank screening

[0074] By adjusting the opening of the material flow gate under the trough and the amplitude of the vibrator, the material flows of coke, pellets and sintered ore are controlled to be less than 15kg / s, 20kg / s and 30kg / s respectively; at the same time, the sieve plate is checked at least 4 times per shift and cleaned in time to ensure that the ω (<5mm) of the powder entering the furnace meets the specified requirement of ≤3.0%.

[0075] 2.1.4 Stabilize the air volume entering the furnace

[0076] The blast furnace continues to adhere to the principle of "taking wind as the key" and stabilize the kinetic energy of the blast. In view of the lower grade of high-aluminum materials entering the furnace and the increased viscosity of slag, in order to ensure the air permeability of the blast furnace material column, the blast furnace coal ratio is reduced from (180~185) kg / t to (170±5) kg / t, and the coke load is adjusted from 5.25 to 5.10~5.15; the wind pressure is controlled from 425~430 kPa to (420±5) kPa, and the average air volume entering the furnace reaches 3101m 3 / min, the actual average wind speed is maintained at 258.4m / s, and the change of the air volume entering the furnace and the actual wind speed is shown in Figure 5 The center temperature of the furnace bottom remained stable at 396~400℃, the furnace hearth was active and the furnace condition was stable.

[0077] 2.1.5 Adjustment of furnace front trench repair cycle

[0078] Optimization of trench repair cycle: cancel mid-term pouring, and adjust the trench repair interval from 90 days to 60 days; adjust the trench repair time from 22 hours to 26 hours to improve the quality of trench repair (originally, both overhaul and pouring took longer than the time limit); maintain the interval time of double-field trench repair at more than 10 days to reduce the impact of trench repair on the blast furnace.

[0079] 2.2 Ensure that the furnace is sufficiently hot

[0080] 2.2.1 Improving gas utilization

[0081] 2.2.1.1 Mine batch adjustment

[0082] As the ore batch increases, the thickness of the coke layer in the soft melting zone increases, the coke-ore interface effect weakens, and the furnace condition stabilizes; as the ore batch increases, the center ore-coke ratio increases, the top layer of the soft melting zone decreases, and the resistance loss of the blocky zone increases. The relationship between batch weight and pressure drop is as follows: Figure 6 shown. Figure 7 Point A in the middle has the lowest pressure difference in the whole furnace, and the corresponding batch weight is a more suitable batch weight.

[0083] The blast furnace is loaded by a loading car, and the volume of the loading car is 9.0m 3 According to the traditional CC↓0O↓ (CC represents 2 cars of coke, 00 represents 2 cars of ore) alternating loading, the ore batch of 30.5t / batch is already full (500~600kg of diced coke / batch), which does not meet the production needs of the blast furnace.

[0084] The composite A+B (A: CC↓00↓, B: CC↓00↓00↓) method is adopted for feeding, and the ore batch is raised to: 44.0~45.0t / batch; as the blast furnace coal ratio increases from 150~160kg / t to 170~180kg / t, and reaches a maximum of 180~190kg / t, the thickness of the coke layer in the soft melting zone decreases, and the stability of the blast furnace is weakened. In order to ensure the thickness of the coke layer in the soft melting zone of the blast furnace, the composite feeding method is changed from A+B to A+2B, and the ore batch is adjusted: 45.0t / batch→46.0t / batch→47.0t / batch-48.0t / batch, and the furnace condition stability is enhanced. The subsequent blast furnace is matched with high-aluminum materials, and the smelting strength is controlled in a planned manner. The feeding method continues to maintain the A+2B composite method. The size of the ore batch is selected according to the number of feeding cars 32±1 cars / h to keep the thickness of the coke layer in the soft melting zone stable.

[0085] 2.2.1.2 Fabric Matrix Adjustment

[0086] The blast furnace charging method was changed from A+B to A+2B, the ore batches were increased, the central airflow was slightly weakened, the ore platform width was reduced from 8° to 6°, the coke platform width remained unchanged, the ore-coke angle difference was adjusted from 1.34° to 1.31°, the central airflow was stabilized, and the distribution matrix was adjusted as follows:

[0087] Before adjustment: After adjustment: By rationally selecting ore batches and fine-tuning the burden matrix, the central airflow was improved, furnace stability was enhanced, blast furnace gas utilization increased from 45.0% to 46.5%, with a maximum of 47.5%, and the operating fuel ratio decreased by (5~8) kg / t.

[0088] 2.2.2 Reasonable control of furnace temperature

[0089] According to the principle of low-silicon smelting: 1) High top pressure is conducive to silicon reduction smelting. Due to the restriction of furnace top equipment, the maximum top pressure used is 226~228kPa, which is lower than the top pressure of 250kPa of the same-sized blast furnace, and the pressure difference of 190~200kPa is relatively high; 2) Increasing the R2 basicity of slag is conducive to silicon reduction smelting, R2 basicity = ω(CaO):ω(SiO2); 3) Using high-aluminum material, the slag-iron ratio increases from 351.50kg / t to 370.20kg / t, which is not conducive to silicon reduction smelting.

[0090] In view of the characteristics of high-alumina slag, the furnace temperature is reasonably selected on the premise that the physical heat of molten iron is not lower than 1490℃. Combined with the heat release accompanying slag formation in the slag-making process, the heat release of slag formation per kilogram of CaO (or MgO) is 4.18×270kJ, and the slag R2 basicity is reasonably adjusted.

[0091] Combining the above experience and actual production situation, we have been constantly exploring and adjusting. From October 18 to November 26, the average ω[Si] was 0.41%, the average ω[S] was 0.023%, R2 was 1.21, the physical heat of molten iron was 1507℃, the heat of the furnace was sufficient, the furnace condition was stable, and the physical heat of molten iron and the ω[Si] content change graph is shown in the figure. Figure 7 .

[0092] 2.3 Reasonable adjustment of slag composition

[0093] The ω(Al2O3) of slag with high aluminum material increases, with an average of 16.0% and a maximum of 17.04%. The viscosity of the slag increases, affecting desulfurization. Practical experience shows that there is a suitable R2 basicity at a certain furnace temperature. The reason is that if the R2 basicity is too high, some 2CaO·SiO2 solid particles will appear in the slag, the melting temperature of the slag will increase, the fluidity of the slag will decrease, and the stability will deteriorate, affecting the stability of the furnace condition. Adding a small amount of MgO to the slag can reduce the melting temperature and viscosity of the slag, which is beneficial to desulfurization and stabilizing the furnace condition. Combined with the characteristics of high aluminum slag, the R2 basicity of the slag is reasonably selected, and the R4 basicity of the slag is stabilized by increasing the magnesium-aluminum ratio of the slag. R4 basicity = [ω(CaO)+ω(MgO)]: [(ω(SiO2)+ω(Al2O3)] to meet production needs.

[0094] 1) Sintering began to use high-aluminum powder and simultaneously increased the proportion of dolomite powder. The sintered ore ω(MgO) was adjusted from 2.20% to 2.40%~2.50%, with a maximum of 2.70%~2.80%; the slag magnesium-aluminum ratio gradually increased from an average of 0.57 to 0.63, with a maximum of 0.71. The average slag R2 basicity was 1.21, and the average slag R4 basicity was 1.02. At 1500℃, the slag viscosity was 0.330~0.360Pa·s, meeting the requirement of ≤0.400Pa·s. The average ω[S] was 0.023%, the furnace condition was stable, and the molten iron qualified rate was 100%. The changes of ω(Al2O3) and ω(MgO) in the slag are shown in Figure 8 , slag R2, R4, magnesium-aluminum ratio changes see Fig. 9 .

[0095] 2) According to the production organization and cost reduction requirements, a small amount of self-circulating materials is continuously used in sintering. The ratio of sintering and self-circulating materials is shown in Table 7.

[0096] Table 7 Sintering and self-circulating material ratio (%)

[0097] name Steelmaking ash Environmental gray Gravity Gray Steel sludge Tailings Ratio 0.90 1.20 0.60 1.50 1.20

[0098] Among them, the ω(K2O) of steelmaking ash, gravity ash, steel sludge and tailings are 1.22%, 0.88%, 0.77% and 0.37% respectively; ω(Na20) are 0.72%, 0.63%, 0.55% and 0.45% respectively; after sintering, the alkali metal load of the blast furnace increases: the alkali load of the blast furnace is 2.60~2.80kg / t, which is close to the specified value ≤3.00kg / t. Increasing the MgO content in the slag improves the desulfurization capacity of the slag, thereby reducing the binary basicity of the slag to achieve the purpose of alkali removal. The R2 basicity of the high-aluminum slag is reduced to 1.19~1.22, the magnesium-aluminum ratio is increased to 0.64~0.66, and the slag alkali removal rate is maintained at 105%~110%, meeting the slag alkali removal needs.

[0099] After actual production exploration, the slag ω (Al2O3) increased to 16.00~17.10%, and the slag R2 basicity was controlled at 1.22±0.02. By adjusting the magnesium-aluminum ratio (generally controlled at 0.64±0.02), the slag R4 basicity was ensured to be 1.02±0.02. The slag viscosity was maintained at 0.330~0.360Pa·s at 1500℃, reaching the specified requirement of ≤0.400Pa.s, meeting the needs of slag desulfurization, alkali removal and stable furnace conditions.

[0100] 3 Effects

[0101] From October 18 to November 26, 2023, the blast furnace used high-aluminum materials, and took optimization and adjustment measures from three aspects: physical heat of molten iron, slag composition, and permeability of the material column. The furnace condition was stable, the cost was reduced in an orderly manner, and the expected effect was achieved. 1) After the blast furnace used high-aluminum materials, the furnace grade ω (TFe) dropped by 0.90-1.40%, and the blast furnace output decreased, but the furnace condition remained stable. The daily output of the blast furnace reached 4279t / d, the wind temperature was 1211℃, the oxygen enrichment rate was 4.94%, the coal ratio was 172.4kg / t, and the fuel ratio was 515.6kg / t. The comparison of the changes in the fuel ratio and the coal ratio is shown in Fig.10 .

[0102] 2) The average air volume entering the furnace reaches 3101m 3 / min, the actual average wind speed was maintained at 258.4m / s, the center temperature of the furnace bottom was continuously stable at 396-400℃, the furnace cylinder was active and the furnace condition was stable.

[0103] 3) When 9% Sierra Leone powder is used in sintering, the sintering cost is reduced by RMB 14.51 / t, and the cost of molten iron raw materials is reduced by RMB 17.68 / t; when 3% laterite nickel ore is used in sintering, the sintering cost is reduced by RMB 13.36 / t, and the cost of molten iron raw materials is reduced by RMB 16.30 / t; when 8% Sierra Leone blocks are used in blast furnace, the cost of molten iron raw materials is reduced by RMB 24.8 / t. In total, the cost of molten iron raw materials is reduced by RMB 58.78 / t, the fuel cost is increased by RMB 22.32 / t, and the cost of molten iron is reduced by RMB 36.46 / t.

Claims

1. A method for operating a blast furnace using high-aluminum material, characterized in that: Adjustment measures are taken from three aspects: improving the permeability of the material column, ensuring sufficient heat in the furnace, and reasonably adjusting the slag composition to stabilize the furnace condition. The specific contents include the following: In terms of the air permeability of the material column: maintain the complementarity between raw materials and fuel, give full play to the role of lump ore drying and screening, strengthen the screening under the trough, stabilize the air volume entering the furnace, and adjust the cycle of repairing trenches in front of the furnace to enhance the air permeability of the material column; To ensure sufficient heat in the furnace: improve gas utilization and reasonably control furnace temperature to ensure sufficient heat in the furnace; Reasonable adjustment of slag composition: When using high-aluminum powder in sintering to form high-aluminum material, simultaneously increase the proportion of dolomite powder in the sintered ore to ensure that the R4 basicity is 1.02±0.02, the slag R2 basicity is 1.22±0.02, and the slag viscosity is ≤0.400Pa.s at 1500℃.

2. The method for operating a blast furnace using high-aluminum materials according to claim 1, characterized in that: Maintaining the complementarity between raw materials and fuel refers to optimizing and improving the quality of pulverized coal while stabilizing the mainstream coke structure. The stabilizing the mainstream coke structure refers to adopting a 25% water quenching + 75% dry quenching structure. The optimizing and improving the quality of pulverized coal refers to ensuring that the high calorific value of the injected coal is maintained above 7500kCal / kg, and that the pulverized coal equal to 200 mesh accounts for more than 70% of the total pulverized coal in terms of mass percentage.

3. The method for operating a blast furnace using high-aluminum materials according to claim 1, characterized in that: The said giving full play to the role of lump ore drying and screening means that the moisture content of the lump ore drying is ≤2.00% by mass, the powder entering the furnace is ≤3.0% by mass, the lump ore drying furnace temperature is 650-700°C, and the roller screen is a square hole screen with an aperture of 5mm × 10mm.

4. The method for operating a blast furnace using high-aluminum materials according to claim 1, characterized in that: The enhanced under-trough screening refers to adjusting the opening of the under-trough material flow gate and the amplitude of the vibrator, so that, by mass percentage, the coke is less than 15kg / s, the pellets are less than 20kg / s, the sintered ore is less than 30kg / s, and the powder entering the furnace is ≤3.0%. The powder entering the furnace refers to the particle size of the material entering the furnace being less than 5mm.

5. The method for operating a blast furnace using high-aluminum materials according to claim 1, characterized in that: The stable air volume entering the furnace refers to reducing the blast furnace coal ratio, reducing the coke load, and reducing the wind pressure, so that the average air volume entering the furnace is 3101±110m3 / min and the actual average wind speed is 258.4±10m / s.

6. The method for operating a blast furnace using high-aluminum materials according to claim 1, characterized in that: The improved coal gas utilization refers to improving coal gas utilization from two aspects: ore batch adjustment and charging matrix adjustment. The ore batch adjustment refers to raising the ore batch to: 45.0~48.0t / batch, and the ore batch size is adjusted according to the number of charging cars 32±1 cars / h; the charging matrix adjustment refers to changing the blast furnace charging method from A+B to A+2B, reducing the ore platform width from 8° to 6°, keeping the coke platform width unchanged, and adjusting the ore-coke angle difference from 1.34° to 1.31°, wherein A represents CC↓OO↓, B represents CC↓OO↓OO↓, CC↓ represents 2 cars of coke, OO↓ represents 2 cars of ore, and 2B represents that the B charging sequence is executed twice per cycle.

7. The method for operating a blast furnace using high-aluminum materials according to claim 1, characterized in that: The reasonable control of the furnace temperature means that the physical heat of the molten iron is not lower than 1490°C.

Citation Information

Cited By

  • Method for improving charging ore batch of blast furnace smelting

    CN119932237A