Efficient heat treatment method for large rotating wheel forged piece

Through two normalization and two tempering treatments, combined with quenching treatment, the problem of long heat treatment time of large-scale rotor forgings is solved, and the effect of shortening heat treatment time and improving strength and toughness is achieved.

CN118957215AActive Publication Date: 2024-11-15CHINA FIRST HEAVY IND +1

Patent Information

Application Number
CN202411165916.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

How to further shorten the heat treatment time of forgings while ensuring the finer grain size and better mechanical properties of the 04Cr13Ni5Mo steel large-scale rotor forgings.

Method used

By controlling the heating and cooling rate, the thermal stress and tissue stress are reduced, the grain nucleation is promoted, the grain coarseness is avoided, and the temperature is insulated at an appropriate temperature to fully Intensitization, and finally quenching is performed to improve toughness.

Benefits of technology

The heat treatment time of large-scale rotor forgings is significantly shortened, while obtaining finer grain size, higher strength and higher toughness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957215A_ABST
    Figure CN118957215A_ABST
Patent Text Reader

Abstract

The invention provides an efficient heat treatment method for a large rotating wheel forge piece, and relates to the technical field of heat treatment of steel. According to the heat treatment method, firstly, the forge piece is subjected to normalizing treatment twice, and the temperature rise rate, the normalizing temperature and the heat preservation time in the normalizing treatment process are controlled; therefore, the large rotating wheel forge piece has fine grain size, high strength and high toughness. The tempering temperature of the first tempering treatment is controlled to be 600-640 DEG C, so that the structure in the forge piece is subjected to inverse austenite transformation, the toughness of the forge piece can be effectively improved, the hardness of the forge piece can be reduced, and later rough machining is facilitated. The heat treatment time of the heat treatment method for the large rotating wheel forge piece is short, and the large rotating wheel forge piece obtained through the method has the fine grain size, the high strength and the high toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment of steel, and in particular to an efficient heat treatment method for large runner forgings. Background Art

[0002] 04Cr13Ni5Mo steel is a stainless steel with excellent performance, which is suitable for manufacturing impulse turbine runners. With the continuous innovation of technology, the original small impulse turbine runners cannot meet the use requirements, so it is necessary to develop large impulse turbine runners, and then it is necessary to develop 04Cr13Ni5Mo steel large runner forgings. The diameter of the large impulse turbine runner exceeds 4m and the thickness exceeds 1m, which leads to the large cross-sectional size of the 04Cr13Ni5Mo steel large runner forgings. In the production process, in order to ensure that the 04Cr13Ni5Mo steel large runner forgings have finer grain size and better mechanical properties, it is necessary to heat treat the forgings after forging. Due to the large cross-sectional size of the 04Cr13Ni5Mo steel large runner forgings, the heat treatment time of the forgings is long and the energy consumption is large, which affects the production efficiency. Therefore, how to further shorten the heat treatment time of 04Cr13Ni5Mo steel large runner forgings while ensuring finer grain size and better mechanical properties has become a problem that needs to be solved urgently. Summary of the invention

[0003] The problem solved by the invention is: how to further shorten the heat treatment time of a large-scale runner forging made of 04Cr13Ni5Mo steel while ensuring finer grain size and better mechanical properties of the forging.

[0004] In order to solve the above problems, the present invention provides an efficient heat treatment method for large runner forgings, comprising:

[0005] Step S1, first normalizing treatment: keep the forging blank made of 04Cr13Ni5Mo steel at 150-200°C for 10-20h, heat it to 520-580°C at a rate of 15-25°C / h, then heat it to 1020-1040°C at a rate of 50-60°C / h, keep it for 6-8h, furnace cool it to 940-960°C, keep it for 15-18h, and air cool it to 150-200°C to obtain a first intermediate forging;

[0006] Step S2, second normalizing treatment: the first intermediate forging is kept at 150-200° C. for 10-20 hours, heated to 520-580° C. at a rate of 15-25° C. / h, then heated to 1020-1040° C. at a rate of 50-60° C. / h, kept for 6-8 hours, furnace cooled to 940-960° C., kept for 15-18 hours, and air cooled to 150-200° C. to obtain a second intermediate forging;

[0007] Step S3, performing a first tempering treatment on the second intermediate forging to obtain a third intermediate forging; wherein the tempering temperature of the first tempering treatment is 600-640°C.

[0008] Step S4, quenching the third intermediate forging to obtain a fourth intermediate forging;

[0009] Step S5, performing a second tempering treatment on the fourth intermediate forging to obtain a large runner forging.

[0010] Optionally, in step S3, the first tempering treatment includes:

[0011] The second intermediate forging is kept at 150-200°C for 10-20h, heated to 600-630°C at a first heating rate, kept for 25-40h, cooled to 190-200°C at a first cooling rate, taken out of the furnace and cooled to obtain the third intermediate forging.

[0012] Optionally, in step S3, the first heating rate is 30-40°C / h.

[0013] Optionally, in step S3, the first cooling rate is not higher than 10°C / h.

[0014] Optionally, in step S4, the quenching treatment includes:

[0015] The third intermediate forging is heated to 200-250°C, kept warm for 10-15h, heated to 520-600°C at a rate of 15-25°C / h, then heated to 930-980°C at a rate of 40-60°C / h, kept warm for 15-18h, and air-cooled to 130-200°C to obtain the fourth intermediate forging.

[0016] Optionally, in step S5, the second tempering treatment includes:

[0017] The fourth intermediate forging is kept at 130-200° C. for 10-20 hours, heated to 580-610° C. at a second heating rate, kept for 25-40 hours, cooled to 190-200° C. at a second cooling rate, taken out of the furnace and cooled, to obtain the large runner forging.

[0018] Optionally, in step S5, the second heating rate is 30-40°C / h.

[0019] Optionally, in step S5, the second cooling rate is 5-15°C / h.

[0020] Optionally, in step S1, the diameter of the forging blank is greater than 4 m, and the thickness is greater than 1 m.

[0021] Optionally, in step S1, the components of the forging blank include, by weight percentage: C: 0.01-0.04%, Si: 0-0.6%, Mn: 0.50-1.00%, Cr: 12.0-13.5%, Mo: 0.40-0.80%, Ni: 4.5-6.0%, V: 0-0.07%, Cu: 0-0.50%, W: 0-0.10%, S: 0-0.008%, P: 0-0.020%, and the remainder is Fe and unavoidable impurities; wherein the sum of the mass fractions of V, Cu and W is 0-0.50%.

[0022] Compared with the prior art, the heat treatment method provided in the present invention first performs two normalizing treatments on the forging. During the normalizing treatment, the forging is first kept at 150-200°C for 10-20h to make the forging undergo martensitic transformation, and then the forging is heated to 1020-1040°C. During the heating process, when the temperature of the forging does not reach 520-580°C, the heating rate is slow (15-25°C / h), so that the martensite slowly recovers, which can effectively reduce the thermal stress and structural stress of the forging, and is conducive to improving the strength of the large runner forging; when the temperature of the forging reaches 520-580°C, the heating rate is fast (50- 60℃ / h), which can effectively increase the driving force of material nucleation, promote grain nucleation, and effectively refine the grains, which is conducive to further improving the strength and toughness of large runner forgings; after the forging is heated to 1020-1040℃, the forging is kept at this temperature for a short time (6-8h), which can avoid the coarsening of forging grains due to long-term heat preservation at high temperatures, and greatly reduce the time of normalizing treatment, and then the forging is furnace cooled to 940-960℃, and kept at this temperature for a relatively long time (15-18h), so that the structure in the forging is fully austenitized, thereby further improving the strength and toughness of large runner forgings. By controlling the tempering temperature of the first tempering treatment to 600-640℃, the structure in the forging undergoes reverse austenite transformation, which can effectively improve the toughness of the forging, and is conducive to reducing the hardness of the forging, which is convenient for later rough processing. In summary, the heat treatment method for large runner forgings provided by the present invention has a short heat treatment time, and the large runner forgings obtained by the method have finer grain size, higher strength and higher toughness. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a metallographic structure picture of the large runner forging prepared in Example 1;

[0024] Figure 2 This is a metallographic structure picture of the large runner forging prepared in Example 2;

[0025] Figure 3This is a metallographic structure picture of the large runner forging prepared in Example 3;

[0026] Figure 4 This is a metallographic structure picture of the large runner forging produced in the comparative example. DETAILED DESCRIPTION

[0027] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0028] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0029] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0030] It should be noted that the large-scale runner forging in the present invention refers to a 04Cr13Ni5Mo steel runner forging with a diameter exceeding 4m and a thickness exceeding 1m.

[0031] An embodiment of the present invention provides an efficient heat treatment method for a large runner forging, comprising:

[0032] Step S1, first normalizing treatment: keep the forging blank made of 04Cr13Ni5Mo steel at 150-200°C for 10-20h, heat it to 520-580°C at a rate of 15-25°C / h, then heat it to 1020-1040°C at a rate of 50-60°C / h, keep it for 6-8h, furnace cool it to 940-960°C, keep it for 15-18h, and air cool it to 150-200°C to obtain a first intermediate forging;

[0033] Step S2, second normalizing treatment: the first intermediate forging is kept at 150-200° C. for 10-20 hours, heated to 520-580° C. at a rate of 15-25° C. / h, then heated to 1020-1040° C. at a rate of 50-60° C. / h, kept for 6-8 hours, furnace cooled to 940-960° C., kept for 15-18 hours, and air cooled to 150-200° C. to obtain a second intermediate forging;

[0034] Step S3, performing a first tempering treatment on the second intermediate forging to obtain a third intermediate forging; wherein the tempering temperature of the first tempering treatment is 600-640°C.

[0035] Step S4, quenching the third intermediate forging to obtain a fourth intermediate forging;

[0036] Step S5, performing a second tempering treatment on the fourth intermediate forging to obtain a large runner forging.

[0037] The heat treatment method provided by the embodiment of the present invention first performs two normalizing treatments on the forging. During the normalizing treatment, the forging is first kept at 150-200°C for 10-20h to make the forging undergo martensitic transformation, and then the forging is heated to 1020-1040°C. During the heating process, when the temperature of the forging does not reach 520-580°C, the heating rate is slow (15-25°C / h), so that the martensite slowly recovers, which can effectively reduce the thermal stress and structural stress of the forging, and is conducive to improving the strength of the large runner forging; when the temperature of the forging reaches 520-580°C, the heating rate is fast (50-60°C / h). / h), which can effectively increase the driving force of material nucleation, promote grain nucleation, and thus effectively refine the grains, which is conducive to further improving the strength and toughness of large runner forgings; after the forging is heated to 1020-1040℃, the forging is kept at this temperature for a short time (6-8h), which can avoid the coarsening of forging grains due to long-term heat preservation at a higher temperature, and greatly reduce the time of normalizing treatment, and then the forging is furnace cooled to 940-960℃, and kept at this temperature for a relatively long time (15-18h), so that the structure in the forging is fully austenitized, thereby further improving the strength and toughness of large runner forgings. By controlling the tempering temperature of the first tempering treatment to 600-640℃, the structure in the forging undergoes reverse austenite transformation, which can effectively improve the toughness of the forging, and is conducive to reducing the hardness of the forging, which is convenient for later rough processing. In summary, the heat treatment method for large runner forgings provided in the embodiment of the present invention has a short heat treatment time, and the large runner forgings obtained by the method have finer grain size, higher strength and higher toughness.

[0038] It should be noted that the forging blank in the embodiment of the present invention is forged from 04Cr13Ni5Mo steel ingot, the initial forging temperature during the forging process is 1180°C, and the final forging temperature is 850°C.

[0039] In some embodiments of the present invention, in step S3, the first tempering treatment includes:

[0040] The second intermediate forging is kept at 150-200°C for 10-20h, heated to 600-630°C at a first heating rate, kept for 25-40h, cooled to 190-200°C at a first cooling rate, and cooled out of the furnace to obtain the third intermediate forging; the first heating rate is 30-40°C / h, and the first cooling rate is not higher than 10°C / h.

[0041] In this embodiment, the second intermediate forging is kept at 150-200°C for 10-20h, which can ensure sufficient transformation of the core structure of the forging and reduce the residual austenite content, which is beneficial to further improve the strength of the forging; because the grain size of the forging is finer after the secondary normalizing treatment, it will not bring the risk of cracking when the temperature is raised to 600-630°C at a relatively fast rate (30-40°C / h), and finally the temperature is slowly cooled to reduce the internal stress of the forging.

[0042] In some embodiments of the present invention, in step S4, the quenching treatment includes:

[0043] The third intermediate forging is heated to 200-250°C, kept warm for 10-15h, heated to 520-600°C at a rate of 15-25°C / h, then heated to 930-980°C at a rate of 40-60°C / h, kept warm for 15-18h, and air-cooled to 130-200°C to obtain the fourth intermediate forging.

[0044] In this embodiment, the forging is kept at 200-250°C for 10-20h to make the temperature inside and outside the forging uniform, and then the forging is heated to 930-980°C. During the heating process, when the temperature of the forging does not reach 520-600°C, the heating rate is slow (15-25°C / h), so that the martensite recovers slowly, which can effectively reduce the thermal stress and organizational stress of the forging, and is beneficial to further improve the strength of the large runner forging; when the temperature of the forging reaches 520-600°C, the heating rate is fast (40-60°C / h), which can effectively increase the driving force for material nucleation, promote grain nucleation, and effectively refine the grains, which is beneficial to further improve the strength and toughness of the large runner forging; at 930-980°C, the temperature is kept for 15-18h to heat the core of the forging to above 900°C to ensure sufficient austenitization.

[0045] In some embodiments of the present invention, in step S5, the second tempering treatment includes:

[0046] The fourth intermediate forging is kept at 130-200°C for 10-20h, heated to 580-610°C at a second heating rate, kept for 25-40h, cooled to 190-200°C at a second cooling rate, and cooled out of the furnace to obtain the large runner forging; the second heating rate is 30-40°C / h, and the second cooling rate is 5-15°C / h.

[0047] In this embodiment, the fourth intermediate forging is kept at 130-200°C for 10-20h, which can ensure sufficient transformation of the core structure of the forging and reduce the residual austenite content, which is beneficial to further improve the strength of the forging; keeping it at 580-610°C (the temperature is slightly higher than the Ac1 temperature of the forging) allows a small amount of reverse austenite transformation to occur in the forging, which is beneficial to further improve the toughness of the forging.

[0048] In some embodiments of the present invention, in step S1, the diameter of the forging blank is greater than 4 m, and the thickness is greater than 1 m.

[0049] In some embodiments of the present invention, in step S1, the components of the forging blank include, by weight percentage: C: 0.01-0.04%, Si: 0-0.6%, Mn: 0.50-1.00%, Cr: 12.0-13.5%, Mo: 0.40-0.80%, Ni: 4.5-6.0%, V: 0-0.07%, Cu: 0-0.50%, W: 0-0.10%, S: 0-0.008%, P: 0-0.020%, and the remainder is Fe and unavoidable impurities; wherein the sum of the mass fractions of V, Cu and W is 0-0.50%.

[0050] The present invention is further described below in conjunction with specific embodiments.

[0051] Example 1

[0052] A1. First normalizing treatment: a forging blank made of 04Cr13Ni5Mo steel is kept at 175°C for 15 hours, heated to 550°C at a rate of 20°C / h, then heated to 1030°C at a rate of 55°C / h, kept at this temperature for 7 hours, furnace cooled to 950°C, kept at this temperature for 16.5 hours, and air cooled to 175°C to obtain a first intermediate forging; the diameter of the forging blank is 4800 mm and the height is 1000 mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.

[0053] A2. Second normalizing treatment: keep the first intermediate forging at 175°C for 15 hours, heat it to 550°C at a rate of 20°C / h, then heat it to 1030°C at a rate of 55°C / h, keep it for 7 hours, furnace cool it to 950°C, keep it for 16.5 hours, and air cool it to 175°C to obtain a second intermediate forging.

[0054] A3. First tempering treatment: keep the second intermediate forging at 175°C for 15 hours, heat it to 615°C at a first heating rate, keep it at that temperature for 32 hours, cool it to 195°C at a first cooling rate, take it out of the furnace and cool it to obtain the third intermediate forging; wherein, the first heating rate is 35°C / h, and the first cooling rate is 8°C / h.

[0055] A4, quenching treatment: heat the third intermediate forging to 225°C, keep it at this temperature for 12.5 hours, heat it to 560°C at a rate of 20°C / h, heat it to 955°C at a rate of 50°C / h, keep it at this temperature for 16.5 hours, and air-cool it to 165°C to obtain the fourth intermediate forging.

[0056] A5. Second tempering treatment: keep the fourth intermediate forging at 165°C for 15 hours, heat it to 595°C at a second heating rate, keep it for 32 hours, cool it to 195°C at a second cooling rate, cool it out of the furnace, and obtain the large runner forging; wherein the second heating rate is 35°C / h, and the second cooling rate is 10°C / h.

[0057] Example 2

[0058] A1. First normalizing treatment: a forging blank made of 04Cr13Ni5Mo steel is kept at 150°C for 20 hours, heated to 520°C at a rate of 15°C / h, then heated to 1020°C at a rate of 50°C / h, kept for 8 hours, furnace cooled to 940°C, kept for 18 hours, and air cooled to 150°C to obtain a first intermediate forging; the diameter of the forging blank is 4900 mm and the height is 1120 mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.

[0059] A2. Second normalizing treatment: the first intermediate forging is kept at 150°C for 20 hours, heated to 520°C at a rate of 15°C / h, then heated to 1020°C at a rate of 50°C / h, kept at that temperature for 8 hours, furnace cooled to 940°C, kept at that temperature for 18 hours, and air cooled to 150°C to obtain a second intermediate forging.

[0060] A3. First tempering treatment: keep the second intermediate forging at 150°C for 20 hours, heat it to 600°C at a first heating rate, keep it for 40 hours, cool it to 190°C at a first cooling rate, take it out of the furnace and cool it to obtain the third intermediate forging; wherein, the first heating rate is 30°C / h, and the first cooling rate is 8°C / h.

[0061] A4, quenching treatment: heat the third intermediate forging to 200°C, keep it warm for 15 hours, heat it to 520°C at a rate of 15°C / h, then heat it to 930°C at a rate of 40°C / h, keep it warm for 18 hours, and air-cool it to 130°C to obtain the fourth intermediate forging.

[0062] A5. Second tempering treatment: keep the fourth intermediate forging at 130°C for 20 hours, heat it to 580°C at a second heating rate, keep it for 40 hours, cool it to 190°C at a second cooling rate, take it out of the furnace and cool it to obtain the large runner forging; wherein the second heating rate is 30°C / h, and the second cooling rate is 5°C / h.

[0063] Example 3

[0064] A1. First normalizing treatment: a forging blank made of 04Cr13Ni5Mo steel is kept at 200°C for 10 hours, heated to 580°C at a rate of 25°C / h, then heated to 1040°C at a rate of 60°C / h, kept for 6 hours, furnace cooled to 960°C, kept for 15 hours, and air cooled to 200°C to obtain a first intermediate forging; the diameter of the forging blank is 4000 mm and the height is 1000 mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.

[0065] A2. Second normalizing treatment: keep the first intermediate forging at 200°C for 10 hours, heat it to 580°C at a rate of 25°C / h, then heat it to 1040°C at a rate of 60°C / h, keep it for 6 hours, furnace cool it to 960°C, keep it for 15 hours, and air cool it to 200°C to obtain a second intermediate forging.

[0066] A3. First tempering treatment: keep the second intermediate forging at 200°C for 10-20h, heat it to 630°C at a first heating rate, keep it for 25h, cool it to 200°C at a first cooling rate, cool it out of the furnace, and obtain the third intermediate forging; wherein, the first heating rate is 40°C / h, and the first cooling rate is 8°C / h.

[0067] A4. Quenching treatment: heat the third intermediate forging to 250°C, keep it at this temperature for 10 hours, heat it to 600°C at a rate of 25°C / h, then heat it to 980°C at a rate of 60°C / h, keep it at this temperature for 15 hours, and air-cool it to 200°C to obtain the fourth intermediate forging.

[0068] A5. Second tempering treatment: keep the fourth intermediate forging at 200°C for 10 hours, heat it to 610°C at a second heating rate, keep it for 25 hours, cool it to 200°C at a second cooling rate, take it out of the furnace and cool it to obtain the large runner forging; wherein the second heating rate is 40°C / h, and the second cooling rate is 15°C / h.

[0069] Comparative Example

[0070] A1. First normalizing treatment: keep the forging blank at 650°C for 15h, heat it to 1040°C at a rate of 50°C / h, keep it for 36h, and air-cool it to 145°C to obtain a first intermediate forging; wherein the diameter of the forging blank is 4900mm and the height is 1120mm; the components of the forging blank include, by weight percentage: C: 0.02%, Si: 0.3%, Mn: 0.70%, Cr: 12.5%, Mo: 0.60%, Ni: 5.0%, V: 0.03%, Cu: 0.20%, W: 0.05%, S: 0.004%, P: 0.010%, and the balance is Fe and unavoidable impurities.

[0071] A2. Second normalizing treatment: the first intermediate forging is kept at 145°C for 20 hours, heated to 550°C at a rate of 30°C / h, kept for 15 hours, then heated to 1020°C at a rate of 50°C / h, kept for 36 hours, and air-cooled to 145°C to obtain a second intermediate forging.

[0072] A3. Third normalizing treatment: keep the second intermediate forging at 145°C for 20 hours, heat it to 550°C at a rate of 30°C / h, keep it for 10 hours, then heat it to 980°C at a rate of 50°C / h, keep it for 36 hours, and air-cool it to 145°C to obtain the third intermediate forging.

[0073] A4. First tempering treatment: the third intermediate forging is kept at 145°C for 20 hours, heated to 620°C at a rate of 35°C / h, kept at this temperature for 45 hours, cooled to 200°C at a rate of 10°C / h, and air-cooled to room temperature to obtain a fourth intermediate forging.

[0074] A5. Quenching treatment: the fourth intermediate forging is heated to 1000° C. and kept at this temperature for 19 hours, and then cooled to 145° C. by blasting to obtain a fifth intermediate forging.

[0075] A6. Second tempering treatment: the fifth intermediate forging is heated to 580° C., kept at this temperature for 29 hours, and air-cooled to 145° C. to obtain a sixth intermediate forging.

[0076] A7. Third tempering treatment: The sixth intermediate forging is heated to 600° C. and kept at this temperature for 36 hours. The forging is then taken out of the furnace and cooled to obtain a large runner forging.

[0077] Compared with Examples 1-3, the heat treatment of forgings in the comparative example involves more steps and a longer heat treatment time.

[0078] Experimental example

[0079] The metallographic structures of the large runner forgings prepared in Examples 1-3 and Comparative Examples were characterized. Figure 1-4 ,from Figure 1-4 It can be seen that the grain sizes of the large runner forgings prepared in Examples 1-3 and the comparative example are 3.5, 3.8, 4.5 and 2.8, respectively. It can be seen that the grain sizes of the large runner forgings prepared in Examples 1-3 are finer than those in the comparative example. It should be noted that the higher the grain size grade, the finer the grain size. Figure 1-4 The length represented by the middle scale bar is 100 μm.

[0080] The mechanical properties and flaw detection limit sensitivity of the large runner forgings prepared in Examples 1-3 and the comparative example were characterized, and the results are shown in Table 1. It can be seen from Table 1 that, compared with the comparative example, the yield strength, tensile strength, elongation after fracture and AKv of the large forgings in Examples 1-3 are higher, indicating that the large forgings in Examples 1-3 have higher strength and toughness; it can be seen from Table 1 that, compared with the comparative example, the flaw detection limit sensitivity of the large forgings in Examples 1-3 is higher.

[0081] Table 1

[0082]

[0083]

[0084] It should be noted that the radial and axial directions in Table 1 correspond to the radial and axial properties of the forgings respectively, Rp0.2 represents the yield strength, Rm represents the tensile strength, AKv is used to characterize the impact toughness, representing the energy absorbed by the material when subjected to an impact load, A represents the elongation after fracture, and Z represents the reduction of area.

[0085] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. An efficient heat treatment method for large runner forgings, characterized in that: include: Step S1, first normalizing treatment: keep the forging blank made of 04Cr13Ni5Mo steel at 150-200°C for 10-20h, heat it to 520-580°C at a rate of 15-25°C / h, then heat it to 1020-1040°C at a rate of 50-60°C / h, keep it for 6-8h, furnace cool it to 940-960°C, keep it for 15-18h, and air cool it to 150-200°C to obtain a first intermediate forging; Step S2, second normalizing treatment: the first intermediate forging is kept at 150-200° C. for 10-20 hours, heated to 520-580° C. at a rate of 15-25° C. / h, then heated to 1020-1040° C. at a rate of 50-60° C. / h, kept for 6-8 hours, furnace cooled to 940-960° C., kept for 15-18 hours, and air cooled to 150-200° C. to obtain a second intermediate forging; Step S3, performing a first tempering treatment on the second intermediate forging to obtain a third intermediate forging; wherein the tempering temperature of the first tempering treatment is 600-640°C. Step S4, quenching the third intermediate forging to obtain a fourth intermediate forging; Step S5, performing a second tempering treatment on the fourth intermediate forging to obtain a large runner forging.

2. The high-efficiency heat treatment method for large runner forgings according to claim 1, characterized in that: In step S3, the first tempering treatment includes: The second intermediate forging is kept at 150-200°C for 10-20h, heated to 600-630°C at a first heating rate, kept for 25-40h, cooled to 190-200°C at a first cooling rate, taken out of the furnace and cooled to obtain the third intermediate forging.

3. The high-efficiency heat treatment method for large runner forgings according to claim 2, characterized in that: In the step S3, the first heating rate is 30-40°C / h.

4. The high-efficiency heat treatment method for large runner forgings according to claim 2, characterized in that: In step S3, the first cooling rate is no higher than 10°C / h.

5. The high-efficiency heat treatment method for large runner forgings according to claim 1, characterized in that: In step S4, the quenching treatment includes: The third intermediate forging is heated to 200-250°C, kept warm for 10-15h, heated to 520-600°C at a rate of 15-25°C / h, then heated to 930-980°C at a rate of 40-60°C / h, kept warm for 15-18h, and air-cooled to 130-200°C to obtain the fourth intermediate forging.

6. The high-efficiency heat treatment method for large runner forgings according to claim 1, characterized in that: In step S5, the second tempering treatment includes: The fourth intermediate forging is kept at 130-200° C. for 10-20 hours, heated to 580-610° C. at a second heating rate, kept for 25-40 hours, cooled to 190-200° C. at a second cooling rate, taken out of the furnace and cooled, to obtain the large runner forging.

7. The high-efficiency heat treatment method for large runner forgings according to claim 6, characterized in that: In the step S5, the second heating rate is 30-40°C / h.

8. The high-efficiency heat treatment method for large runner forgings according to claim 6, characterized in that: In the step S5, the second cooling rate is 5-15°C / h.

9. The high-efficiency heat treatment method for large runner forgings according to claim 1, characterized in that: In the step S1, the diameter of the forging blank is greater than 4 m, and the thickness is greater than 1 m.

10. The high-efficiency heat treatment method for large runner forgings according to claim 1, characterized in that: In the step S1, the components of the forging blank include, by weight percentage: C: 0.01-0.04%, Si: 0-0.6%, Mn: 0.50-1.00%, Cr: 12.0-13.5%, Mo: 0.40-0.80%, Ni: 4.5-6.0%, V: 0-0.07%, Cu: 0-0.50%, W: 0-0.10%, S: 0-0.008%, P: 0-0.020%, and the remainder is Fe and unavoidable impurities; wherein the sum of the mass fractions of V, Cu and W is 0-0.50%.

Citation Information

Patent Citations

  • Heat treatment method for martensitic stainless steel forgings for nuclear-power compression elastic rings

    CN103820611A

  • Forging and heat treatment method of 9Cr18MoV steel forging

    CN104099456A

  • Annealing process of 04Cr13Ni5Mo super martensitic stainless steel medium plate for water and electricity

    CN112430714A

  • Heat treatment method for reducing near surface flaw detection sensitivity of rotor forging and rotor forging

    CN117025902A

  • Heat treatment method for oversized 0Cr13Ni5Mo martensitic stainless steel forgings

    CN117165746A

Cited By

  • Post-forging heat treatment method and auxiliary tool for fountain forge piece

    CN119553057A

  • Heat treatment method for large 04cr13ni5mo steel runner forged piece

    WO2026041154A1

  • Post-forging heat treatment method for runner bucket forging, and auxiliary tool

    WO2026118610A1

  • Method for manufacturing large rotor forged part with low energy consumption, and large rotor forged part

    WO2026218519A1