Cold forging steel sub-temperature spheroidizing annealing method

By employing a sub-temperature spheroidizing annealing method for cold heading steel, and using a stepped heating and holding process with multi-stage cooling, the problem of uneven microstructure in the existing cold heading steel spheroidizing annealing technology has been solved. This method achieves reduced hardness and increased plasticity, improves central segregation defects, and meets the subsequent processing requirements of cold heading steel.

CN118957216APending Publication Date: 2024-11-15山西建龙实业有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411040352.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing technologies fail to effectively control heating and cooling rates during sub-temperature spheroidizing annealing of cold heading steel, resulting in the inability to achieve the expected spheroidized structure of 5-6 grade spheroidization (spheroidized body + dotted spheroidized body + ferrite). Consequently, the hardness and plasticity of cold heading steel cannot meet the requirements for subsequent processing.

Method used

A sub-temperature spheroidizing annealing method for cold heading steel is adopted, which involves a stepped heating and holding process and a multi-stage cooling process. The specific steps include heating from room temperature to 700℃ in a heating furnace and holding for 1 hour, then heating to 715℃-725℃ and holding for 4.5-5.5 hours, cooling in the furnace to 700℃ and holding for 0.5 hours, then cooling to 675-685℃ and holding for 2.5-3 hours, continuing to cool to 540℃-555℃ and holding for 0.5 hours, and finally air cooling to room temperature.

Benefits of technology

It achieves a uniform and diffused microstructure after spheroidizing annealing of cold heading steel, reduces hardness, improves plasticity, and improves central segregation defects, and has a short-cycle annealing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957216A_ABST
    Figure CN118957216A_ABST
Patent Text Reader

Abstract

The invention relates to the field of steel annealing. The invention relates to a cold heading steel sub-temperature spheroidizing annealing method, which is characterized in that sub-temperature spheroidizing annealing is adopted after a wire rod for producing a fastener by adopting a cold heading process under a room temperature condition is finished, and the sub-temperature spheroidizing annealing is performed by adopting the following annealing processes in the sub-temperature spheroidizing annealing: in a heating furnace, heating the product to be subjected to sub-temperature spheroidizing annealing from room temperature to 700 DEG C, and preserving heat for 1 hour when the temperature is increased by 100 DEG C every time; continuously heating to 715-725 DEG C, preserving heat for 4.5-5.5 hours, cooling to 700 DEG C along with the furnace, preserving heat for 0.5 hour, cooling to 675-685 DEG C along with the furnace, and preserving heat for 2.5-3 hours; continuously cooling to 540-555 DEG C along with the furnace, and preserving heat for 0.5 hour when the temperature is reduced by 20 DEG C; and taking out from the heating furnace, and air-cooling to room temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of steel annealing. Background Art

[0002] SCM435 wire is a medium carbon alloy steel. It is a wire that can be used to produce fasteners using cold heading technology at room temperature. It is widely used to make high-strength and ultra-high-strength standard parts such as 10.9-12.9 grade screws, bolts, nuts, and self-tapping screws. Because it deforms greatly during processing, it needs to be spheroidized annealed before processing. Therefore, before leaving the factory, the steel mill needs to spheroidize the wire under laboratory conditions to determine whether its organizational properties after spheroidizing annealing can meet the subsequent processing requirements.

[0003] Existing spheroidizing annealing tests mainly use two methods: sub-temperature spheroidizing annealing and two-phase zone spheroidizing annealing. Compared with two-phase zone spheroidizing annealing, sub-temperature spheroidizing annealing has the advantages of fast annealing speed and low energy consumption.

[0004] Sub-temperature spheroidizing annealing is to heat the steel with a matrix structure of ferrite + pearlite to a certain temperature below Ac1 and keep it warm for a long time, using the self-spheroidization of the initial pearlite structure, and then cool it to about 550℃ at a certain cooling rate and take it out for air cooling.

[0005] After searching, the patent documents represented by Chinese patent application numbers CN109487052A, CN109628713B, CN109517949B, and CN103866095A disclose the heating temperature, the insulation temperature, and the test cut-off temperature, but do not specify the residence time of each heating and cooling stage. The heating rate and the cooling rate are partially given, but the box-type resistance furnace commonly used in laboratories does not have the conditions for controlling the heating and cooling rates. The expected test results cannot be obtained by fully following the known test methods. Summary of the invention

[0006] The technical problem to be solved by the present invention is: how to provide a sub-temperature spheroidizing annealing method for cold heading steel, for cold heading steel mainly composed of bainite and pearlite, a 5-6 grade spheroidized structure of spheroidized body + point spheroidized body + ferrite can be obtained after spheroidizing annealing, and the hardness is reduced from 230-240HV before annealing to 154HV-162HV after annealing. The hardness and plasticity requirements meet the subsequent processing requirements of cold heading steel.

[0007] The technical solution adopted by the present invention is: a method for cold heading steel sub-temperature spheroidizing annealing, for the wire rod of the fastener produced by the cold heading process under room temperature, after the product is completed, the sub-temperature spheroidizing annealing is adopted, and the following annealing process is adopted during the sub-temperature spheroidizing annealing: Step 1: Step heating and heat preservation: in a heating furnace, heat the product to be subjected to sub-temperature spheroidizing annealing from room temperature to 700°C, and keep the temperature for 1 hour every time the temperature rises by 100°C; Step 2: Continue heating to 715-725°C and keep warm for 4.5-5.5 hours, then cool with the furnace to 700°C and keep warm for 0.5 hours, then cool with the furnace to 675-685°C and keep warm for 2.5-3 hours; Step 3: Continue cooling with the furnace to 540℃-555℃, and keep warm for 0.5h every time the temperature drops by 20℃; Step 4: Take it out of the heating furnace and air cool it to room temperature.

[0008] The weight percentage of the wire is: C 0.34%-0.36%, Si 0.17i%-0.27%, Mn 0.65%-0.75%, P≤0.025%, S≤0.025%, Cr 0.95%-1.05%, Mo 0.155%-0.215%, Als 0.030%-0.040%, and the balance is Fe and impurities that cannot be separated.

[0009] The wire is SCM435 wire with a diameter of 16mm.

[0010] The beneficial effects of the present invention are as follows: the present invention provides a feasible method for sub-temperature spheroidizing annealing of cold heading steel by clearly stipulating the dwelling temperature and holding time in the heating and cooling stages during the annealing process; the present invention adds a second-stage holding platform for sub-temperature spheroidizing annealing, further ensuring the uniform dispersion distribution of the annealing structure, reducing the hardness of the structure after annealing, and improving the plasticity; at the same time, the method of the present invention also has the characteristics of short annealing cycle and can effectively improve the central segregation defects of raw materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is the original metallographic structure of the SCM435 wire of the present invention; Figure 2 This is the metallographic structure after spheroidizing annealing of Example 1 of the present invention; Figure 3 This is the metallographic structure after spheroidizing annealing in Example 2 of the present invention; Figure 4 This is the metallographic structure after spheroidizing annealing in Example 3 of the present invention; Figure 5 This is the metallographic structure after spheroidizing annealing of Example 4 of the present invention. DETAILED DESCRIPTION

[0012] The national standard used for measuring microhardness in the embodiment of the present invention is "GB / T4340.1-2009 Metallic Materials Vickers Hardness Test Part 1: Test Method".

[0013] The national standard adopted for the spheroidized structure rating in the embodiment of the present invention is "GB∕T 38770-2020 Inspection and Rating of Spheroidized Structure of Low and Medium Carbon Steel".

[0014] The microhardness measurement device used in the embodiment of the present invention is the FALCON500 fully automatic micro Vickers hardness tester produced by Inno, Netherlands.

[0015] The equipment used for metallographic observation of the spheroidized structure in the embodiment of the present invention is a German Zeiss Axio Imager.M2m upright fully automatic metallographic microscope. Example 1

[0016] In this embodiment, the weight percentage of the steel (SCM435 wire) is: C 0.5%, Si 0.26%, Mn 0.71%, P≤0.018%, S≤0.005%, Cr 0.8%, Mo 0.210%, Als 0.033%, and the balance is Fe and impurities that cannot be separated. The wire diameter is 16 mm. The original metallographic structure is as follows Figure 1 shown.

[0017] After the product is produced, the following annealing process is used for annealing during sub-temperature spheroidizing annealing: Step 1: Step heating and heat preservation: in a heating furnace (a box-type resistance furnace for laboratory use), heat the product to be sub-temperature spheroidizing annealing from room temperature to 700°C, and keep the temperature for 1 hour every time the temperature rises by 100°C; Step 2: Continue heating to 715°C and keep warm for 5.5 hours, then cool with the furnace to 700°C and keep warm for 0.5 hours, then cool with the furnace to 685°C and keep warm for 3 hours; Step 3: Continue to cool down to 545°C with the furnace, and keep warm for 0.5h every time the temperature drops by 20°C; Step 4: Take it out of the heating furnace and air cool it to room temperature.

[0018] The annealing process used in the sub-temperature spheroidizing annealing is shown in Table 1.

[0019] Table 1

[0020] Example 1 Test results are as follows Figure 2 As shown in Table 2. The annealed structure is uniformly dispersed, effectively improving the central segregation defects of the raw materials.

[0021] Table 2 Example 2

[0022] The difference from Example 1 is as shown in Table 1. The test results of Example 2 are as shown in Table 1. Figure 3 As shown in Table 2. The annealed structure is uniformly dispersed, effectively improving the central segregation defects of the raw materials. Example 3

[0023] The difference from Example 1 is as shown in Table 1. The test results of Example 3 are as shown in Table 1. Figure 4 As shown in Table 2. The annealed structure is uniformly dispersed, effectively improving the central segregation defects of the raw materials. Example 4

[0024] The difference from Example 1 is as shown in Table 1. The test results of Example 4 are as shown in Table 1. Figure 5 As shown in Table 2. The annealed structure is uniformly dispersed, effectively improving the central segregation defects of the raw materials.

[0025] It can be seen from Examples 1-4 that within the set range, one stage of heat preservation has a greater impact on the rating and hardness of the spheroidized structure. When the temperature of one stage of heat preservation is 718-720°C, the rating of the spheroidized structure is 6, but the hardness is 154-158HVS. When the temperature of one stage of heat preservation is slightly higher or lower, the rating of the spheroidized structure is 5, but the hardness is 161-162HVS.

Claims

1. A sub-temperature spheroidizing annealing method for cold heading steel, characterized in that: For the wire rods produced by cold heading process at room temperature, after the products are completed, they are subjected to sub-temperature spheroidizing annealing. During sub-temperature spheroidizing annealing, the following annealing process is used for annealing: Step 1: Step heating and heat preservation: in a heating furnace, heat the product to be subjected to sub-temperature spheroidizing annealing from room temperature to 700°C, and keep the temperature for 1 hour every time the temperature rises by 100°C; Step 2: Continue heating to 715-725°C and keep warm for 4.5-5.5 hours, then cool with the furnace to 700°C and keep warm for 0.5 hours, then cool with the furnace to 675-685°C and keep warm for 2.5-3 hours; Step 3: Continue to cool down with the furnace to 540℃-555℃, and keep warm for 0.5h every time the temperature drops by 20℃; Step 4: Take it out of the heating furnace and air cool it to room temperature.

2. The method for sub-temperature spheroidizing annealing of cold heading steel according to claim 1, characterized in that: The weight percentage of the wire is: C 0.34%-0.36%, Si 0.17%-0.27%, Mn 0.65%-0.75%, P≤0.025%, S≤0.025%, Cr0.95%-1.05%, Mo 0.155%-0.215%, Als 0.030%-0.040%, and the balance is Fe and impurities that cannot be separated.

3. A sub-temperature spheroidizing annealing method for cold heading steel according to claim 2, characterized in that: The wire is SCM435 wire with a diameter of 16mm.

Citation Information

Patent Citations

  • Spheroidizing annealing method for Cr and Mo steel with sheet type microstructure

    CN103866095A

  • Spheroidizing annealing method for cold heading steel containing B

    CN109487052A

  • A spheroidizing annealing method for shaft steel

    CN109517949B

  • A spheroidizing annealing method for low carbon steel

    CN109628713B