Method for removing copper from lixivium of retired ternary battery
By controlling the pH value in the leaching liquid of the retired ternary lithium battery and using ultrasonic assisted reactions and oxidants to form iron hydroxide precipitation, the problem of poor copper removal effect in the existing technology is solved, and copper ions is effectively removed and ternary front drive is ensured. Effect of body purity.
Patent Information
- Application Number
- CN202311433306.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has poor copper removal effect in the leaching liquid of retired ternary lithium battery and is relatively high in cost, making it difficult to ensure the purity of the ternary precursor.
By measuring the pH of the leaching solution and controlling it in the range of 4.0-6.0, iron powder is added for ultrasonic assisted reaction, followed by adding an oxidant and adjusting the pH to form iron hydroxide precipitation to achieve the removal of copper ions.
It achieves efficient removal of copper ions, ensures the purity of the ternary precursor, reduces process costs, and is simple to operate.
Smart Images

Figure CN118957262A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for removing copper from a leaching solution, and in particular to a method for removing copper from a ternary battery leaching solution. Background Art
[0002] With the rapid development of the global new energy vehicle industry, electric vehicles are gradually becoming the mainstream of the future. Through the analysis of automobiles, the use of new energy vehicles such as electric vehicles can alleviate and improve the current climate problems in the world to a great extent.
[0003] The nickel-cobalt-manganese synthesis of ternary battery precursors is mainly achieved by purchasing battery-grade nickel-cobalt-manganese sulfate from the market, which is then dissolved and prepared before entering the reactor to produce the nickel-cobalt-manganese ternary precursor.
[0004] At present, in China, the wet recycling and impurity removal process of retired ternary lithium batteries is mainly traditional process technology: after a series of pre-treatment processes, the waste batteries are screened and crushed to obtain battery black powder, and the battery black powder is leached with sulfuric acid and reducing agent, and copper, iron, aluminum, calcium and magnesium are removed. After the extraction pre-liquid is obtained, there are roughly two processes: one is to first fully extract the nickel-cobalt-manganese mixed salt solution and then fully strip it, and then add ammonia water and liquid alkali to make the nickel-cobalt-manganese salt solution co-precipitate to generate nickel-cobalt-manganese hydroxide for recovery; the other is to separate nickel sulfate, cobalt sulfate and manganese sulfate by graded extraction, and then evaporate, concentrate and crystallize them separately to make battery-grade nickel sulfate, cobalt sulfate and manganese sulfate crystals for recovery.
[0005] During the recycling process of used ternary lithium batteries, the leachate contains many impurity elements that affect the performance of the ternary precursor. All ternary lithium battery manufacturers have regulations that prohibit magnetic foreign matter such as copper and zinc in the equipment, so they need to be removed in the leachate.
[0006] CN11215987A uses manganese powder to remove copper ions, and manganese and copper ions undergo a substitution reaction to generate Mn 2+ The Cu in the solution 2+ It is displaced and then filtered out, but the cost is high and not economical enough. Summary of the invention
[0007] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for removing copper from the leachate of retired ternary batteries with good copper removal effect.
[0008] The technical solution adopted by the present invention to solve the technical problem is as follows: A method for removing copper from a retired ternary battery leachate comprises the following steps:
[0009] (1) Measure the pH value of the leachate of retired ternary batteries and control it within the range of 4.0-6.0; when the pH value of the leachate of retired ternary batteries is within this range, it can be directly processed; when it is not within this pH range, an acid hydrolysis regulator can be added for control;
[0010] (2) turning on the ultrasonic device, adding iron powder to the retired ternary battery leachate, and performing an ultrasonic-assisted reaction; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0011] (3) adding an oxidant to the copper-removed solution to reduce the Fe 2+ All are oxidized to Fe 3+ ; Ammonia water is added to adjust the pH value to 4.5-7.5, and the solid-liquid separation is performed, and the obtained liquid part is the leaching purification liquid.
[0012] After the iron powder is added in step (2), a reaction occurs in which the iron powder replaces the copper ions.
[0013] After adding ammonia water to adjust the pH value in step (3), iron hydroxide precipitate is formed in the solution.
[0014] By adopting the above technical solution, the copper ion removal rate is high, and no other difficult-to-remove substances are introduced, which can effectively ensure the purity of the ternary precursor.
[0015] Preferably, in the retired ternary battery leachate: Ni 2+ Content 20-70g / L, Co 2+ Content 10-25g / L, Mn 2+ Content 10-25g / L, Li + Content 1-5g / L, Cu 2+ Content 1-3g / L, Fe 3+ Content 0.8-1.8g / L, Ca 2+ Content 0.015-0.035g / L, Mg 2+ Content 0.2-0.5g / L, SO4 2- Content 140-200g / L.
[0016] More preferably, in the retired ternary battery leachate: Ni 2+ Content 50-60g / L, Co 2+ Content 14-20g / L, Mn 2 + Content 14-20g / L, Li + Content 2-4g / L, Cu 2+ Content 1.2-2.5g / L, Fe 3+ Content 0.8-1.4g / L, Ca 2+Content 0.018-0.032g / L, Mg 2+ Content 0.25-0.4g / L, SO4 2- Content 140-170g / L.
[0017] The composition of the retired ternary battery leachate is basically as described above, and the method of the present invention has a good effect when used for the retired ternary battery leachate with the above composition.
[0018] Preferably, the pH value of the retired ternary battery leachate is controlled at 4.0-4.5.
[0019] When the pH value of the retired ternary battery leachate is within this range, it can be directly processed, and when it is not within this pH range, an acid hydrolysis regulator can be used for control. The above technical solution has a good copper removal effect.
[0020] Preferably, in step (2), the frequency of ultrasound is 15 to 50 kHz, and the output power of ultrasound is 800 to 4000 W.
[0021] By adopting the above technical solution, a better copper removal effect is achieved.
[0022] More preferably, in step (2), the frequency of ultrasound is 15 to 30 kHz, and the output power of ultrasound is 1200 to 2500 W.
[0023] By adopting the above technical solution, a better copper removal effect is achieved.
[0024] More preferably, in step (2), the frequency of ultrasound is 15 to 30 kHz, and the output power of ultrasound is 1600 to 2500 W.
[0025] By adopting the above technical solution, a better copper removal effect is achieved.
[0026] Preferably, in step (2), the amount of iron powder used is 1.0-2.0 times the theoretical amount.
[0027] Iron powder is the reactant of the reaction of replacing copper ions, and should be in an equivalent amount or in excess. By adopting the above technical solution, a better copper removal effect is achieved.
[0028] More preferably, in step (2), the amount of iron powder used is 1.3-1.5 times the theoretical amount.
[0029] Iron powder is the reactant of the reaction of replacing copper ions, and should be in equivalent or excessive amount. Unreacted iron powder can be removed during the subsequent solid-liquid separation, so an appropriate excess has the best effect. By adopting the above technical solution, a better copper removal effect is achieved.
[0030] Preferably, in step (2), the ultrasound-assisted reaction time is 1 to 2 hours.
[0031] By adopting the above technical solution, a better copper removal effect is achieved.
[0032] Preferably, in step (2), the temperature of the ultrasound-assisted reaction is 40-60°C.
[0033] By adopting the above technical solution, a better copper removal effect is achieved.
[0034] More preferably, in step (2), the temperature of the ultrasound-assisted reaction is 55-60°C.
[0035] By adopting the above technical solution, a better copper removal effect is achieved.
[0036] Preferably, in step (3), the oxidant is one or more of ozone, hydrogen peroxide, sodium persulfate and sodium percarbonate.
[0037] By adopting the above technical solution, a better oxidation effect is achieved.
[0038] Preferably, in step (3), aqueous ammonia is added to adjust the pH value to 4.5-5.5.
[0039] Adding ammonia water can form iron hydroxide precipitation in the solution, and the iron hydroxide precipitation is generally completely precipitated at pH = 3.7. By adopting the above technical solution, a better iron removal effect is achieved.
[0040] The present invention utilizes copper ions with greater electronegativity in the iron replacement solution, so that the copper ions in the solution can be removed more thoroughly, and the operation is simple and easy to implement. Ultrasonic waves can cause the solution to vibrate violently, causing instantaneous high temperature, which can cause the peeling between the solid reactant and the reaction product, and can increase the contact area between the iron powder and the nickel-cobalt-manganese leachate to accelerate the reaction speed, so that the copper ions in the leachate can be removed more thoroughly. After adding an oxidant to the copper removal solution, ammonia water is used to adjust the pH to remove iron, and the formed iron hydroxide precipitate will not be dissolved by ammonia water, which can effectively ensure the iron removal rate; if necessary, the excess ammonia water can also be evaporated by heating.
[0041] Beneficial effects of the present invention:
[0042] (1) The copper ion removal rate is high and no other difficult-to-remove substances are introduced, which can effectively ensure the purity of the ternary precursor;
[0043] (2) The process is simple and the investment required to improve the copper ion removal rate is small. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a curve chart showing the change of copper ion removal rate over time during the copper removal reaction in Comparative Example 1.
[0045] Figure 2 It is a curve chart showing the change of copper ion removal rate over time during the copper removal reaction of Comparative Example 2 and Example 1.
[0046] Figure 3 It is a curve chart showing the change of copper ion removal rate over time during the copper removal reaction process of Example 2.
[0047] Figure 4 It is a curve chart showing the change of copper ion removal rate over time during the copper removal reaction process in Example 3. DETAILED DESCRIPTION
[0048] The present invention is further described below in conjunction with the embodiments, comparative examples and accompanying drawings. The solutions of the present invention include but are not limited to the specific implementation methods listed below.
[0049] The raw materials used in the examples and comparative examples of the present invention were all obtained through conventional commercial channels.
[0050] In each embodiment and comparative example, when calculating the copper ion concentration, the formula used is as follows, where the unit is mg / L.
[0051]
[0052] Comparative Example 1
[0053] In the leachate of retired ternary battery used in this comparative example: Ni 2+ Content 55.3g / L, Co 2+ Content 19.2g / L, Mn 2+ Content 18.8g / L, Li + Content 3.2g / L, Cu 2+ Content 1.8g / L, Fe 3+ Content 1.2g / L, Ca 2+ Content 0.031g / L, Mg 2+ Content 0.3g / L, SO4 2- The content is 163.2g / L, and the pH value is 4.2.
[0054] The method for removing copper from the leachate of retired ternary batteries in this comparative example does not involve ultrasonic treatment, and includes the following steps:
[0055] (1) The pH value of the leaching solution of retired ternary batteries was measured and the pH value was 4.2, which met the requirements and did not need to be adjusted;
[0056] (2) 500 ml of the retired ternary battery leachate is placed in a 1 L beaker, the beaker is placed in a constant temperature water bath, iron powder is added to the retired ternary battery leachate to react; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0057] The reaction temperature is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0058] The amount of iron powder used is 1.4 times the copper ion content;
[0059] The ultrasound-assisted reaction time is 1 h;
[0060] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0061] In step (2) of this comparative example, an ICP plasma emission spectrometer was used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction, and the copper ion removal rate was calculated. The results are as follows: Figure 1 The results show that the final removal rate of copper ions is 25.3%.
[0062] Comparative Example 2
[0063] In the leachate of retired ternary battery used in this comparative example: Ni 2+ Content 60.3g / L, Co 2+ Content 21.3g / L, Mn 2+ Content 20.4g / L, Li + Content 3.9g / L, Cu 2+ Content 2.2g / L, Fe 3+ Content 1.9g / L, Ca 2+ Content 0.038g / L, Mg 2+ Content 0.6g / L, SO4 2- Content 159.1g / L, pH value 4.2.
[0064] The method for removing copper from the leachate of retired ternary batteries in this comparative example does not involve ultrasonic treatment, but involves stirring, and includes the following steps:
[0065] (1) The pH value of the leaching solution of retired ternary batteries was measured and the pH value was 4.2, which met the requirements and did not need to be adjusted;
[0066] (2) 500 ml of the retired ternary battery leachate was placed in a 1 L beaker, the beaker was placed in a constant temperature water bath, a mechanical stirring device was placed in the solution, the speed was set to 60 r / min, iron powder was added to the retired ternary battery leachate to react; after the reaction was completed, the solid and liquid were separated, and the obtained liquid part was the copper-removed liquid;
[0067] The reaction temperature is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0068] The amount of iron powder used is 1.4 times the copper ion content;
[0069] The ultrasound-assisted reaction time is 1 h;
[0070] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0071] In step (2) of this comparative example, an ICP plasma emission spectrometer was used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction, and the copper ion removal rate was calculated. The results are as follows: Figure 2 The results show that the final removal rate of copper ions is 64.4%.
[0072] Comparative Example 3
[0073] In the leachate of retired ternary battery used in this comparative example: Ni 2+ Content 55.9g / L, Co 2+ Content 19.0g / L, Mn 2+ Content 18.3g / L, Li + Content 3.2g / L, Cu 2+ Content 1.6g / L, Fe 3+ Content 1.5g / L, Ca 2+ Content 0.031g / L, Mg 2+ Content 0.3g / L, SO4 2- The content is 161.9g / L, and the pH value is 4.3.
[0074] The method for removing copper from the leachate of retired ternary batteries in this comparative example comprises the following steps:
[0075] (1) The pH value of the leachate from retired ternary batteries was measured and found to be 4.3, which met the requirements and did not require adjustment;
[0076] (2) 500 ml of the retired ternary battery leachate is placed in a 1L beaker, the beaker is placed in a constant temperature water bath, and an ultrasonic device is placed in the retired ternary battery leachate; the ultrasonic device is turned on, and iron powder is added to the retired ternary battery leachate to perform an ultrasonic-assisted reaction; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0077] The setting frequency of the ultrasonic device is 20kHz and the output power is 300W;
[0078] The temperature of the ultrasound-assisted reaction is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0079] The amount of iron powder used is 1.4 times the copper ion content;
[0080] The ultrasound-assisted reaction time is 1 h;
[0081] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0082] In step (2) of this comparative example, an ICP plasma emission spectrometer was used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction to calculate the copper ion removal rate. The results showed that the final copper ion removal rate was 43.7%.
[0083] Example 1
[0084] In the leaching solution of retired ternary batteries used in this embodiment: Ni 2+ Content 56.3g / L, Co 2+ Content 19.4g / L, Mn 2+ Content 18.9g / L, Li + Content 3.2g / L, Cu 2+ Content 1.9g / L, Fe 3+ Content 1.2g / L, Ca 2+ Content 0.031g / L, Mg 2+ Content 0.3g / L, SO4 2- The content is 163.8g / L, and the pH value is 4.1.
[0085] The method for removing copper from the leachate of retired ternary batteries in this embodiment comprises the following steps:
[0086] (1) The pH value of the leaching solution of retired ternary batteries was measured and the pH value was 4.1, which met the requirements and did not need to be adjusted;
[0087] (2) 500 ml of the retired ternary battery leachate is placed in a 1L beaker, the beaker is placed in a constant temperature water bath, and an ultrasonic device is placed in the retired ternary battery leachate; the ultrasonic device is turned on, and iron powder is added to the retired ternary battery leachate to perform an ultrasonic-assisted reaction; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0088] The setting frequency of the ultrasonic device is 20kHz and the output power is 800W;
[0089] The temperature of the ultrasound-assisted reaction is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0090] The amount of iron powder used is 1.4 times the copper ion content;
[0091] The ultrasound-assisted reaction time is 1 h;
[0092] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0093] In step (2) of this embodiment, an ICP plasma emission spectrometer is used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction, and the copper ion removal rate is calculated. The results are as follows: Figure 2 The results show that the final removal rate of copper ions is 63.1%.
[0094] Example 2
[0095] In the leaching solution of retired ternary batteries used in this embodiment: Ni 2+ Content 55.9g / L, Co 2+ Content 19.0g / L, Mn 2+ Content 18.3g / L, Li + Content 3.2g / L, Cu 2+ Content 1.6g / L, Fe 3+ Content 1.5g / L, Ca 2+ Content 0.031g / L, Mg 2+ Content 0.3g / L, SO4 2- The content is 161.9g / L, and the pH value is 4.3.
[0096] The method for removing copper from the leachate of retired ternary batteries in this embodiment comprises the following steps:
[0097] (1) The pH value of the leachate from retired ternary batteries was measured and found to be 4.3, which met the requirements and did not require adjustment;
[0098] (2) 500 ml of the retired ternary battery leachate is placed in a 1L beaker, the beaker is placed in a constant temperature water bath, and an ultrasonic device is placed in the retired ternary battery leachate; the ultrasonic device is turned on, and iron powder is added to the retired ternary battery leachate to perform an ultrasonic-assisted reaction; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0099] The setting frequency of the ultrasonic device is 20kHz and the output power is 1600W;
[0100] The temperature of the ultrasound-assisted reaction is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0101] The amount of iron powder used is 1.4 times the copper ion content;
[0102] The ultrasound-assisted reaction time is 1 h;
[0103] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0104] In step (2) of this embodiment, an ICP plasma emission spectrometer is used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction, and the copper ion removal rate is calculated. The results are as follows: Figure 3 The results show that the final removal rate of copper ions is 94.1%.
[0105] Example 3
[0106] In the leaching solution of retired ternary batteries used in this embodiment: Ni 2+ Content 56.3g / L, Co 2+ Content 19.4g / L, Mn 2+ Content 18.9g / L, Li + Content 3.2g / L, Cu 2+ Content 1.9g / L, Fe 3+ Content 1.2g / L, Ca 2+ Content 0.031g / L, Mg 2+ Content 0.3g / L, SO4 2- The content is 163.8g / L, and the pH value is 4.1.
[0107] The method for removing copper from the leachate of retired ternary batteries in this embodiment comprises the following steps:
[0108] (1) The pH value of the leaching solution of retired ternary batteries was measured and the pH value was 4.1, which met the requirements and did not need to be adjusted;
[0109] (2) 500 ml of the retired ternary battery leachate is placed in a 1L beaker, the beaker is placed in a constant temperature water bath, and an ultrasonic device is placed in the retired ternary battery leachate; the ultrasonic device is turned on, and iron powder is added to the retired ternary battery leachate to perform an ultrasonic-assisted reaction; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0110] The setting frequency of the ultrasonic device is 20kHz and the output power is 2200W;
[0111] The temperature of the ultrasound-assisted reaction is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0112] The amount of iron powder used is 1.4 times the copper ion content;
[0113] The ultrasound-assisted reaction time is 1 h;
[0114] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0115] In step (2) of this embodiment, an ICP plasma emission spectrometer is used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction, and the copper ion removal rate is calculated. The results are as follows: Figure 4 The results show that the final removal rate of copper ions is 99.9%.
[0116] Example 4
[0117] In the leaching solution of retired ternary batteries used in this embodiment: Ni 2+ Content 56.3g / L, Co 2+ Content 19.4g / L, Mn 2+ Content 18.9g / L, Li + Content 3.2g / L, Cu 2+ Content 1.9g / L, Fe 3+ Content 1.2g / L, Ca 2+ Content 0.031g / L, Mg 2+ Content 0.3g / L, SO4 2- The content is 163.8g / L, and the pH value is 4.1.
[0118] The method for removing copper from the leachate of retired ternary batteries in this embodiment comprises the following steps:
[0119] (1) The pH value of the leaching solution of retired ternary batteries was measured and the pH value was 4.1, which met the requirements and did not need to be adjusted;
[0120] (2) 500 ml of the retired ternary battery leachate is placed in a 1L beaker, the beaker is placed in a constant temperature water bath, and an ultrasonic device is placed in the retired ternary battery leachate; the ultrasonic device is turned on, and iron powder is added to the retired ternary battery leachate to perform an ultrasonic-assisted reaction; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0121] The setting frequency of the ultrasonic device is 20kHz and the output power is 1200W;
[0122] The temperature of the ultrasound-assisted reaction is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0123] The amount of iron powder used is 1.4 times the copper ion content;
[0124] The ultrasound-assisted reaction time is 1 h;
[0125] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0126] In step (2) of this embodiment, an ICP plasma emission spectrometer is used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction to calculate the copper ion removal rate. The results show that the final copper ion removal rate is 70.6%.
[0127] Comparative Example 4
[0128] In the leachate of retired ternary battery used in this comparative example: Ni 2+ Content 60.3g / L, Co 2+ Content 21.3g / L, Mn 2+ Content 20.4g / L, Li + Content 3.9g / L, Cu 2+ Content 2.2g / L, Fe 3+ Content 1.9g / L, Ca 2+ Content 0.038g / L, Mg 2+ Content 0.6g / L, SO4 2- Content 159.1g / L, pH value 4.2.
[0129] Theoretically, the higher the rotation speed, the higher the copper ion removal rate will be. Therefore, in order to further explore the effect of stirring rate on copper ion removal rate, the method for removing copper from retired ternary battery leachate in this comparative example does not perform ultrasonic treatment, but performs stirring. A total of three tests with different rotation speeds (respectively 120r / min, 240r / min and 480r / min) are carried out, including the following steps:
[0130] (1) The pH value of the leaching solution of retired ternary batteries was measured and the pH value was 4.2, which met the requirements and did not need to be adjusted;
[0131] (2) 500 ml of the retired ternary battery leachate is placed in a 1 L beaker, the beaker is placed in a constant temperature water bath, a mechanical stirring device is placed in the solution, the corresponding speed is set, and iron powder is added to the retired ternary battery leachate to react; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid;
[0132] The reaction temperature is 60°C, that is, the temperature of the constant temperature water bath is set to 60°C;
[0133] The amount of iron powder used is 1.4 times the copper ion content;
[0134] The ultrasound-assisted reaction time is 2 hours;
[0135] (3) Add hydrogen peroxide to the copper-removed solution to make the Fe 2+ All are oxidized to Fe 3+ Ammonia water was added to adjust the pH value to 6.5, and the solid-liquid separation was performed. The obtained liquid part was the leaching purification liquid.
[0136] In step (2) of this comparative example, a plasma emission spectrometer ICP was used to measure the copper ion concentration of the sampled solution at different times during the iron powder replacement copper removal reaction, and the copper ion removal rate was calculated. The results showed that:
[0137] In the test with a rotation speed of 120 r / min, the removal rate of copper ions was 78.6% after 1 hour, and the final removal rate of copper ions was 88.4% after 2 hours;
[0138] In the test with a rotation speed of 240 r / min, the removal rate of copper ions was 85.4% after 1 h, and the final removal rate of copper ions was 93.6% after 2 h;
[0139] In the test with a rotation speed of 480r / min, the removal rate of copper ions was 90.7% after 1 hour, and the final removal rate of copper ions was 94.1% after 2 hours.
[0140] Analysis of the results of the embodiments and comparative examples
[0141] The replacement reaction is slow when there is no stirring in the solution, mainly because only the hydrogen generated can provide a little energy to make the solution slightly fluctuate when the replacement reaction occurs in the solution, which is not conducive to the forward reaction, so the final removal rate is not very high (Comparative Example 1); the replacement efficiency of iron powder after introducing the stirring device is significantly increased, because mechanical rotation can increase the contact area between iron powder and copper ions in the solution, and the mass transfer efficiency is improved to improve the reaction speed in the system (Comparative Example 2). The removal rate of copper ions can be increased to a certain extent by increasing the stirring speed, but the copper ion removal rate will gradually stabilize with the increase of the stirring speed, and the improvement of the copper ion removal rate by continuing to increase the rotation speed is not obvious (Comparative Example 4), and it is difficult to provide high-speed stirring in a larger device, and it is difficult to improve the copper ion removal rate by further increasing the rotation speed.
[0142] In contrast, although the improvement of the copper ion removal rate by ultrasound at a lower power is relatively limited (Comparative Example 3), when the ultrasonic power is set to 800W, the copper ion removal efficiency is very close to that at a mechanical stirring speed of 60r / min (Example 1); when the ultrasonic power is in the range of 1200W to 1600W, the copper ion removal rate is significantly improved (Example 2); when the ultrasonic power is increased to 2200W, the copper ion removal rate is very close to 100% (Example 3).
[0143] Ultrasonic waves can induce the cavitation bubbles in the system to burst, and the released energy will cause local high temperature, which will increase the overall temperature of the system. Increasing the power of ultrasonic waves can make the bubbles implode more frequently, and more work will be done on the solution per unit time, which will cause a greater liquid phase thermal effect. This will increase the reaction thermodynamics to a certain extent and strengthen the replacement reaction.
[0144] As described in Example 3, when the ultrasonic power was 2200 W, the removal rate of copper ions reached 95.3% after only 10 minutes of reaction. Figure 2 It can be found that the copper removal rate of the replacement reaction with iron powder is always high in the first 30 minutes of the reaction, and then it slows down significantly; it is speculated that this is because the surface of the iron powder is wrapped by the replaced copper ions, which hinders the further replacement of copper ions in the solution with the iron powder. When the ultrasonic power is large enough, it can not only accelerate the replacement reaction of copper ions in the solution and iron powder, but also strengthen the diffusion of the solution in the product layer produced on the surface of the iron powder, so that when the ultrasonic power exceeds a certain level, the removal rate of copper ions suddenly increases rapidly. A good copper removal effect can be obtained in a shorter time.
Claims
1. A method for removing copper from retired ternary battery leachate, characterized in that: The following steps are involved: (1) Measure the pH value of the leaching solution of retired ternary batteries and control it between 4.0 and 6.0; (2) Turn on the ultrasonic device and add iron powder to the leaching solution of the retired ternary battery to carry out an ultrasonic-assisted reaction; after the reaction is completed, the solid and liquid are separated, and the obtained liquid part is the copper-removed liquid; (3) Add an oxidant to the copper-removed solution to make Fe 2+ All are oxidized to Fe 3+ ; Ammonia water is added to adjust the pH value to 4.5-7.5, and the solid-liquid separation is performed. The obtained liquid part is the leaching purification liquid.
2. The method for removing copper from retired ternary battery leachate according to claim 1, characterized in that: In the retired ternary battery leachate: Ni 2+ Content 20-70g / L, Co 2+ Content 10-25g / L, Mn 2+ Content 10-25g / L, Li + Content 1-5g / L, Cu 2+ Content 1-3g / L, Fe 3+ Content 0.8-1.8g / L, Ca 2+ Content 0.015-0.035g / L, Mg 2+ Content 0.2-0.5g / L, SO4 2- Content 140-200g / L.
3. The method for removing copper from retired ternary battery leachate according to claim 1 or 2, characterized in that: In step (1), the pH value of the retired ternary battery leachate is controlled at 4.0-4.
5.
4. The method for removing copper from retired ternary battery leachate according to any one of claims 1 to 3, characterized in that: In step (2), the frequency of ultrasound is 15-50 kHz, and the output power of ultrasound is 800-4000 W.
5. The method for removing copper from retired ternary battery leachate according to any one of claims 1 to 4, characterized in that: In step (2), the amount of iron powder used is 1.0-2.0 times the theoretical amount.
6. The method for removing copper from retired ternary battery leachate according to any one of claims 1 to 5, characterized in that: In step (2), the ultrasound-assisted reaction time is 1 to 2 hours.
7. The method for removing copper from retired ternary battery leachate according to any one of claims 1 to 6, characterized in that: In step (2), the temperature of the ultrasound-assisted reaction is 40-60°C.
8. The method for removing copper from retired ternary battery leachate according to any one of claims 1 to 7, characterized in that: In step (3), the oxidant is one or more of ozone, hydrogen peroxide, sodium persulfate, and sodium percarbonate.
9. The method for removing copper from retired ternary battery leachate according to any one of claims 1 to 8, characterized in that: In step (3), ammonia water is added to adjust the pH value to 4.5-5.5.
Citation Information
Patent Citations
Method for removing impurities from waste battery leachate
CN111304441A