Method for recycling valuable metal from residual oil hydrogen production filter cake
Through baking and chemical treatment technology, valuable metals Ni, Mo, and V were successfully recovered from residual oil hydrogen-producing filter cakes, solving the problems of high treatment costs and environmental pollution, and achieving efficient utilization of resources and environmental protection effects.
Patent Information
- Application Number
- CN202411030020.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
The residual oil hydrogen-producing filter cake is costly and has the risk of environmental pollution. The prior art has failed to effectively recover the valuable metals Ni, Mo, and V in it, resulting in waste of resources and environmental pollution.
The hydrogen-forming filter cake is produced by roasting residue oil to obtain metal ash residue, and alkali leach and acid leach treatment. Combined with inorganic acid, magnesium salt, anionic resin and ammonia water analysis, pure ammonium molybdate, ammonium metavanadate and nickel sulfate solutions are separated. Realize the recycling and recycling of valuable metals.
It improves resource utilization, reduces production costs, realizes high recovery of valuable metals, reduces, resource utilization and harmless treatment of waste, and reduces wastewater emissions.
Smart Images

Figure CN118957266A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource recycling, and in particular to a method for recycling valuable metals from residual oil hydrogen production filter cake. Background Art
[0002] In recent years, with the continuous growth of oil demand and the shrinking reserves of shallow and easily exploitable light crude oil, the proportion of heavy and inferior crude oil with high sulfur, high metal content and high residual carbon in the global crude oil supply has shown an increasing trend year by year. The combined process of solvent deasphalting, deoiling, asphalt gasification and deasphalted oil hydrogenation and catalytic cracking is an effective means to solve the processing of inferior heavy oil. This process uses C3-C5 as the extraction solvent, extracts deasphalted oil from vacuum residue oil and uses it as the raw material of the catalytic cracking unit after hydrogenation, and the deoiled asphalt is produced by the residue oil hydrogenation unit. Many companies have successfully applied it and achieved good economic benefits. The main product of the residue oil hydrogenation unit is hydrogen, but some solid by-products will also be produced in the hydrogen production process, the most important of which is the carbon black filter cake. In addition to a large amount of water, the filter cake also contains carbon with calorific value, valuable metals Ni, Mo, V, etc. and trace amounts of organic matter. Taking the hydrogen production of Zhejiang Petrochemical's residue oil hydrogenation unit as an example, the filter cake composition is: H 2 O 80%, NiS 1.40%, V 2 O 5 3.4%, FeS0.656%, NaOH 0.23%, CaO 0.27%, MgO 0.08%, Al 2 O 3 0.08%, MoO 3 2.13%, SiO 20.445%, organic matter 11.223% (CH). On the one hand, according to environmental protection regulations, residual oil filter cakes are hazardous wastes and cannot be directly shipped out of the factory, which will increase the processing cost; on the other hand, Ni, Mo, and V are valuable metals, which are in great demand in metallurgy, petrochemicals, and materials. The methods for treating filter cakes generally include: sending them to specific landfills or waste treatment facilities for disposal, recycling heavy metals such as nickel and vanadium in the filter cakes, and converting the filter cakes into heat energy through fluidized bed combustion technology. However, due to the large production scale of residual oil hydrogen production projects and the large output of filter cakes, if the filter cakes are simply incinerated or landfilled, it is easy to cause resource waste and high processing costs; at the same time, due to the special properties of the filter cakes themselves, they are prone to spontaneous combustion during long-term storage, which poses a safety risk and is also prone to environmental pollution. How to treat the residual oil hydrogen production filter cakes at a low cost and with reduced environmental pollution has become a problem that needs to be solved. At present, the waste nickel-molybdenum-vanadium catalysts in domestic refineries are mostly treated by sodium roasting. There is no report on the industrial application of valuable metal recovery for residual oil hydrogen production filter cakes. The present invention provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake to solve the above problems. Therefore, Ni, Mo and V are recovered from the residual oil hydrogen production filter cake to achieve the recycling of metals, which can reduce environmental pollution and generate economic benefits. Summary of the invention
[0003] In order to solve the above problems, the present invention provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake.
[0004] The present invention provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, the method comprising the following steps:
[0005] The residual oil hydrogen production filter cake is roasted to obtain metallic ash;
[0006] alkaline leaching of the metal ash to obtain molybdenum-vanadium leaching solution and alkaline leaching residue;
[0007] Adding inorganic acid and magnesium salt to the molybdenum-vanadium leaching solution to remove impurities, and then adsorbing with a first anion resin and analyzing with ammonia water to obtain a pure ammonium molybdate solution and a molybdenum removal tail liquid;
[0008] Adding ammonium salt to the molybdenum removal tail liquid to precipitate vanadium, and then washing and drying to obtain a pure ammonium metavanadate product and vanadium precipitation tail liquid;
[0009] Adding the alkaline leaching residue into dilute sulfuric acid for acid leaching to obtain a nickel sulfate solution and acid leaching residue;
[0010] Hydrogen peroxide and calcium oxide are added to the nickel sulfate solution for purification to obtain a pure nickel sulfate solution and purified slag.
[0011] Furthermore, the method further comprises:
[0012] The vanadium precipitation tail liquid is adsorbed by a second anion resin and analyzed by sodium hydroxide to obtain a vanadium analysis liquid and a vanadium removal tail liquid; and the vanadium analysis liquid is returned to the vanadium precipitation step;
[0013] The vanadium removal tail liquid is heated and distilled to condense free ammonia to obtain ammonia water, and the ammonia water is returned to the ammonia water analysis step;
[0014] The pure nickel-sulfur solution is evaporated and crystallized to obtain NiSO 4 7H 2 O and crystallization mother liquor; and returning the crystallization mother liquor to the acid leaching process.
[0015] Furthermore, the residual oil hydrogen production filter cake is calcined at a temperature of 500° C. to 650° C. and for a time of 3 to 4 hours.
[0016] Furthermore, the working condition parameters of the alkali leaching include: adding 1.2 times the theoretical amount of alkali and 15% of the oxidant of the material at a solid-liquid ratio of 1:5-8, and leaching for 2 hours at 150°C-180°C and 0.5MPa-0.8MPa.
[0017] Furthermore, the volume fraction of the aqueous ammonia is 10-15%, and the mass percentage concentration of the dilute sulfuric acid is 10-15%.
[0018] Furthermore, when an inorganic acid and a magnesium salt are added to the molybdenum-vanadium leachate for impurity removal, the added mass ratio of the molybdenum-vanadium leachate, the inorganic acid and the magnesium salt is (6-10):(0.5-1):(0.05-0.1).
[0019] Furthermore, the inorganic acid includes at least one of sulfuric acid and hydrochloric acid.
[0020] Furthermore, the magnesium salt includes at least one of magnesium chloride and magnesium sulfate.
[0021] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:
[0022] The embodiment of the present invention provides a method for recycling valuable metals from residual oil hydrogen production filter cakes. While disposing of the waste residual oil hydrogen production filter cakes, the waste residual oil hydrogen production filter cakes are roasted by using the heat generated by combustion, and various valuable metals are recovered by wet treatment, thereby improving the utilization rate of waste resources, overcoming the shortcomings of the prior art, and achieving waste reduction, resource utilization, and harmlessness. Specifically:
[0023] 1) High resource utilization rate: The filter cake of hydrogen production from residue contains 11.223% organic matter (CH) with a relatively high calorific value. The filter cake of hydrogen production from residue oil is roasted to remove organic carbon deposits. The flue gas generated by the roasting can be used as a waste heat utilization device to generate steam for heating heat sources in various production processes. After vanadium removal, the liquid is condensed with cold water using low-temperature distillation to obtain 10-15% dilute ammonia water, which is returned to the molybdenum ion exchange device for analytical liquid.
[0024] 2) Energy saving and emission reduction: The pure nickel sulfate obtained after sulfuric acid leaching and purification is vacuum concentrated and cooled to produce NiSO 4 7H 2 The crystallization mother liquor and washing water are returned to the nickel leaching acid, and the acid is recycled to reduce the amount of wastewater discharged.
[0025] 3) High metal recovery rate. The obtained metal ash is subjected to high temperature and high pressure oxidation leaching in an alkaline system to obtain a high molybdenum and vanadium rate. The molybdenum and vanadium mixed liquid uses a special molybdenum-absorbing resin to selectively adsorb molybdenum, and the recovery rate of molybdenum and vanadium is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 A schematic flow chart of a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake provided in an embodiment of the present invention.
[0029] Figure 2 A schematic flow chart of a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0032] The present invention provides a method for recycling valuable metals from residual oil hydrogen production filter cake, such as Figure 1 As shown, the method comprises the following steps:
[0033] The residual oil hydrogen production filter cake is roasted to obtain metallic ash;
[0034] alkaline leaching of the metal ash to obtain molybdenum-vanadium leaching solution and alkaline leaching residue;
[0035] Adding inorganic acid and magnesium salt to the molybdenum-vanadium leaching solution to remove impurities, and then adsorbing with a first anion resin and analyzing with ammonia water to obtain a pure ammonium molybdate solution and a molybdenum removal tail liquid;
[0036] Adding ammonium salt to the molybdenum removal tail liquid to precipitate vanadium, and then washing and drying to obtain a pure ammonium metavanadate product and vanadium precipitation tail liquid;
[0037] Adding the alkaline leaching residue into dilute sulfuric acid for acid leaching to obtain a nickel sulfate solution and acid leaching residue;
[0038] Hydrogen peroxide and calcium oxide are added to the nickel sulfate solution for purification to obtain a pure nickel sulfate solution and purified slag.
[0039] The embodiment of the present invention provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake. While disposing of the waste residual oil hydrogen production filter cake, the heat generated during the combustion of the waste residual oil hydrogen production filter cake is used for roasting, and various valuable metals are recovered by wet disposal, thereby improving the utilization rate of waste resources, overcoming the shortcomings of the prior art, and achieving the reduction, resource utilization and harmlessness of waste.
[0040] The present invention roasts the filter cake of hydrogen production from residual oil in a roasting furnace to remove organic carbon deposits. The metal ash obtained by roasting in the roasting furnace is leached in an alkaline system to extract molybdenum and vanadium. The molybdenum-vanadium leaching solution is purified and impurized by adding an appropriate amount of inorganic acid and magnesium salt to obtain a purified solution. The purified solution is selectively adsorbed with molybdenum by a macroporous anion resin multi-stage series device, and the molybdenum-rich resin is analyzed with dilute ammonia water to obtain a pure ammonium molybdate solution and a vanadium removal tail liquid. The ammonium molybdate solution is concentrated and crystallized to obtain an ammonium molybdate product. The molybdenum removal tail liquid is added with an ammonium salt reagent to precipitate vanadium to obtain a vanadium precipitation tail liquid and a vanadium precipitate. The precipitate is washed with water and dried to obtain a pure ammonium metavanadate product. The vanadium precipitation tail liquid is selectively adsorbed with a macroporous anion resin device, and the vanadium-rich resin is analyzed with sodium hydroxide to obtain a sodium vanadate solution and a vanadium removal tail liquid. The sodium vanadate solution is returned to the vanadium precipitation process. The vanadium removal tail liquid is subjected to low-temperature distillation to condense free ammonia to obtain dilute ammonia water, and the dilute ammonia water is used for ammonia for molybdenum analysis. The oxidized alkaline leaching residue is added with 10%-15% dilute sulfuric acid to obtain nickel sulfate and acidic leaching residue. The nickel sulfate solution leached from sulfuric acid is purified by adding hydrogen peroxide and calcium oxide to remove molybdenum, vanadium and iron to obtain pure nickel sulfur solution and purified slag. The purified slag is returned to the alkali leaching process to recover molybdenum and vanadium. The purified pure nickel sulfate solution is concentrated by vacuum evaporation, and then cooled and crystallized by water for solid-liquid separation. The solid is filtered and washed to obtain the product NiSO 4 7H 2 O, crystallization mother solution is the black acid return acid leaching nickel process.
[0041] In some specific embodiments, the method for recovering and recycling valuable metals from residual oil hydrogen production filter cake comprises the following steps:
[0042] S1. Oxidative roasting: The residual oil hydrogen production filter cake is roasted in a roaster to remove organic carbon deposits;
[0043] S2. Oxidative alkaline leaching: The metal ash obtained by roasting in the roasting furnace is leached in an alkaline system to extract molybdenum and vanadium;
[0044] S3. Purification and impurity removal: The molybdenum-vanadium leachate is added with an appropriate amount of inorganic acid and magnesium salt to purify and remove impurities to obtain a purified solution;
[0045] S4. Molybdenum extraction: The purified liquid is selectively adsorbed with a macroporous anion resin RCX-5143 multi-stage series device for molybdenum, and the molybdenum-rich resin is decomposed with dilute ammonia to obtain a pure ammonium molybdate solution and a vanadium-free tail liquid. The ammonium molybdate solution is concentrated and crystallized to obtain an ammonium molybdate product;
[0046] S5. Vanadium extraction: adding ammonium salt reagent to the molybdenum tail liquid to precipitate vanadium to obtain vanadium precipitation tail liquid and vanadium precipitate, washing and drying the precipitate with water to obtain pure ammonium metavanadate product; selectively adsorbing vanadium by macroporous anion resin device on the vanadium precipitation tail liquid, decomposing the vanadium-rich resin with sodium hydroxide to obtain sodium vanadate solution and vanadium removal tail liquid, and returning the sodium vanadate solution to the vanadium precipitation step;
[0047] S6 ammonia regeneration: the vanadium removal tail liquid produced by S5 is heated to evaporate the free ammonia condensed to obtain dilute ammonia water, which is used for ammonia for molybdenum analysis in S4;
[0048] S7. Nickel leaching: The alkaline leaching residue produced in S2 is added with 10%-15% dilute sulfuric acid to obtain nickel sulfate and acidic leaching residue;
[0049] S8. Nickel purification: The nickel sulfate solution produced by S6 is purified by adding hydrogen peroxide and calcium oxide to obtain a pure nickel sulfur solution and purified slag, and the purified slag is returned to the alkali leaching process to recover molybdenum and vanadium;
[0050] S9. Nickel crystallization: The pure nickel sulfate solution produced by S7 is concentrated by vacuum evaporation, and then cooled and crystallized by water for solid-liquid separation. The solid is filtered and washed to obtain the product NiSO 4 7H 2 O, crystallization mother solution is the black acid return acid leaching nickel process.
[0051] In some specific embodiments, the S1 residual oil hydrogen production filter cake is calcined at a temperature of 500° C. to 650° C. and for a time of 3 to 4 hours.
[0052] In some specific embodiments, the S2 metal ash is added with 1.2 times of alkali (theoretical dosage) and 15% of the oxidant of the material at a solid-liquid ratio of 1:5-8, and leached at 150°C-180°C and 0.5MPa-0.8MPa high pressure for 2 hours.
[0053] In some specific embodiments, the oxidant in S2 is one of sodium nitrate, sodium hypochlorite, sodium nitrite, hydrogen peroxide liquid oxygen
[0054] In some specific embodiments, in S2, the base is sodium hydroxide, sodium carbonate, and a mixture of sodium hydroxide and sodium carbonate.
[0055] In some specific embodiments, the inorganic acid described in S3 is one of sulfuric acid and hydrochloric acid, and the magnesium salt is one of magnesium chloride and magnesium sulfate.
[0056] In some specific embodiments, the platinum-absorbing resin in S4 is a macroporous ionic resin containing a basic group of an amine complex.
[0057] In some specific embodiments, the ammonium salt described in S5 is one of ammonium chloride, ammonium sulfate, ammonium carbonate, and ammonium nitrate.
[0058] In some specific embodiments, the vanadium absorbing resin described in S5 is a macroporous anionic resin containing a basic group of an amine complex.
[0059] In some specific embodiments, the vanadium removal tail liquid in S6 is subjected to low temperature fine distillation to obtain 12-15% dilute ammonia water, which is used as ammonia for molybdenum analysis in S4, and the liquid NH after ammonium distillation is NH 4+ ≤10ppm.
[0060] In some specific embodiments, the S2 alkaline leaching residue described in S7 is leached with 10%-15% dilute sulfuric acid at 80°C-85°C at a solid-to-liquid ratio of 1:10.
[0061] In some specific embodiments, the hydrogen peroxide and calcium oxide described in S8.
[0062] In some specific embodiments, the water-cooled crystallization temperature in S9 is controlled at about 40°C to 45°C, and the product NiSO is obtained after washing and filtration. 4 7H 2 O, crystallization mother liquor and washing water return S7 nickel leaching acid.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] The present invention provides a method for recycling valuable metals from residual oil hydrogen production filter cake, which has a simple process flow, easy to control reaction conditions, low production cost, high molybdenum and vanadium leaching rate, recovery rate of more than 99%, and high resource utilization. Compared with the prior art, the advantages of the present invention are:
[0065] (1) The method provided by the present invention has a high one-time leaching rate of molybdenum and vanadium in the alkaline system in step S2, with molybdenum reaching 99% and vanadium reaching 98%, thereby reducing energy consumption and production costs.
[0066] (2) The method provided by the present invention dissolves the residual molybdenum and vanadium in the alkaline leaching residue with sulfuric acid in step S7, and then recovers the small amount of molybdenum and vanadium generated in the nickel sulfate solution with hydrogen peroxide and calcium oxide in step S8, and the recovery rate of valuable metals is high.
[0067] (3) The method provided by the present invention is to adsorb molybdenum by using a multi-stage series device in step S4, and adsorb the basic groups of the molybdenum resin containing amine complexes, which are easily ionized in water to produce OH - ions, MoO contained in water 4 2- Ions are ionized by ion exchange resins - Ion exchange was performed to make the anion MoO 4 2- is transferred to the resin, and the O H- When the resin is exchanged with water, the exchange capacity can reach 30-50g / l. After the resin is saturated with adsorption, it is analyzed with dilute ammonia solution. - MoO adsorbed on the resin functional groups 4 2- Ion exchange is performed to restore the exchange capacity of the resin. No transformation or sulfidation is required during the exchange and regeneration process, which reduces energy consumption and production costs.
[0068] (4) The method provided by the present invention uses a vanadium absorbing resin in step S5, which is a macroporous weakly alkaline anion exchange resin with polyamine functional groups and very durable. After regeneration with sodium hydroxide, it has an excellent regeneration effect, and has extremely low requirements for flushing. It can resist high organic pollution and selectively remove vanadium in depth. The exchange and regeneration process does not require transformation to reduce energy consumption and reduce production costs.
[0069] (5) The method provided by the present invention is to perform low-temperature ammonium evaporation on the liquid after molybdenum removal in step S6 to obtain 15% dilute ammonia water for recycling.
[0070] (6) The method provided by the present invention is to produce NiSO by vacuum concentrating and cooling the purified nickel sulfate solution in step S8. 4 7H 2 O, crystallization mother liquor and washing water are returned to S6 nickel leaching acid, the acid is recycled and the wastewater discharge is reduced.
[0071] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0072] Example 1
[0073] This example provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, such as Figure 2 As shown, the following process is included:
[0074] Step (1): 20 kg of residual oil hydrogen filter cake is placed in a roasting furnace for roasting, heated to 550°C for 4 hours, and then cooled to obtain metal ash. Metal ash sampling and analysis data: NiO8.99%, V 2 O 5 36.75%, Fe 2 O 3 4%, Na 2 O1.64%, CaO3%, Al 2 O 3 0.405%、SiO 2 0.89%, MoO 3 23.6%, Mg and other oxides 3%, residual carbon 0.025%;
[0075] Step (2): 1 kg of metal ash was added to an autoclave at a solid-liquid ratio of 1:6, and then 100 g of sodium nitrite and 500 g of caustic soda flakes were added, the temperature was raised to 160° C., and the reaction was carried out under a pressure of 5 kg for 2 hours. After the reaction was completed, the temperature was lowered and the pressure was released, and the feed liquid was filtered to obtain 6200 ml of solution and 132 g of alkali leached residue, which were tested and calculated as shown in Table 1;
[0076] Table 1
[0077]
[0078] Step (3): Purification: Add appropriate amount of hydrochloric acid and magnesium chloride to obtain 6200 ml of filtrate at 85° C. for 2 hours and filter to obtain 6400 ml of purified liquid and filter residue;
[0079] Step (4): Molybdenum-vanadium separation: 6400 ml of purified liquid is firstly selectively adsorbed by a macroporous anion resin multi-stage series device, and the molybdenum-rich resin is resolved by 12% dilute ammonia water to obtain a pure ammonium molybdate solution and a molybdenum-free tail liquid. The ammonium molybdate solution is concentrated and crystallized to obtain an ammonium molybdate product, which is shown in Table 2 after detection and calculation;
[0080] Table 2
[0081]
[0082] Step (5): vanadium precipitation: add ammonium chloride to the obtained 6400 ml molybdenum removal tail liquid at 65° C. and precipitate vanadium for 2 hours, filter to obtain 6600 ml vanadium precipitation tail liquid and ammonium metavanadate, and then pass the vanadium precipitation tail liquid through a vanadium anion resin device to adsorb vanadium, and use 10% sodium hydroxide to dissolve the vanadium-rich resin to obtain a pure sodium vanadate solution and a vanadium removal tail liquid, which are tested and calculated as shown in Table 3;
[0083] Table 3
[0084]
[0085] Step (6): nickel leaching: the alkaline leaching residue produced in step (2) was added with 15% dilute sulfuric acid at a solid-liquid ratio of 1:10 and leached at 85°C for 2 hours. After the reaction was completed, 1000 ml of nickel sulfate solution and 30 g of acidic leaching residue were obtained by filtration and washing, and the results were tested and calculated as shown in Table 4;
[0086] Table 4
[0087]
[0088] Step (7): nickel purification: 1000 ml of nickel sulfate solution was added with hydrogen peroxide and calcium oxide to react at 80° C. for 2 hours. After the reaction was completed, 1100 ml of pure nickel sulfate solution and 40 g of purified slag were obtained by filtration and washing. The results of the test and calculation are shown in Table 5.
[0089] Table 5
[0090]
[0091] Step (8): Nickel crystallization: 1100 ml of pure sulfur-nickel solution was concentrated by vacuum evaporator, and then cooled and crystallized by water for solid-liquid separation. The solid was filtered and washed to obtain the product NiSO 4 7H 2 O and 500 ml of crystallization mother liquor, after testing and calculation, as shown in Table 6;
[0092] Table 6
[0093]
[0094]
[0095] Step (9): The obtained vanadium-free liquid is evaporated at low temperature, and the evaporated gas is condensed with cold water to obtain 12% dilute ammonia water. The ammonium evaporated liquid NH 4 + ≤10ppm.
[0096] Example 2
[0097] This example provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, which is different from Example 1 in that: step (2) adopts high-pressure and high-temperature leaching, specifically: 1 kg of metal ash is added to an autoclave at a solid-liquid ratio of 1:6, and then 500 g of flake caustic soda is added, the temperature is raised to 160°C, and the reaction is carried out under a pressure of 5 kg for 2 hours. After the reaction is completed, the temperature is lowered and the pressure is released, and the feed liquid is filtered to obtain 6200 ml of solution and 300 g of alkali leached residue. After detection and calculation, the results are shown in Table 7.
[0098] Table 7
[0099]
[0100] Example 3
[0101] This example provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, which differs from Example 1 in that: step (2) adopts normal pressure leaching, specifically: 100g of metal ash is added to a 2L kettle at a solid-liquid ratio of 1:8, and then 50g of flake caustic soda is added, the temperature is raised to 95°C, and the reaction is carried out under normal pressure for 3 hours. After the reaction is completed, the temperature is lowered and filtered, and the feed liquid is filtered to obtain 1L of solution and 60g of alkali leaching residue, which is tested and calculated as shown in Table 8.
[0102] Table 8
[0103]
[0104] Example 4
[0105] This example provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, which is different from Example 3 in that: 100g of metal ash is added to a normal pressure reactor at a solid-liquid ratio of 1:8, and then 50g of flake caustic soda and 15g of sodium hypochlorite are added, the temperature is raised to 95°C, and the reaction is carried out under normal pressure for 3 hours. After the reaction is completed, the reaction is filtered and washed to obtain 1L of feed liquid and 40g of alkaline leaching residue; after detection and calculation, it is shown in Table 9.
[0106] Table 9
[0107]
[0108] Example 5
[0109] This example provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, which differs from Example 1 in that: in step (1), a sodium roasting method is adopted, specifically: 100g of metal ash is mixed with carbonic acid at a rate of 40% of the material amount, and then put into a roasting furnace for sodium roasting, the temperature is raised to 650°C, roasted for 4 hours, and after cooling, the sodium roasting product cannot be separated from the roasting boat.
[0110] Example 6
[0111] This example provides a method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, which differs from Example 1 in that: in step (2), a roasting deoiling-sodium roasting method is adopted, specifically: 100g of metal ash is mixed with carbonic acid at 40% of the material amount, and then put into a roasting furnace for sodium roasting, the temperature is raised to 650°C, and roasted for 4 hours. After cooling, the sodium roasting product cannot be separated from the roasting boat.
[0112] In summary, the present invention provides a method for recycling valuable metals from residual oil hydrogen production filter cakes. The filter cakes are roasted to remove organic carbon deposits. The filter cakes contain 11.223% (C, H) of organic matter and have a relatively high calorific value. The flue gas generated by the roasting can be used as a heating source for production by using a waste heat utilization device to generate steam. The obtained metal ash is subjected to high-temperature and high-pressure oxidation in an alkaline system to extract molybdenum and vanadium with a high rate. The molybdenum-vanadium mixed liquid uses a special molybdenum-absorbing resin to selectively adsorb molybdenum, and the recovery rate of molybdenum and vanadium is high. The ammonium molybdate solution is analyzed with dilute ammonia water, and the ammonium molybdate solution is concentrated and crystallized to obtain an ammonium molybdate product. The sodium vanadate solution after molybdenum separation is precipitated by ammonium salt to obtain ammonium metavanadate that meets the standards for chemical reagents, catalysts, and mordant raw materials in the petroleum and chemical industries. The nickel-containing solution purified by sulfuric acid leaching is vacuum concentrated and cooled and crystallized to produce NiSO 4 7H 2 The product quality of Ni37.8% meets the catalyst standard and is used to prepare raw materials for other nickel salt industries. The crystallization mother liquor and washing water are returned to the nickel leaching acid, and the acid is recycled to reduce wastewater discharge.
[0113] Vanadium removal The liquid after ammonium evaporation is evaporated at low temperature, and the evaporated gas is condensed with cold water to obtain 10-15% dilute ammonia water, which is returned to the molybdenum ion exchange device for analytical solution, basically achieving rational utilization of resources. 4 + ≤10ppm.
[0114] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0115] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.
Claims
1. A method for recovering and recycling valuable metals from residual oil hydrogen production filter cake, characterized in that: The method comprises the following steps: The residual oil hydrogen production filter cake is roasted to obtain metallic ash; alkaline leaching of the metal ash to obtain molybdenum-vanadium leaching solution and alkaline leaching residue; Adding inorganic acid and magnesium salt to the molybdenum-vanadium leaching solution to remove impurities, and then adsorbing with a first anion resin and analyzing with ammonia water to obtain a pure ammonium molybdate solution and a molybdenum removal tail liquid; Adding ammonium salt to the molybdenum removal tail liquid to precipitate vanadium, and then washing and drying to obtain a pure ammonium metavanadate product and vanadium precipitation tail liquid; Adding the alkaline leaching residue into dilute sulfuric acid for acid leaching to obtain a nickel sulfate solution and acid leaching residue; Hydrogen peroxide and calcium oxide are added to the nickel sulfate solution for purification to obtain a pure nickel sulfate solution and purified slag.
2. The method for recovering and recycling valuable metals from residual oil hydrogen production filter cake according to claim 1, characterized in that: The method further comprises: The vanadium precipitation tail liquid is adsorbed by a second anion resin and analyzed by sodium hydroxide to obtain a vanadium analysis liquid and a vanadium removal tail liquid; and the vanadium analysis liquid is returned to the vanadium precipitation step; The vanadium removal tail liquid is heated and distilled to condense free ammonia to obtain ammonia water, and the ammonia water is returned to the ammonia water analysis step; The pure nickel-sulfur solution is evaporated and crystallized to obtain NiSO4·7H2O and a crystallization mother liquor; and the crystallization mother liquor is returned to the acid leaching process.
3. The method for recovering and recycling valuable metals from residual oil hydrogen production filter cake according to claim 1, characterized in that: The calcination temperature of the residual oil hydrogen production filter cake is 500℃~650℃, and the calcination time is 3~4h.
4. The method for recovering and recycling valuable metals from residual oil hydrogen production filter cake according to claim 1, characterized in that: The working condition parameters of the alkali leaching include: adding 1.2 times the theoretical amount of alkali and 15% of the oxidant of the material at a solid-liquid ratio of 1:5-8, and leaching for 2 hours at 150°C-180°C and 0.5MPa-0.8MPa.
5. The method for recovering and recycling valuable metals from residual oil hydrogen production filter cake according to claim 1, characterized in that: The volume fraction of the ammonia water is 10-15%, and the mass percentage concentration of the dilute sulfuric acid is 10-15%.
6. The method for recovering and recycling valuable metals from residual oil hydrogen production filter cake according to claim 1, characterized in that: When inorganic acid and magnesium salt are added to the molybdenum-vanadium leaching solution for impurity removal, the added mass ratio of the molybdenum-vanadium leaching solution, the inorganic acid and the magnesium salt is (6-10):(0.5-1):(0.05-0.1).
7. The method for recovering and recycling valuable metals from residual oil hydrogen production filter cake according to claim 1, characterized in that: The inorganic acid includes at least one of sulfuric acid and hydrochloric acid.
8. The method for recovering and recycling valuable metals from residual oil hydrogen production filter cake according to claim 1, characterized in that: The magnesium salt includes at least one of magnesium chloride and magnesium sulfate.