Method for reducing energy consumption of rotary hearth furnace for treating zinc-containing dust

By adding calcium oxide and lignin reducing agent during the treatment of zinc-containing dust in a rotary hearth furnace, efficient energy utilization and resource utilization of zinc dust are achieved, solving the problems of high energy consumption and large flue gas volume in rotary hearth furnaces, and improving the calcium ferrite formation rate and zinc removal rate.

CN118957292AActive Publication Date: 2024-11-15ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411041703.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Rotary hearth furnaces consume a lot of energy and produce a large volume of flue gas when processing zinc-containing dust, resulting in low energy efficiency. Existing technologies are unable to effectively reduce energy consumption and flue gas volume.

Method used

By adding calcium oxide and a small amount of reducing agent lignin, and then calcining at high temperature, zinc dust is converted into calcium ferrite and elemental zinc, reducing the heat consumption and flue gas volume of the reduction reaction. At the same time, lignin is used as a reducing agent to reduce the consumption of non-renewable energy.

Benefits of technology

It significantly reduced the energy consumption and flue gas volume of the rotary hearth furnace for treating zinc-containing dust, improved the calcium ferrite formation rate and zinc removal rate, saved 42.35% energy and reduced the processing cost by 29.34%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957292A_ABST
    Figure CN118957292A_ABST
Patent Text Reader

Abstract

The invention provides a method for reducing energy consumption of a rotary hearth furnace for treating zinc-containing dust, which comprises the following steps: adding sufficient calcium oxide and a small amount of reducing agent, and converting the zinc-containing dust into calcium ferrite and elemental zinc through high-temperature roasting. The high-calcium low-carbon condition promotes iron oxide to convert calcium ferrite, on one hand, heat absorbed by the reduction reaction of the iron oxide is reduced, on the other hand, the flue gas amount generated by the reduction reaction and heat taken away by the flue gas are reduced, and the problems that the energy consumption is high and the flue gas amount is large when the rotary hearth furnace is used for treating zinc-containing dust are solved to a certain extent; meanwhile, lignin is added as a reducing agent, so that zinc oxide can be effectively reduced, consumption of non-renewable energy sources (pulverized coal) is reduced, and environmental protection and social benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of treating zinc-containing dust in a rotary hearth furnace, and particularly relates to a method for reducing energy consumption of treating zinc-containing dust in a rotary hearth furnace. Background Art

[0002] The steel industry is a resource- and energy-intensive industry. A large amount of industrial dust, such as zinc-containing dust, is generated during the steel production process. Zinc-containing dust contains high levels of elements such as iron and carbon, and has a very high recycling and utilization value for steel companies. At the same time, zinc-containing dust also contains zinc, potassium, sodium and other elements, which have a significant adverse effect on steel production, especially blast furnace production. Therefore, zinc-containing dust in steel plants generally cannot be directly recycled in steel plants, which causes a large amount of zinc-containing dust to accumulate and seriously pollute the environment. Therefore, the resource utilization of zinc-containing dust has become a serious problem facing steel plants.

[0003] The rotary hearth furnace is efficient and large-scale in treating zinc-containing dust, and is the main way to utilize zinc-containing dust in steel plants. The rotary hearth furnace process mainly uses carbon-containing pellets to self-reduced under high temperature conditions to remove zinc and obtain metallized pellets, wherein the main source of the reducing agent carbon powder is the carbon in the dust removal ash or the added coke powder and coal powder. For example, the patent with the publication number of CN101386913A published on March 18, 2009 discloses a method for recovering zinc oxide from zinc-containing dust in a rotary hearth furnace. The disclosed technical solution is: the zinc-containing dust is mixed with coal and additives, and then briquetting and drying is carried out and then sent to the rotary hearth furnace for direct reduction. The zinc in the dust is recovered from the exhaust gas, and the material blocks after zinc removal are directly reduced by the rotary hearth furnace and then cooled or briquetting before use. This technology has a wide adaptability to zinc-containing raw materials, can maximize the rational use of resources, has low requirements on the calorific value of the fuel, high flue gas temperature, and high zinc removal rate, and the treated dust becomes direct reduced iron. However, the rotary hearth furnace has a high reaction temperature, and the large amount of flue gas takes away a lot of heat, resulting in low energy efficiency. Therefore, the rotary hearth furnace process still needs to be improved. How to improve the energy efficiency of the rotary hearth furnace and reduce energy consumption is an urgent problem to be solved in the rotary hearth furnace process.

[0004] In addition to adding coal powder and coke powder, calcium oxide is added to the zinc-containing dust to reduce the melting point of the slag when other processes are used to treat zinc-containing dust. For example, the patent with publication number CN 111647704 A published on September 11, 2020 discloses a zinc recovery method based on a HIsmelt smelting reduction furnace. By adding zinc-containing dust during the ironmaking process of the HIsmelt smelting reduction furnace, and collecting the dust in the escaping furnace gas for cyclic injection, the zinc content in the atmosphere of the smelting reduction furnace is effectively increased, so that the collected zinc-rich dust has a higher zinc content; and by wet processing the zinc-rich dust, a zinc oxide product with higher purity is obtained, thereby achieving effective enrichment and recovery of zinc. The reduction reaction still mainly occurs during the treatment process, and the purpose of adding calcium oxide is to lower the melting point. Summary of the invention

[0005] The purpose of the present invention is to provide a method for reducing the energy consumption of zinc-containing dust in a rotary hearth furnace, by adding sufficient calcium oxide (referred to as high calcium) and a small amount of reducing agent (referred to as low carbon), and converting zinc-containing dust into calcium ferrite and elemental zinc through high-temperature roasting. The high calcium and low carbon conditions promote the conversion of iron oxide into calcium ferrite, which reduces the heat absorbed by the reduction reaction of iron oxide on the one hand, and reduces the amount of flue gas generated by the reduction reaction and the heat carried away by the flue gas on the other hand, and reduces the problems of high energy consumption and large amount of flue gas in the treatment of zinc-containing dust in the rotary hearth furnace to a certain extent; at the same time, adding lignin as a reducing agent can not only effectively reduce zinc oxide, but also reduce the consumption of non-renewable energy (coal powder), which has environmental protection and social benefits.

[0006] The specific technical solutions of the present invention are as follows:

[0007] The present invention provides a method for reducing energy consumption of treating zinc-containing dust in a rotary hearth furnace, comprising the following steps:

[0008] 1) Mix the reducing agent, zinc-containing dust and calcium oxide, and send the resulting mixture into a rotary hearth furnace, heat and keep it warm, and then cool it down along with the furnace;

[0009] 2) Calcium ferrite pellets are discharged from the rotary hearth furnace, and the flue gas discharged from the rotary hearth furnace is heat exchanged to remove zinc to obtain zinc powder containing zinc oxide.

[0010] The reducing agent accounts for 2-4% by weight in the mixture, preferably 2-3% by weight;

[0011] The reducing agent comprises the following raw materials in percentage by weight: 60% to 70% lignin, 20% to 25% anthracite powder, and the remainder of a high-efficiency catalyst;

[0012] The particle size of the lignin is 200-18 mesh;

[0013] The high-efficiency catalyst comprises the following raw materials in 100% by mass: 10-20% cobalt oxide, 15-25% cerium oxide, 3-6% potassium chloride, and 49-72% nickel oxide; the total is 100%.

[0014] The zinc-containing dust accounts for 70-73% by mass in the mixture, preferably 71%;

[0015] The zinc-containing dust is selected from blast furnace, converter or electric furnace dust, with a dust particle size of <0.1 mm and a moisture content of <6%;

[0016] The calcium oxide accounts for 23-28% by mass in the mixture, preferably 26-27% by mass;

[0017] The particle size of the calcium oxide is 200-18 mesh;

[0018] The moisture content of the reducing agent, zinc-containing dust and calcium oxide is reduced to below 2% by drying, and then mixed;

[0019] Preferably, the reducing agent, zinc-containing dust and calcium oxide are mixed, sent to a high-pressure briquetting machine and pressed into green balls with a diameter of 10 to 40 mm, and then sent to a rotary hearth furnace;

[0020] The rotary hearth furnace is fueled by coke oven gas and protected by nitrogen atmosphere;

[0021] In step 1), the heating and heat preservation is specifically: heating to 1250° C. in a rotary hearth furnace, keeping the temperature for 15-25 minutes, and then cooling down with the furnace. Preferably, the temperature is 1250° C. and the heat preservation time is 25 minutes.

[0022] In step 1), during the insulation period, nitrogen was first passed for 15 minutes and then switched to air for 10 minutes;

[0023] Alternatively, during the insulation period, nitrogen was passed for 15 minutes and then switched to oxygen for 10 minutes;

[0024] Alternatively, nitrogen is always introduced during the insulation period;

[0025] In step 2), after the insulation is completed, the calcium ferrite pellets are discharged from the rotary hearth furnace and can be used as additives for sintering and converters, and can also be used as raw materials for negative expansion materials and photocatalytic materials.

[0026] In step 2), the high-temperature flue gas discharged from the rotary hearth furnace is heat exchanged to remove zinc, and zinc powder containing zinc oxide can be obtained. The high-temperature flue gas is first dusted, and then heat is recovered by a heat exchanger. After heat exchange, air is added to oxidize the zinc vapor to obtain zinc oxide dust, which is cooled by a cooler and finally recovered by a bag dust collector.

[0027] In step 2), the specific recovery process is:

[0028] First, it enters the dust removal chamber to make large dust particles fall down, and then heat is exchanged through the heat exchanger. The physical sensible heat in the flue gas can preheat the combustion air of the rotary hearth furnace. The air is added to oxidize the zinc vapor to obtain zinc oxide dust, which is further cooled by the cooler. In order to increase the concentration of zinc oxide in the finished product, the low-concentration zinc oxide dust collected at the bottom of the cooler is sent to the batching room through a pipeline to participate in the batching again, and then recycled and enriched for use. The cooled exhaust gas is sent to the dust collector, and the zinc oxide is recovered and sent to the silo for storage. The outlet of the dust collector is equipped with an induced draft fan to obtain the pressure drop required by the flue gas system. The exhaust gas can also be used to dry the system materials.

[0029] The working temperature of the rotary hearth furnace is 1250-1350℃, and the main heat transfer mode is radiation heat transfer. During the treatment process, the reduction reaction of iron / zinc oxide mainly occurs. The simultaneous reduction of iron and zinc causes a large amount of flue gas to take away a large amount of heat, and the energy efficiency is low. How to improve the energy efficiency of the rotary hearth furnace and reduce energy consumption is an urgent problem to be solved in the rotary hearth furnace process. In view of the high energy consumption of the rotary hearth furnace process, the present invention provides a method for reducing the energy consumption of the rotary hearth furnace for treating zinc-containing dust. Coal powder is used as a reducing agent, with a high carbon content, low oxygen content, and strong reduction effect, so the dezincification rate is high, but due to the good reduction effect, more iron oxides are reduced, and the amount of calcium ferrite generated is reduced; lignin is used as a biomass raw material. Compared with the traditional carbonaceous reducing agent (coal powder), lignin has a lower carbon content and a higher oxygen content, so the reduction effect is slightly lower than that of coal powder, so the dezincification rate is lower than the dezincification rate using coal powder as a reducing agent; the combustion of lignin consumes part of the carbon element, and the large porosity is conducive to the generation of calcium ferrite, so the calcium ferrite generation rate is high. The use of a single reducing agent cannot achieve the removal of zinc oxide and the generation of calcium ferrite well. Therefore, the present invention selects lignin as the main additive of the mixed reducing agent, and then adds part of coal powder and a high-efficiency catalyst to promote the removal of zinc oxide. The removal of zinc oxide needs to ensure that the residual zinc rate in the pellets after roasting is below 0.5%. It is calculated that the zinc removal rate needs to reach more than 93%, and the calcium ferrite generation is maintained at more than 90%, which can ensure the subsequent utilization of the calcium ferrite pellets.

[0030] The invention dries zinc-containing dust, a reducing agent and calcium oxide, mixes them, and then compresses them into blocks and sends them into a rotary hearth furnace for high-temperature roasting. Zinc in the dust is recovered from the exhaust gas, and the calcium ferrite pellets obtained after zinc removal can be further utilized. Under high-calcium and low-carbon conditions, the invention utilizes the high-temperature reduction process of the rotary hearth furnace to rapidly volatilize zinc in the zinc-containing dust, and the zinc removal rate can reach 94.0%. At the same time, the iron oxide in the zinc-containing dust and the calcium oxide generate calcium ferrite, and the generation rate of calcium ferrite can reach 93.1%. The successful separation of iron and zinc elements in the zinc-containing dust is achieved, and the reduction of zinc oxide and the formation of calcium ferrite are achieved, while the reduction of iron oxide is suppressed.

[0031] Compared with the traditional rotary hearth furnace process, the pellet output of the present invention is higher. The traditional rotary hearth furnace process can only obtain 585.97kg of metallized pellets by processing 1t of zinc-containing dust and carbon-containing pellets. The new process of the present invention can obtain 930.79kg of calcium ferrite pellets by processing 1t of zinc-containing dust and carbon-containing pellets, which increases the output by 58.85%. Moreover, under the same reaction temperature conditions (1250°C), the heat expenditure of the traditional rotary hearth furnace process for processing 1t of zinc-containing dust and carbon-containing pellets is 6144.53MJ, while the heat expenditure of the present invention is 3542.25MJ, which saves 42.35% and greatly reduces energy consumption. From an economic point of view, the traditional rotary hearth furnace process costs 1135.97 yuan to process 1t of zinc-containing dust and carbon-containing pellets, while the present invention only costs 802.68 yuan to process 1t of pellets, which can reduce the cost by 29.34% per ton, greatly reducing the processing cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The effects of different reducing agents on the formation rate of calcium ferrite and the dezincification rate;

[0033] Figure 2 Comparison of thermal dezincification rates between conventional rotary hearth furnace and process example 6 of the present invention;

[0034] Figure 3 Heat expenditure of conventional rotary hearth furnace process and embodiment 6 of the present invention;

[0035] Figure 4 Thermal cost expenditure of conventional rotary hearth furnace process and Example 6 of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0038] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0039] The dust treated by the present invention has a particle size of less than 0.1 mm and a moisture content of less than 6%; the dust is electric furnace dust.

[0040] The moisture content of each of the raw materials of the reducing agent, zinc-containing dust and calcium oxide is reduced to below 2% by drying before use.

[0041] Example 1

[0042] A method for reducing energy consumption of treating zinc-containing dust in a rotary hearth furnace comprises the following steps:

[0043] 1) According to the mass percentage, 71% zinc dust, 2% reducing agent and 27% calcium oxide are mixed to obtain a mixture. Among them, the reducing agent includes 69% lignin, 25% anthracite powder, and the balance is a high-efficiency catalyst. The specific raw materials and proportions are shown in Table 2. The lignin and calcium oxide are passed through an 18-mesh sieve, and the particle size is below 18 mesh. The mixture is sent to a high-pressure ball press to be pressed into raw balls of 10 to 40 mm, and then sent to a rotary hearth furnace. The fuel used in the rotary hearth furnace is coke oven gas, and the nitrogen atmosphere is protected. The mixture is heated to 1250° C. in the rotary hearth furnace and maintained for about 25 minutes. During the insulation period, nitrogen is first passed for 15 minutes and then switched to air for 10 minutes, and then the temperature is reduced with the furnace.

[0044] 2) Calcium ferrite pellets discharged from the rotary hearth furnace; After heat exchange and zinc removal of the high-temperature flue gas discharged from the rotary hearth furnace, zinc powder containing zinc oxide can be obtained. First, the high-temperature flue gas is dusted, and then heat is recovered by a heat exchanger. After heat exchange, air is added to oxidize the zinc vapor to obtain zinc oxide dust, which is cooled by a cooler and finally recovered by a bag dust collector.

[0045] Comparative Example 1

[0046] A method for reducing energy consumption of treating zinc-containing dust in a rotary hearth furnace comprises the following steps:

[0047] 1) According to the mass percentage, 71% zinc dust, 2% coal powder and 27% calcium oxide are mixed to obtain a mixture. The coal powder and calcium oxide are sieved through an 18-mesh sieve, and the particle size is less than 18 mesh. The mixture is sent to a high-pressure ball press to be pressed into raw balls of 10 to 40 mm, and then sent to a rotary hearth furnace. The fuel used in the rotary hearth furnace is coke oven gas, and the nitrogen atmosphere is protected. The mixture is heated to 1250° C. in the rotary hearth furnace and maintained for about 25 minutes. During the insulation period, nitrogen is first passed for 15 minutes and then switched to air for 10 minutes, and then the temperature is lowered with the furnace.

[0048] 2) Same as Example 1.

[0049] Comparative Example 2

[0050] A method for reducing energy consumption of treating zinc-containing dust in a rotary hearth furnace comprises the following steps:

[0051] 1) According to the mass percentage, 71% zinc dust, 2.5% biomass carbon powder and 26.5% calcium oxide are mixed to obtain a mixture. The biomass carbon powder and calcium oxide are sieved through an 18-mesh sieve, and the particle size is less than 18 mesh. The mixture is sent to a high-pressure ball press to be pressed into raw balls of 10 to 40 mm, and then sent to a rotary hearth furnace. The fuel used in the rotary hearth furnace is coke oven gas, and the nitrogen atmosphere is protected. The mixture is heated to 1250° C. in the rotary hearth furnace and maintained for about 25 minutes. During the insulation period, nitrogen is first passed for 15 minutes and then switched to air for 10 minutes, and then the temperature is reduced with the furnace.

[0052] 2) Same as Example 1.

[0053] Comparative Example 3

[0054] A method for reducing energy consumption of treating zinc-containing dust in a rotary hearth furnace comprises the following steps:

[0055] 1) According to the mass percentage, 71% zinc dust, 2.5% lignin and 26.5% calcium oxide are mixed to obtain a mixture. The lignin and calcium oxide are passed through an 18-mesh sieve, and the particle size is below 18 mesh. The mixture is sent to a high-pressure ball press to be pressed into 10-40 mm green balls, and then sent to a rotary hearth furnace. The fuel used in the rotary hearth furnace is coke oven gas, and the nitrogen atmosphere is protected. The rotary hearth furnace is heated to 1250° C. and maintained for about 25 minutes. During the insulation period, nitrogen is first passed for 15 minutes and then switched to air for 10 minutes, and then the temperature is reduced with the furnace.

[0056] 2) Same as Example 1.

[0057] After the treatment of Example 1 and Comparative Examples 1-3, the calcium ferrite generation rate and the zinc removal rate were statistically analyzed. The results are as follows: Figure 1 shown.

[0058] In Example 1, a mixed reducing agent is selected as the reducing agent. Compared with coal powder, biomass carbon powder and lignin, the calcium ferrite generation rate and the zinc removal rate are significantly improved, and the calcium ferrite generation rate and the zinc removal rate are 93.7% and 92.95% respectively.

[0059] In Comparative Example 1, coal powder is used as a reducing agent, and the formation rate of calcium ferrite is low, only 86.5%. This is because the coal powder has a strong reducing effect, resulting in more iron oxides being reduced and the calcium ferrite formation rate is low. At the same time, the coal powder participates in the reaction slowly and requires a longer reaction time. Therefore, the dezincification rate does not meet the requirements.

[0060] In Comparative Example 2, biomass carbon powder was selected as the reducing agent, the amount of calcium ferrite generated and the zinc removal rate were not high, and the reaction effect was poor.

[0061] In Comparative Example 3, lignin was selected as the reducing agent, and the calcium ferrite generation rate was relatively high. Compared with the biomass carbon powder, the generation amount of calcium ferrite was increased, but the zinc removal rate still could not meet the requirements.

[0062] The present invention selects to add lignin, coal powder and a high-efficiency catalyst and mix them in a certain proportion to prepare a high-efficiency reducing agent. When lignin is used as the reducing agent, the calcium ferrite generation rate is high, but the zinc removal rate is not high. The coal powder has a strong reduction effect. The addition of coal powder can promote the reduction of zinc oxide, but the coal powder has the problem of slow participation in the reaction. Therefore, a small amount of high-efficiency catalyst is added to catalyze the reduction of lignin, coal powder and zinc oxide.

[0063] The experiment was carried out in accordance with Example 1, with the raw material dosage ratio, insulation temperature, insulation time and the gas introduced during insulation being changed. The results are shown in Table 1.

[0064] Table 1 Experimental results under different experimental conditions

[0065]

[0066]

[0067] Table 1 shows that:

[0068] In comparative example 4, at a reaction temperature of 1150° C., a reaction time of 25 min, and a nitrogen atmosphere, the formation rate of calcium ferrite and the dezincification rate were only 87.2% and 58.7%, respectively, because the reaction temperature was too low and the reaction could not be fully achieved.

[0069] In comparative example 5, the reaction temperature was raised to 1200°C, and other reaction conditions remained unchanged, the formation rate of calcium ferrite increased to 88.7%, and the zinc removal rate increased to 77.8%, indicating that increasing the reaction temperature is beneficial to the formation of calcium ferrite and the removal of zinc oxide.

[0070] In Example 2, the temperature is further increased to 1250°C, and other reaction conditions remain unchanged. The formation rate of calcium ferrite increases to 90.1%, and the dezincification rate increases to 92.6%. However, if the temperature is further increased, calcium ferrite will decompose due to high temperature, so the reaction temperature needs to be controlled at about 1250°C.

[0071] In comparative example 6, at a reaction temperature of 1250° C., a reaction time of 5 min, and a nitrogen atmosphere, the calcium ferrite generation rate and the zinc removal rate were only 89.4% and 74.9%. This was because the reaction time was too short and the reaction was not complete, resulting in a low calcium ferrite generation rate and a low zinc removal rate.

[0072] In Example 3, the reaction time was extended to 15 min, the formation rate of calcium ferrite increased to 89.9%, and the dezincification rate increased to 85.2%.

[0073] In Example 2, the reaction time was extended to 25 minutes, the formation rate of calcium ferrite increased to 90.1%, and the dezincification rate increased to 92.6%. The reaction time of a rotary hearth furnace is generally about 25 minutes. Too long a heat preservation time will lead to high energy consumption, so the reaction time needs to be controlled at about 25 minutes.

[0074] In comparative example 7, the amount of reducing agent was reduced. When the reaction temperature was 1250°C, the reaction time was 25 min, and the amount of high-efficiency reducing agent added was 1%, the formation rate of calcium ferrite and the dezincification rate were 92.6% and 51.6% respectively under nitrogen atmosphere. This is because the amount of reducing agent added was too low and zinc oxide could not be completely reduced.

[0075] In Example 2, the amount of reducing agent added was increased to 2%, and the formation rate of calcium ferrite decreased to 90.1%, but the dezincification rate increased to 92.6%. This is because increasing the amount of reducing agent added promoted the reduction reaction of iron oxide and zinc oxide, and the increase in the reduction degree of iron oxide led to a decrease in the amount of iron oxide involved in the formation reaction of calcium ferrite, so the formation rate of calcium ferrite decreased.

[0076] In Comparative Example 8, the amount of reducing agent added was increased to 3%, the formation rate of calcium ferrite decreased to 77.3%, but the dezincification rate increased to 94.5%.

[0077] Comparative Examples 9 and 10, as well as Examples 1 and 4 to 6, attempt to promote the formation of calcium ferrite and the removal of zinc oxide by changing the reaction atmosphere, because an oxidizing atmosphere is conducive to the formation of calcium ferrite, but is not conducive to the reduction of zinc oxide, and changing the reaction atmosphere has a significant effect on the formation of calcium ferrite and the removal of zinc oxide. Taking all factors into consideration, the optimal conditions are 15 minutes of nitrogen and 10 minutes of air atmosphere (the cost of air is lower than that of oxygen), 3% of reducing agent, 71% of zinc dust, 26% of calcium oxide, and 1250°C for 25 minutes of reaction, and the calcium ferrite formation rate and zinc removal rate are 93.1% and 94%, respectively.

[0078] Comparative Example 11-Comparative Example 13

[0079] The process was carried out in accordance with Example 1, except that the catalyst raw materials and proportions were different, and the specific control was as shown in Table 2.

[0080] Table 2 High efficiency catalyst composition and its influence on calcium ferrite formation rate and zinc removal rate

[0081] Reaction conditions Cobalt oxide (%) Cerium oxide (%) Potassium chloride (%) Nickel oxide (%) Calcium ferrite generation rate (%) Zinc removal rate (%) Example 1 14 17 4 65 93.7 92.95 Comparative Example 11 14 17 1 68 92.5 78.65 Comparative Example 12 5 10 2 83 86.5 76.25 Comparative Example 13 30 30 10 30 81.5 73.25

[0082] Compared with Example 1, only the raw materials and proportions of one or more high-efficiency catalysts do not meet the requirements of the present invention, which leads to a significant decrease in the calcium ferrite formation rate and the zinc removal rate.

[0083] The conventional rotary hearth furnace processes zinc-containing dust, and the final product is metallized pellets. The specific method is: 87% of zinc-containing dust and 13% of coal powder are prepared into carbon-containing pellets and added into the rotary hearth furnace to realize the resource utilization of zinc-containing dust. The atmosphere is always maintained as nitrogen. Other experimental conditions are the same as step 1 of Example 1).

[0084] Figure 2 The zinc removal rates of the conventional rotary hearth furnace and the process (new process) of Example 6 of the present invention are compared; the mass fraction of zinc in the raw material is detected, the mass of zinc in the pellets before the reaction is calculated according to the mass of the pellets, the zinc content in the product is measured again after the reaction, and the zinc removal rate is calculated by calculation. The calculation formula is the mass of zinc in the pellets before the reaction minus the mass of zinc in the pellets after the reaction, divided by the mass of zinc in the pellets before the reaction.

[0085] Figure 3 Heat expenditure of conventional rotary hearth furnace process and Example 6 (new process) of the present invention; Figure 4 Thermal cost expenditure of traditional rotary hearth furnace process and embodiment 6 of the present invention. The material and energy consumed by the traditional rotary hearth furnace process and the new process embodiment 6 at the same reaction temperature to treat 1t of zinc-containing dust and carbon-containing pellets were calculated by the material balance method, and the energy-quality balance of the new process and the traditional rotary hearth furnace process was compared and analyzed. The economic feasibility of the new process was analyzed by calculating the cost required for the new process and the traditional rotary hearth furnace process to treat 1t of zinc-containing dust and carbon-containing pellets. Under the same reaction temperature conditions (1250°C), the heat expenditure of the traditional rotary hearth furnace process to treat 1t of zinc-containing dust and carbon-containing pellets is 6144.53MJ, and the heat expenditure of the present invention is 3542.25MJ, which saves 42.35% and greatly reduces energy consumption. From an economic point of view, the traditional rotary hearth furnace process costs 1135.97 yuan to treat 1t of zinc-containing dust and carbon-containing pellets, and the present invention only costs 802.68 yuan to treat 1t of pellets, which can reduce the cost by 29.34% per ton, greatly reducing the processing cost. The dezincification rate of the present invention is not lower than that of the traditional process, and the economic efficiency is more superior.

[0086] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.

Claims

1. A method for reducing energy consumption of treating zinc-containing dust in a rotary hearth furnace, characterized in that: The method comprises the following steps: 1) Mix the reducing agent, zinc-containing dust and calcium oxide, and send the resulting mixture into a rotary hearth furnace, heat and keep it warm, and then cool it down along with the furnace; 2) Calcium ferrite pellets are discharged from the rotary hearth furnace, and the flue gas discharged from the rotary hearth furnace is subjected to heat exchange to remove zinc, thereby obtaining zinc powder containing zinc oxide.

2. The method according to claim 1, characterized in that: The zinc-containing dust accounts for 70-73% by mass in the mixture.

3. The method according to claim 1, characterized in that The reducing agent accounts for 2-4% by weight in the mixture.

4. The method according to claim 1, characterized in that: The calcium oxide accounts for 23-28% by mass in the mixture.

5. The method according to claim 1 or 3, characterized in that: The reducing agent comprises the following raw materials in mass percentage: 60% to 70% lignin, 20% to 25% anthracite powder, and the remainder of a high-efficiency catalyst; the high-efficiency catalyst comprises the following raw materials in mass percentage: 10% to 20% cobalt oxide, 15% to 25% cerium oxide, 3% to 6% potassium chloride, and 49% to 72% nickel oxide.

6. The method according to claim 1, characterized in that The heating and heat preservation specifically includes: heating to 1250° C. in a rotary hearth furnace, keeping the temperature for 15-25 minutes, and then cooling down along with the furnace.

7. The method according to claim 6, characterized in that During the insulation period, nitrogen was passed through for 15 minutes and then switched to air for 10 minutes.

8. The method according to claim 6, characterized in that During the insulation period, nitrogen was passed through for 15 minutes and then switched to oxygen for 10 minutes.

9. The method according to claim 6, characterized in that Nitrogen was always introduced during the insulation period.

10. The method according to claim 1, characterized in that In step 2), the high temperature flue gas discharged from the rotary hearth furnace is subjected to heat exchange to remove zinc, thereby obtaining zinc powder containing zinc oxide.

Citation Information

Patent Citations

  • Method for recovering zinc oxide in Zn-containing dust treatment by rotary hearth furnace

    CN101386913A

  • Zinc recovery method based on HIsmelt smelting reduction furnace

    CN111647704A

  • Comprehensive utilization process of zinc-containing iron dust

    CN102534199A

  • Treatment method of zinc-bearing dust for steel works

    CN102776309A