Method for extracting vanadium from molten iron and semi-steel

By using the impact force of the iron flow and the reaction of the vanadium extracting oxidant in the iron water during the blast furnace discharge process, the problem of long and low efficiency of vanadium extraction in the prior art is solved, and rapid and thorough vanadium oxidation and high purity are achieved. The production of vanadium slag improves production efficiency and the quality of vanadium slag.

CN118957307APending Publication Date: 2024-11-15PANZHIHUA IRON & STEEL RES INST OF PANGANG GROUP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411170397.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing molten vanadium extraction process fails to effectively utilize the molten impact force during blast furnace discharge, resulting in a long time to extract vanadium, low efficiency, and insufficient purity and yield of vanadium slag.

Method used

During the blast furnace discharge process, when the molten iron enters 10% to 20% of the molten iron tank, a vanadium extracting oxidant is added, and the impact force of the iron flow makes it fully react with the molten iron. After the iron discharge is completed, the molten iron tank is transported to the vanadium extracting. The converter combines the appropriate oxygen supply intensity and oxygen blowing time to oxidize the high-purity vanadium slag.

Benefits of technology

The impact force of the iron flow accelerates the oxidation reaction, shortens the vanadium extraction time, improves the oxidation rate of vanadium and the purity of the slag, reduces production costs, enhances thermal efficiency, and reduces uncertain factors to stabilize product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957307A_ABST
    Figure CN118957307A_ABST
Patent Text Reader

Abstract

The method comprises the steps that during blast furnace tapping, when the weight of the molten iron entering a molten iron tank reaches 10%-20% of the tapping amount, a vanadium extraction oxidizing agent is added into the molten iron tank, the vanadium extraction oxidizing agent and the molten iron are fully reacted through the impact force of iron flow, and the vanadium is extracted through the vanadium extraction oxidizing agent; and after tapping is finished, the molten iron tank is hoisted to a vanadium extraction converter, iron and surface slag are mixed into the converter, and semi-steel and vanadium slag are obtained after the vanadium extraction converter reaction is finished. According to the method, the molten iron impact force is effectively utilized for stirring and vanadium extraction in the tapping process, so that the formation of a vanadium extraction slag system is accelerated, the vanadium extraction time of the converter is shortened, and the vanadium extraction production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel smelting, and in particular to a method for extracting vanadium from molten iron and semi-steel. Background Art

[0002] my country is a country with a large amount of vanadium-titanium magnetite. Many large steel enterprises use vanadium-titanium magnetite for smelting. The molten iron smelted by vanadium-titanium magnetite blast furnace has a high vanadium content. Vanadium is an important resource. Therefore, vanadium must be extracted before molten iron is used for steelmaking to produce vanadium slag. At present, there are many production methods for producing vanadium slag at home and abroad, mainly including New Zealand's ladle vanadium blowing process, South Africa's shaking ladle vanadium extraction process, Russia and China's converter vanadium extraction process, etc. Other vanadium extraction processes include vanadium extraction from vanadium-containing steel slag and stone coal vanadium extraction process.

[0003] The production process system of vanadium extraction in converters at home and abroad is to add coolant + process temperature + continuous improvement of blowing time. Vanadium extraction from hot metal is a selective oxidation technology. The vanadium extraction from converter gas supply is an exothermic process. The oxidation of elements such as [Si], [Mn], [V], and [C] causes the molten pool to heat up rapidly. The oxidation of [Si] and [Mn] occurs before the oxidation of [V]. It is impossible for vanadium extraction to inhibit their reaction. The conversion temperature of [C] and [V] is about 1385℃. Therefore, in order to obtain a high oxidation rate of [V] and a [V] yield, a vanadium extraction coolant must be added to control the molten pool temperature to approach the conversion temperature of [C] and [V], so as to achieve the purpose of vanadium extraction and carbon preservation, and reduce [V] to below 0.05%. The terminal semi-steel temperature of vanadium extraction should not be too high. The vanadium extraction process is mainly vanadium oxidation in the early stage and vanadium reduction in the later stage, but the vanadium blowing process is mainly vanadium reduction. Therefore, when cooling down, coolant is added to reduce the temperature of the molten iron to an appropriate range. During converter smelting, the vanadium in the semi-steel is oxidized by controlling the blowing time and process temperature to increase the yield.

[0004] For example, Chinese patent application number CN200510132606.1 discloses a coolant for vanadium extraction from molten iron and a process for vanadium extraction from molten iron and calcium control. The chemical composition (Wt%) of the vanadium extraction coolant is: 56-60% iron oxide scale, 30-40% iron ore powder, and 5-10% binder. The coolant can increase the vanadium extraction rate and vanadium slag grade, and stabilize the calcium oxide content of the vanadium slag.

[0005] For example, Chinese patent application number CN200810304225.0 discloses a vanadium-extracting coolant and its preparation method and use method. The coolant is produced with iron oxide scale or vanadium-extracting sludge, vanadium-containing iron concentrate, and a binder as raw materials, and contains 80%-95% iron oxide, 3-6% SiO2, 0.1-0.6% V2O5, and 1-3% MgCl2.

[0006] For example, a Chinese patent application numbered CN201510006728.X discloses a method for extracting vanadium from vanadium-containing molten iron. The vanadium-containing molten iron is stirred at a stirring speed of 50 to 150 r / min, an immersion depth of a stirring head of 200 to 800 mm, and a stirring time of 20 to 40 min. While stirring, iron oxide is sprayed into the molten iron in an amount of 15 to 50 kg / tFe. After the spraying and stirring are completed, the vanadium slag is scraped out to obtain semi-steel.

[0007] The above scheme has not yet mentioned the technical solution of extracting vanadium by utilizing the impact force of molten iron in the blast furnace iron-making process. In view of this, improvements should be made to the existing technology. Summary of the invention

[0008] The main purpose of the present invention is to provide a method for extracting vanadium from molten iron and semi-steel, which can effectively utilize the impact force of molten iron to stir and extract vanadium during the iron-tapping process, thereby accelerating the formation of a vanadium-extracting slag system, shortening the vanadium-extracting time in a converter, and contributing to improving the vanadium-extracting production efficiency.

[0009] According to one aspect of the present invention, a method for extracting vanadium from molten iron is provided, which comprises adding a vanadium-extracting oxidant into the molten iron tank when the weight of the molten iron entering the molten iron tank reaches 10-20% of the tapping amount during iron tapping from a blast furnace, allowing the vanadium-extracting oxidant to fully react with the molten iron through the impact force of the iron flow, and after the tapping is completed, hoisting the molten iron tank to a vanadium-extracting converter and adding iron and surface slag into the furnace, and obtaining semi-steel and vanadium slag after the reaction in the vanadium-extracting converter is completed.

[0010] According to one embodiment of the present invention, the vanadium-extracting oxidant includes a manganese source and an iron-containing material.

[0011] According to one embodiment of the present invention, TFe>60% in the iron-containing material by weight.

[0012] According to one embodiment of the present invention, the weight ratio of the manganese source to the iron-containing material is 1-2:8-9.

[0013] According to one embodiment of the present invention, the amount of vanadium extraction oxidant added is 30-50 kg / (t iron).

[0014] According to one embodiment of the present invention, the particle size range of the vanadium extraction oxidant is 1-5 mm.

[0015] According to one embodiment of the present invention, the production parameters of the vanadium extraction converter reaction are oxygen supply intensity 2~3m 3 / (t.min), oxygen supply pressure 0.7~1.2MPa, oxygen blowing time 3~5min.

[0016] According to one embodiment of the present invention, the manganese source includes manganese ore and / or manganese-containing waste.

[0017] According to one embodiment of the present invention, the manganese ore includes one or more of manganese ore, hausmannite or francone.

[0018] According to another aspect of the present invention, a semi-steel is provided, which is prepared by using any one of the methods in the above technical solutions.

[0019] In a method for extracting vanadium from molten iron according to an embodiment of the present invention, by effectively utilizing the impact force of the molten iron to stir and extract vanadium during the iron tapping process, it is beneficial to accelerate the formation of a vanadium-extracting slag system, shorten the vanadium extraction time in the converter, and help improve the vanadium extraction production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the drawings required for use in the embodiment will be briefly introduced below. Obviously, the drawings described below are only some implementation cases of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 A process flow chart of a method for extracting vanadium from molten iron according to an exemplary embodiment of the present invention is shown. DETAILED DESCRIPTION

[0022] The detailed description of the following embodiments is used to exemplify the principles of the present invention, but cannot be used to limit the scope of the present invention. The present invention can be implemented in many different forms and is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

[0023] The present invention provides these embodiments to make this disclosure thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.

[0024] It should be noted that, in the description of the present invention, unless otherwise specified, the meaning of "multiple" is greater than or equal to two; the terms "upper", "lower", "left", "right", "inner", "outer", etc., indicating the orientation or positional relationship, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. When the absolute position of the object being described changes, the relative positional relationship may also change accordingly.

[0025] It should also be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected or indirectly connected through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. When a specific device is described as being located between a first device and a second device, there may or may not be an intermediate device between the specific device and the first device or the second device.

[0026] All terms used in the present invention have the same meanings as those understood by those of ordinary skill in the art to which the present disclosure belongs, unless otherwise specifically defined. It should also be understood that terms defined in general dictionaries, for example, should be interpreted as having meanings consistent with their meanings in the context of the relevant technology, and should not be interpreted in an idealized or extremely formal sense, unless explicitly defined herein.

[0027] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, these technologies, methods, and equipment should be considered part of the specification.

[0028] like Figure 1 As shown, the present invention provides a method for extracting vanadium from molten iron, which comprises: S1, when the weight of the molten iron entering the molten iron tank reaches 10-20% of the amount of iron tapped during iron tapping from a blast furnace, adding a vanadium-extracting oxidant into the molten iron tank; S2, allowing the vanadium-extracting oxidant to fully react with the molten iron through the impact force of the iron flow; S3, after the iron tapping is completed, hoisting the molten iron tank to a vanadium-extracting converter and adding iron and surface slag into the furnace, and obtaining semi-steel and vanadium slag after the reaction in the vanadium-extracting converter is completed.

[0029] In the method for extracting vanadium from molten iron according to an embodiment of the present invention, by effectively utilizing the impact force of the molten iron to stir and extract vanadium during the iron tapping process, it is beneficial to accelerate the formation of the vanadium extraction slag system, shorten the vanadium extraction time in the converter, and help improve the vanadium extraction production efficiency.

[0030] Specifically, the violent impact of molten iron can break the original static or inefficient mixing state, causing the contact area between the molten iron and the vanadium-extracting oxidant or related reactants to increase dramatically, thereby accelerating the chemical reaction rate and facilitating the formation and aggregation of target products such as vanadium oxides.

[0031] By controlling the impact force of the iron flow and the type and amount of the oxidant, the oxidation of other elements in the molten iron (such as Si, Ti, Mn, etc.) can be minimized, thereby improving the purity of the vanadium slag.

[0032] The impact force of the iron flow can also enhance the stirring effect of the molten pool, making the temperature and concentration distribution in the molten pool more uniform. This helps to eliminate local overheating or overcooling and improve the stability of reaction kinetics.

[0033] In the process of vanadium extraction from molten iron, the generated V2O5 will enter the slag phase together with oxides of other easily oxidizable elements. The impact force of the iron flow helps to promote the separation of slag and steel, making it easier to separate vanadium slag from molten iron.

[0034] Since the impact force of the iron flow improves the oxidation reaction efficiency, the amount of oxidant used can be reduced to a certain extent. This helps to reduce production costs.

[0035] A sufficient oxidation reaction can release more heat energy, which can be recycled to improve the thermal efficiency of the entire vanadium extraction process.

[0036] By optimizing the oxidation reaction conditions and the slag-steel separation effect, higher purity vanadium slag can be obtained, which helps to improve the quality of subsequent products such as ferrovanadium and industrial V2O5.

[0037] The impact force of the iron flow helps to reduce fluctuations and uncertainties in the reaction process, thereby stabilizing product quality.

[0038] In some specific embodiments, the vanadium extraction oxidant includes a manganese source and an iron-containing material. As an oxidant, the manganese source can accelerate the oxidation reaction, shorten the reaction time, and improve production efficiency. In addition, the manganese source may also promote the release and leaching of vanadium by improving the microstructure of the ore or slag.

[0039] In some specific embodiments, the iron-containing material has TFe>60% by weight. Certain oxides (such as FeO) contained in the iron-containing material have certain oxidizing properties and can promote the oxidation of vanadium to a certain extent. When the TFe content in the iron-containing material is high, it may mean that these potential oxidizing components also increase accordingly, thereby facilitating the oxidation process of vanadium.

[0040] Based on the above examples, the weight ratio of manganese source to iron-containing material is 1-2:8-9. The main component of manganese ore is MnO, which can act as a low-melting-point oxide to reduce the melting point of vanadium slag, promote the increase of FeO activity in the slag, and improve the effect of oxidizing vanadium in molten iron.

[0041] Based on the above examples, the amount of vanadium extraction oxidant added is 30-50 kg / (t iron).

[0042] In some specific embodiments, the particle size of the vanadium extraction oxidant is in the range of 1 to 5 mm. The oxidant with a particle size of 1 to 5 mm can significantly increase the contact area with the vanadium ore or vanadium slag, making the oxidation reaction more sufficient and rapid. This helps to accelerate the oxidation process of vanadium and improve the leaching rate of vanadium.

[0043] In some specific embodiments, the production parameters of the vanadium extraction converter reaction are oxygen supply intensity 2-3m 3 / (t.min), oxygen supply pressure 0.7~1.2MPa, oxygen blowing time 3~5min. In this application, production parameter control can ensure the continuity and stability of the vanadium extraction process, and reduce production interruptions and adjustment time caused by parameter fluctuations. This helps to improve production efficiency and increase output. Stable process conditions can reduce fluctuations and uncertainties in the production process, and reduce operational difficulty and risk.

[0044] In some specific embodiments, the manganese source includes manganese ore and / or manganese-containing waste. Directly using manganese ore or manganese-containing waste as the manganese source can reduce the exploitation of new manganese ore resources, thereby protecting limited natural resources. In addition, utilizing manganese ore or manganese-containing waste as the manganese source usually has lower cost, because waste treatment is often more economical than new mining.

[0045] In some specific embodiments, the manganese ore includes one or more of manganese ore, ferromanganese ore or ferromanganese ore. Manganese ore is an alkaline manganese oxide mineral, mainly used as a deoxidizer and desulfurizer in iron and steel making processes, and used to make alloys. In practical applications, a suitable manganese ore can be selected as a manganese source according to specific needs.

[0046] The present invention also provides a semi-steel, which is prepared by using any method of the above technical solutions.

[0047] The solution of the present application is described below through specific embodiments.

[0048] Example 1 In the process of blast furnace iron tapping, manganese ore and iron-containing materials are used as vanadium-extracting oxidants. The TFe content in the iron-containing materials used is 62%, the particle size is 1-5 mm, and the weight ratio of manganese ore and iron-containing materials is 1:9. When the weight of molten iron entering the molten iron tank reaches 10% of the iron tapping amount, the vanadium-extracting oxidant is added to the molten iron tank. The amount of oxidant added is 30 kg / (t iron). The impact force of the iron flow is used to achieve full reaction between the vanadium-extracting oxidant and the molten iron. After the iron tapping is completed, the molten iron tank is hoisted to the vanadium-extracting converter and the iron and surface slag are added into the furnace. The vanadium-extracting converter is controlled according to the following vanadium-extracting production parameters: oxygen supply intensity 2m 3 / (t.min), oxygen supply pressure 0.7MPa, oxygen blowing time 5min, no coolant is added to the vanadium extraction converter to control the temperature, and semi-steel and vanadium slag are produced after the reaction. The vanadium content of semi-steel is reduced from 0.30% to 0.02%, and the vanadium oxidation rate is 93.33%.

[0049] Example 2 In the process of blast furnace iron tapping, manganese ore and iron-containing materials are used as vanadium-extracting oxidants. The iron-containing materials used have a TFe content of 60% and a particle size of 1-5 mm. The weight ratio of manganese ore and iron-containing materials is 2:8. When the weight of molten iron entering the molten iron tank reaches 20% of the iron tapping amount, the vanadium-extracting oxidant is added to the molten iron tank. The amount of oxidant added is 50 kg / (t iron). The impact force of the iron flow is used to achieve full reaction between the vanadium-extracting oxidant and the molten iron. After the iron tapping is completed, the molten iron tank is hoisted to the vanadium-extracting converter and the iron and surface slag are added into the furnace. The vanadium-extracting converter is controlled according to the following vanadium-extracting production parameters: oxygen supply intensity 3m 3 / (t.min), oxygen supply pressure 1.2MPa, oxygen blowing time 3min, no coolant is added to the vanadium extraction converter to control the temperature, and semi-steel and vanadium slag are produced after the reaction. The vanadium content of semi-steel is reduced from 0.32% to 0.03%, and the vanadium oxidation rate is 90.63%.

[0050] Example 3 In the process of blast furnace iron tapping, manganese ore and iron-containing materials are used as vanadium-extracting oxidants. The TFe content in the iron-containing materials used is 65%, the particle size is 1-5 mm, and the weight ratio of manganese ore and iron-containing materials is 1.5:8.5. When the weight of molten iron entering the molten iron tank reaches 15% of the iron tapping amount, the vanadium-extracting oxidant is added to the molten iron tank. The amount of oxidant added is 40 kg / (t iron). The impact force of the iron flow is used to achieve full reaction between the vanadium-extracting oxidant and the molten iron. After the iron tapping is completed, the molten iron tank is hoisted to the vanadium-extracting converter and the iron and surface slag are added into the furnace. The vanadium-extracting converter is controlled according to the following vanadium-extracting production parameters: oxygen supply intensity 2.5 m 3 / (t.min), oxygen supply pressure 0.8MPa, oxygen blowing time 4min, no coolant is added to the vanadium extraction converter to control the temperature. After the reaction is completed, the semi-steel and vanadium slag are produced. The vanadium content of the semi-steel drops from 0.35% to 0.04%, and the vanadium oxidation rate is 88.57%.

[0051] After the implementation of the present invention, at least the following beneficial effects are achieved: (1) The impact force of the iron flow can break the surface tension of the molten iron, allowing the vanadium-extracting oxidant to be better dispersed and penetrate into the molten iron, thereby increasing the contact area between the oxidant and the molten iron. This sufficient mixing and contact helps the oxidation reaction proceed more quickly and thoroughly.

[0052] (2) When the oxidant is in full contact with the molten iron, the oxidation reaction can occur more quickly. This not only shortens the reaction time, but also improves the oxidation efficiency of vanadium, allowing more vanadium to be oxidized from the molten iron.

[0053] (3) In the process of vanadium extraction from molten iron, it is usually hoped that vanadium can be quickly and preferentially oxidized to V2O5 for subsequent extraction. The impact force of the iron flow helps to strengthen this selective oxidation process, allowing vanadium to gain an advantage in the process of competing with other elements for oxidation.

[0054] The above are exemplary embodiments disclosed in the present invention. The order disclosed in the above embodiments of the present invention is for description only and does not represent the advantages and disadvantages of the embodiments. However, it should be noted that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope disclosed in the embodiments of the present invention (including the claims) is limited to these examples. Various changes and modifications may be made without departing from the scope defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.

[0055] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.

Claims

1. A method for extracting vanadium from molten iron, characterized in that: Including when the blast furnace is tapping iron, when the weight of the molten iron entering the molten iron tank reaches 10~20% of the tapping amount, a vanadium-extracting oxidant is added to the molten iron tank, and the impact force of the iron flow allows the vanadium-extracting oxidant to fully react with the molten iron. After the tapping is completed, the molten iron tank is hoisted to the vanadium-extracting converter and the iron and surface slag are added into the furnace. After the reaction in the vanadium-extracting converter is completed, semi-steel and vanadium slag are obtained.

2. The method for extracting vanadium from molten iron according to claim 1, characterized in that: The vanadium-extracting oxidant comprises a manganese source and an iron-containing material.

3. The method for extracting vanadium from molten iron according to claim 2, characterized in that: In terms of weight percentage, TFe in the iron-containing material is greater than 60%.

4. The method for extracting vanadium from molten iron according to claim 2, characterized in that: The weight ratio of the manganese source to the iron-containing material is 1-2:8-9.

5. The method for extracting vanadium from molten iron according to claim 1, characterized in that: The amount of the vanadium-extracting oxidant added is 30-50 kg / (t iron).

6. The method for extracting vanadium from molten iron according to claim 1, characterized in that: The particle size range of the vanadium extraction oxidant is 1-5 mm.

7. The method for extracting vanadium from molten iron according to claim 2, characterized in that: The production parameters of the vanadium extraction converter reaction are as follows: oxygen supply intensity is 2-3m 3 / (t.min), oxygen supply pressure 0.7~1.2MPa, oxygen blowing time 3~5min.

8. The method for extracting vanadium from molten iron according to claim 2, characterized in that: The manganese source includes manganese ore and / or manganese-containing waste.

9. The method for extracting vanadium from molten iron according to claim 8, characterized in that: The manganese ore includes one or more of manganese ore, hausmannite or francone.

10. A semi-steel, characterized in that: The method is prepared by any one of claims 1 to 9.