Tank material aluminum alloy smelting process

Through the classification and smelting process of double-chamber furnace and smelting furnace, the problems of large burning and high energy consumption of small and medium-sized wastes in the existing technology have been solved, and the recycling rate of aluminum alloy and the purity of the melt are improved, thus achieving high efficiency, Low cost aluminum alloy recycling.

CN118957325APending Publication Date: 2024-11-15CHONGQING NATIONAL INNOVATION INSTITUTE OF LIGHT ALLOYS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411043482.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing aluminum alloy recycling and smelting technology, small size, thin, oil-containing and coated wastes have greater oxidation and burning, resulting in serious slag-making of aluminum alloy melt, low recycling rate, high energy consumption and cost, and waste of resources. serious.

Method used

The smelting process of dual-chamber furnace and smelting furnace is adopted to classify and process aluminum alloy waste of different sizes and types through classification, reduce oxidation and burning, control smelting conditions, and directly flow into the insulation furnace to refine, avoid secondary transport and casting processes, improve recycling efficiency and Utilization.

Benefits of technology

Effectively reduce the burn-out rate of small-sized waste, improve the recycling rate of aluminum alloy, reduce energy consumption and cost, realize the same-level recycling of high proportion of waste, and meet the high requirements of tank material for melt purity .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of aluminum alloy recycling, and discloses a tank material aluminum alloy smelting process which comprises the following steps: (1) a tank material aluminum alloy classification stage: classifying the recycled tank material aluminum alloy; (2) a graded feeding and smelting stage: feeding different types of classified wastes into different chambers of a double-chamber furnace and a smelting furnace in a graded manner for smelting; and (3) treating outside the furnace. According to the scheme, different types of aluminum waste are put into different furnaces to be smelted, and the smelting conditions (such as the smelting temperature and the circulating smelting time) can be specifically controlled according to the types of the aluminum waste needing to be treated, so that specific smelting is effectively achieved, the aluminum scrap adding amount is increased to the maximum extent, and the recycling efficiency of the aluminum waste is improved; and the same-stage recycling level of the aluminum alloy of the tank body material is improved. And meanwhile, the phenomenon of energy waste easily caused by direct feeding smelting in the prior art and the situation that small-size waste is easily burnt can be effectively avoided, and smelting energy consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloy recycling, and in particular to a can body aluminum alloy smelting process. Background Art

[0002] Aluminum alloy can material (such as cans) is the most mature aluminum product in the current recycling and reuse system, and the average cycle of the "can to can" recycling cycle is only 2 months, that is, the recycled aluminum cans can be re-formed into products on the shelves within 60 days. However, due to the large number of sizes of aluminum alloy can material waste, different sizes of can materials are subject to large oxidation and burning losses during recycling and smelting, especially small-sized, thinner waste, oil-containing and coated waste, which leads to serious slag formation in the aluminum alloy melt, and ultimately affects the product's can break rate. In addition, the quality of recycled can materials in the industry is uneven, and waste cans are often downgraded after recycling, which has brought great obstacles to the development of grade-preserving recycling technology and caused serious waste of resources.

[0003] At present, for the recycling of scrap aluminum from can materials, the existing smelting system is usually equipped with a smelting furnace and a holding furnace, and smelting is carried out in two ways: one is to melt the recycled aluminum scraps together into aluminum liquid, make them into regenerated ingots or complex ingots by casting, and then put the regenerated ingots or complex ingots into a smelting furnace for smelting, and refine them in a holding furnace; the other is to melt the scraps into aluminum liquid, pour the aluminum liquid into an aluminum liquid bag, and then transport it to the furnace door of the smelting furnace, directly add furnace water into the smelting furnace, and refine them in a holding furnace (see the prior art CN117107068A, a method for preserving and reducing recycled aluminum 3 series cans and its equipment). However, the existing technology has the following technical problems: (1) The oxidation and burning loss of small-sized scrap, thin scrap, oil-containing and coated scrap in the above two methods is large, the melt slag is serious, and it is difficult to ensure the purity of the melt, resulting in a low recycling rate of scrap aluminum for the final can body material; (2) The first method has a secondary melting and casting process, which consumes a lot of energy and consumables; (3) The second method has a distance requirement for the aluminum liquid manufacturer to reduce the temperature loss of the aluminum liquid, and more aluminum liquid bag use and transportation costs are required. In addition, the aluminum liquid after transportation has a certain heat loss, thereby increasing the smelting energy consumption. In summary, the cost investment of the existing smelting method is large, the same-level utilization rate of scrap is not high, resulting in a waste of resources.

[0004] In view of this, the development of a can material aluminum alloy smelting process with small burning loss and low energy consumption can not only effectively make up for the shortcomings of the existing technology, but also can simultaneously process different sizes and types of can material scrap aluminum, which is of great significance to improving the same-level recycling level of can material aluminum alloy. Summary of the invention

[0005] The present invention aims to provide a smelting process for aluminum alloy of can body material, so as to solve the technical problem that the recycling burning loss of aluminum alloy of can body material in the existing smelting method is large, resulting in a low recycling rate.

[0006] To achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a can body aluminum alloy smelting process, comprising (i) a can body aluminum alloy classification stage, in which the recycled can body aluminum alloy is classified; (ii) a graded feeding smelting stage, comprising the following steps: S1, double-chamber furnace material preparation and feeding; S2, double-chamber furnace stirring, melting, and slag removal; S3, smelting furnace material preparation and feeding; S4, aluminum liquid in the double-chamber furnace confirmed composition, converter; S5, smelting furnace melting, stirring; S6, smelting furnace refining, slag removal; S7, aluminum liquid composition detection and adjustment in the smelting furnace; S8, aluminum liquid in the smelting furnace converter; S9, refining, standing, and slag removal in a holding furnace; the different types of waste obtained by classification are graded and fed to different chambers of the double-chamber furnace and the smelting furnace for smelting; (iii) an out-of-furnace treatment stage.

[0007] The principles and advantages of this solution are:

[0008] 1. Compared with the prior art, in which the aluminum alloy waste of can body materials (aluminum waste for short) is first melted into aluminum liquid and cast into ingots, and then transferred to a smelting furnace for smelting and an insulation furnace for refining, which results in greater oxidation and burning loss of the aluminum alloy of the can body materials, this scheme first classifies the recycled aluminum alloy of can body materials (also called aluminum waste) of different sizes, and then puts different types of aluminum waste into different positions of a double-chamber furnace (including a heating chamber, a waste chamber and a vortex well) and a smelting furnace for smelting, thereby improving the recycling and smelting capacity of aluminum waste of different sizes and thicknesses, reducing the oxidation and burning loss rate of small-sized and thin-sheet waste, and effectively improving the recycling efficiency of aluminum alloy of can body materials.

[0009] 2. This solution can effectively achieve specific smelting by putting different types of aluminum waste into different furnaces for smelting, and can also specifically control the smelting conditions (such as smelting temperature, cycle smelting time, etc.) according to the type of aluminum waste to be processed, thereby maximizing the amount of waste aluminum added, improving the recycling efficiency of aluminum waste, and improving the recycling level of aluminum alloy of can body materials at the same level. At the same time, it can also effectively avoid the energy waste phenomenon that is easy to occur in the direct feeding smelting of the existing technology, and reduce the smelting energy consumption.

[0010] 3. Compared with the prior art, which requires more transportation costs and energy consumption for refining various aluminum wastes after preliminary melting and casting into ingots, the aluminum liquid obtained by melting in the double-chamber furnace and the melting furnace of this scheme can be directly flowed into the insulation furnace for refining. There is no need to transfer the aluminum liquid for a second time, or to cast it into ingots and then remelt it for use, which effectively saves smelting energy consumption, thereby reducing the recovery and smelting cost of aluminum alloy for can body materials.

[0011] Preferably, as an improvement, in the (i) can body aluminum alloy classification stage, the classification method is as follows: the can body aluminum alloy scrap is classified according to the type of can body aluminum alloy scrap treated with different molten pool specificities:

[0012] (1) Aluminum scraps: Aluminum scraps from the crushing of waste aluminum and milling produced by machining in the factory, with a size less than 5 cm 2 , thickness less than 0.1mm;

[0013] (2) Cutting head and tail waste: Cutting head and tail waste of ingots, the diameter or length of a single waste is greater than 100mm and the weight is not less than 10kg;

[0014] (3) Baled or block-shaped waste: aluminum waste in the form of baled blocks, recycled ingots, or twisted rolls, with a thickness greater than 0.1 mm;

[0015] (4) Waste in the form of flakes or blocks: recycled ingots, residual rolls without liquid, scraps, thin sheets and baled blocks, some heads and tails, and aluminum ingots.

[0016] Beneficial effect: This solution classifies the recycled aluminum alloy of can body materials, making it easier to grade and smelt aluminum scraps of different sizes and thicknesses, thereby effectively improving the recycling rate of aluminum alloy of can body materials.

[0017] Preferably, as an improvement, (ii) the graded feeding and smelting stage is completed in a graded smelting system, the graded smelting system comprises a double-chamber furnace, a smelting furnace and a holding furnace connected by a flow channel, and plugging rods are provided at both ends of the flow channel to control the inflow and outflow of aluminum liquid in the double-chamber furnace, the smelting furnace and the holding furnace; the double-chamber furnace comprises a connected heating chamber and a waste chamber, and the heating chamber, the waste chamber, the smelting furnace and the holding furnace are all provided with furnace doors; the flow channel between the waste chamber and the smelting furnace is a first flow channel, and the flow channel of the smelting furnace and the holding furnace is a second flow channel, and a vortex well is also connected between the waste chamber and the smelting furnace, a debris inlet is provided at the top of the vortex well, and a pipeline at the bottom of the vortex well is connected to the first flow channel.

[0018] Beneficial effect: This solution adopts the above-mentioned setting, which is convenient for simultaneously processing aluminum waste of different classifications, realizing graded smelting of recycled aluminum waste, and thus improving the recycling efficiency of aluminum waste. The applicant has found through long-term experiments that if only a smelting furnace is used to smelt and recycle aluminum waste, it will not be possible to take into account both the processing efficiency and the recycling rate. Specifically, if it is directly put into smelting without grading, it will cause large burnout of small-sized and thin materials and reduce the recycling rate. If only a smelting furnace is used for graded smelting, different types of aluminum waste need to be smelted separately. Not only is it troublesome to adjust the smelting parameters, but the smelting efficiency of a single furnace will also be significantly reduced. If a two-stage or more smelting furnace is used, although the recycling rate and smelting efficiency of aluminum waste can be improved to a certain extent, the degree of improvement is very limited, and the operation of a multi-stage smelting furnace alone will also increase the smelting energy consumption. The present solution combines a double-chamber furnace, a smelting furnace and a holding furnace. The double-chamber furnace is divided into a heating chamber and a waste chamber. The waste chamber is connected to the vortex well, so as to realize "one heating, three utilizations" (i.e., the molten aluminum in the heating chamber is circulated to the waste chamber to melt the cut heads and tails waste, and then transported to the vortex chamber to melt the scrap aluminum material). This effectively improves the utilization rate of the molten aluminum in the heating chamber and reduces the smelting energy consumption in the waste chamber and the vortex well.

[0019] Preferably, as an improvement, in S1, the following steps are included: after feeding the cut head and tail scraps into the heating chamber, heating is started; after feeding the packaged scraps or block scraps into the scrap chamber, the circulation of the aluminum liquid in the heating chamber and the scrap chamber is started immediately after the scraps are fed into the scrap chamber; when the packaged scraps or block scraps contain water or oil, the scraps are first stacked on the furnace bridge in the scrap chamber, and the high temperature of the aluminum liquid is used to bake the scraps until the water and oil evaporate, and then the scraps are pushed into the scrap chamber for smelting; the furnace temperature in the heating chamber is 1050-1120°C, and the furnace temperature in the scrap chamber is 750-850°C; in S2, slag removal is performed when all the raw materials in the double-chamber furnace are melted and the aluminum liquid temperature is ≥720°C.

[0020] Beneficial effect: This solution adopts the above-mentioned setting to facilitate the coordinated treatment of wastes of different sizes and types. Specifically, the thickness of the cut head and tail waste is higher, and the use of a higher furnace temperature can effectively improve its melting efficiency, and circulating the aluminum liquid in the heating chamber to the waste chamber can effectively reduce the melting energy consumption of the cut head and tail waste. In addition, by pre-treating impurities such as water and oil in the cut head and tail waste, its impact on the quality of the aluminum liquid is effectively reduced, further improving the same-level recycling level of aluminum waste.

[0021] Preferably, as an improvement, in S3, flake or block waste is fed into the smelting furnace for smelting, and the order of feeding aluminum waste into the smelting furnace is as follows: thin flakes, scraps and packaged blocks, residual rolls and heads and tails, recycled ingots and aluminum ingots; in S5, after the feeding is completed, it can be ignited and melted, and the furnace temperature in the smelting furnace is 950-1100°C.

[0022] Beneficial effect: This solution can minimize the oxidation and burning of the waste by laying thin waste flakes on the bottom of the double-chamber furnace.

[0023] Preferably, as an improvement, in S4, after the slag removal operation of the double-chamber furnace is completed and the temperature of the aluminum liquid is ≥720°C, a sample is taken, and the composition of each element is analyzed by a direct-reading spectrometer, and the converter is performed after confirming that the composition meets the requirements of the production plan; during the converter process, a part of the aluminum liquid in the double-chamber furnace is directly converted to the smelting chamber, and a part of the aluminum liquid is tangentially pumped to the vortex well to form a vortex, and aluminum scraps are fed into the vortex well, and the aluminum liquid obtained by mixed smelting is then converted to the smelting chamber; the proportion of scraps in each furnace of aluminum waste is ≤30%.

[0024] Beneficial effect: This scheme adopts the above-mentioned setting and confirms the composition requirements with reference to the composition standard GBT 3190-2020, so that the scrap aluminum waste can be directly melted into the smelting furnace for subsequent treatment, without the need to be separately compounded into aluminum liquid and added to the smelting furnace or melted and cast into ingots for remelting and use. The applicant has found through long-term experiments that the scraps are usually obtained by mechanical crushing or machining, and the surface is prone to carry some oil. If the proportion is too high, it will cause serious environmental pollution and serious slag formation in the melt. And the above-mentioned slagging is to fully stir the melt, and the melt temperature reaches above 720°C, so as to effectively ensure the increase of the diffusion rate of elements with high specific gravity such as Mn, ensure the uniformity of the composition of alloy elements with different specific gravity in the melt, and prevent the stratification and segregation of the sample. At the same time, defects such as inclusions, pores, and looseness can be avoided above this temperature.

[0025] Preferably, as an improvement, in S4, the temperature of the aluminum liquid in the double-chamber furnace during the converter is 710-740°C, and the height of the remaining aluminum liquid in the double-chamber furnace after the converter should be higher than the circulating liquid level line of the electromagnetic pump in the furnace to prevent excessive aluminum liquid from affecting the operation of the electromagnetic pump. The height of the circulating liquid level line of the electromagnetic pump is 0.4-0.6 times the height in the furnace to ensure that the space in the lower half of the furnace can effectively melt the aluminum material, and the space in the upper half of the furnace is used for the circulation of aluminum liquid between the two molten pool chambers.

[0026] Beneficial effect: This scheme adopts the above-mentioned setting to facilitate the circulation of aluminum liquid between the chambers of the double-chamber furnace molten pool and improve the melting efficiency. The applicant has found through long-term experiments that if the aluminum liquid temperature in the double-chamber furnace is too high during the converter, it will bring more gas slag to the melt; if the aluminum liquid temperature in the double-chamber furnace is too low during the converter, it will cause the melt temperature to be too low after being transferred to the smelting furnace due to the excessive temperature drop of the launder during the converter, and more energy consumption is required to increase the aluminum liquid temperature. If the remaining aluminum liquid is lower than the circulating liquid level line of the electromagnetic pump in the furnace, the normal operation of the electromagnetic pump will be affected due to the excessive aluminum liquid being transferred out.

[0027] Preferably, as an improvement, in S6, after all the scrap in the smelting furnace is melted, the melt temperature in the smelting furnace is lowered to 720-750°C, and a refining agent of 40-60 kg / hundred tons of melt is added to refine the melt for 20-40 minutes. During refining, the refining tube needs to be inserted to a depth of less than 2 / 3 of the aluminum liquid surface, and the position of the refining point is continuously moved during the refining process.

[0028] Beneficial effect: This scheme facilitates the uniform refining of the melt in the smelting furnace through the above-mentioned settings. The applicant has found through long-term experiments that if the melt temperature is low when the refining agent is added, the melt viscosity will increase, and it will be difficult to remove the melt gas slag through the refining agent; if the melt temperature is high when the refining agent is added, it will cause an increase in the amount of air intake and grain coarsening; if the amount of refining agent added is too small and the refining time is too short, the refining effect is insufficient, reducing the level of melt gas slag removal; if the amount of refining agent added is too large and the refining time is too long, the refining agent itself, as an external pollutant, will increase the slag content level of the melt. At the same time, it should be ensured that the refining tube is inserted to a depth of less than 2 / 3 of the liquid surface. If the refining agent is added to a depth that is too low, the melt near the liquid surface in the furnace cannot be effectively refined; if the refining agent is added to a depth that is too high, the melt near the bottom of the furnace cannot be effectively refined.

[0029] Preferably, as an improvement, in S8, the temperature of the molten aluminum in the smelting furnace is 720-750°C when the molten aluminum is converted into a converter.

[0030] Beneficial effect: This scheme ensures that the aluminum liquid can enter the refining stage in time after being transferred to the holding furnace through the above-mentioned settings. The applicant has found through long-term experiments that if the aluminum liquid temperature is too low in the converter, the temperature of the melt flowing into the holding furnace will be too low due to the excessive temperature drop of the launder, and the gas consumption of the holding furnace needs to be increased to increase the melt temperature. At the same time, the gas slag is difficult to remove due to the increased viscosity of the melt; if the aluminum liquid temperature is too high in the converter, the melt is easy to absorb hydrogen, which reduces the refining effect of the holding furnace and affects the continuity of subsequent production.

[0031] Preferably, as an improvement, in S9, the holding furnace adopts argon refining, the argon flow rate is 200-300L / min, the refining time is 30min-60min, and the standing time is not less than 30min. If the melt is kept in the furnace for more than 4h, it should be re-refined.

[0032] Beneficial effect: This scheme facilitates further refining of the melt and reducing the slag content in the melt through the above-mentioned settings. The applicant has found through long-term experiments that if the argon flow rate is too low, the amount of bubbles generated will be insufficient, which will affect the hydrogen mass transfer and diffusion between the melt and the purification bubbles, and the purification efficiency will be low; if the argon flow rate is too high, it will also increase the degree of melt tumbling, and the slag on the surface of the melt will enter the interior of the melt, causing secondary pollution. If the refining time is less than 30 minutes, the purification effect will be insufficient because the gas slag inside the melt has not completely diffused to the surface of the melt with the bubbles; in order to prevent the slag on the surface of the melt from being brought into the melt again by the movement of the bubbles, the slag diffused to the surface with the bubbles should be cleaned in time, and the refining time should be avoided from being too long from the perspective of saving energy. Because the slag inclusions with small internal size or small specific gravity difference in the melt need a certain amount of time to float or sink, it is difficult to ensure that the slag inclusions are taken out of the melt surface or sink to the bottom of the furnace if the standing time is too short; if the standing time is too long, new slag inclusions are easily generated inside the melt, and re-refining is required, wasting gas consumption and manual slag removal costs.

[0033] Preferably, as an improvement, (iii) the out-of-furnace treatment stage includes the following steps: S10, grain refinement; S11, online degassing; S12, online filtration, and finally completing the casting; in S12, the online filtration adopts a double-deep bed filtration device, and the throughput of the aluminum melt in the small deep bed is 90% or less of the maximum throughput, and the throughput in the large deep bed is 70% or less of the maximum throughput.

[0034] Beneficial effect: This scheme adopts the above scheme to further reduce the slag content in the melt. Specifically, the hydrogen content of the melt is tested in the flow channel between the degassing box and the filter box, and the offline slag measurement method is used to take samples in the flow channel after the double-deep bed filter device, and the slag content is analyzed by metallographic method. The proportion of scrap aluminum added to the tank material of this scheme can reach more than 75%, and the slag content of the melt after flux refining, online degassing, and double-deep bed filtration is ≤0.01mm 2 / kgAl, hydrogen content ≤0.13ml / 100gAl, meeting the quality control requirements of aluminum alloy melt for can material.

[0035] The beneficial effects of this program:

[0036] (1) The present invention adopts a double-chamber furnace to melt scrap aluminum, which can digest more types of small-sized scrap, effectively reduce the burn-out rate when melting small-sized scrap, and avoid the problem that the melting of small-sized scrap easily leads to serious slag formation in the melt;

[0037] (2) The present invention adopts a double-chamber furnace and a smelting furnace to melt different types of waste respectively. The digestible waste includes scraps, thin sheets, scraps, packing blocks, residual rolls, head and tail materials, and recycled ingots. A small amount of oily and water-containing waste can be baked in the double-chamber furnace bridge. After the combustibles and moisture are completely removed, they can be pushed into the furnace for use. The present invention covers almost all types of waste aluminum of all sizes;

[0038] (3) The invention proposes a can body aluminum alloy smelting process with a high proportion of waste material addition, in which the proportion of can body waste material addition can reach more than 75%, which brings good economic benefits to the enterprise and reduces the input cost of raw materials;

[0039] The present invention adopts a combined process of flux refining, online degassing and double-deep bed filtration to purify the aluminum melt of the tank material with a high proportion of waste material addition, which can significantly reduce the hydrogen content and slag content levels of the melt, and ensure that the melt quality under the condition of high waste material addition ratio can also meet the high requirements of the tank material for the melt purity. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a schematic structural diagram of a tank body aluminum alloy smelting system in an embodiment of the present invention.

[0041] Figure 2 It is a top view of the connection between the vortex channel and the inner wall of the vortex well in an embodiment of the present invention.

[0042] Figure 3 The figure is a flow chart of the aluminum alloy smelting process for the tank body material in an embodiment of the present invention. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Unless otherwise specified, the technical means used in the following examples and experimental examples are conventional means well known to those skilled in the art, and the materials, reagents, etc. used can be obtained from commercial sources.

[0044] Description of the drawings: double-chamber furnace 1, heating chamber 11, first furnace door 111, waste chamber 12, second furnace door 121, furnace bridge 122, supplementary heat burner 123, partition wall 13, circulation channel 131, electromagnetic pump 14, first flow channel 2, smelting furnace 3, third furnace door 31, second flow channel 4, insulation furnace 5, fourth furnace door 51, burner 6, plugging drill 7, vortex well 8, vortex channel 81, circulation pump 811, debris inlet 82, aluminum liquid channel 83, third flow channel 9.

[0045] Program Overview

[0046] This solution provides a tank material aluminum alloy smelting system, such as Figure 1 and Figure 2 As shown, it includes a double-chamber furnace 1, a smelting furnace 3 and a holding furnace 5 which are connected by flow channels in sequence. The flow channel between the double-chamber furnace 1 and the smelting furnace 3 is a first flow channel 2, which is convenient for the aluminum liquid in the double-chamber furnace 1 to enter the smelting furnace 3 through the first flow channel 2; the flow channel between the smelting furnace 3 and the holding furnace 5 is a second flow channel 4, which is convenient for the aluminum liquid in the smelting furnace 3 to enter the smelting furnace 3 through the second flow channel 4. Both ends of the first flow channel 2 and the second flow channel 4 are provided with a plugging rod 7 for controlling the aluminum liquid in and out of the double-chamber furnace 1, the smelting furnace 3 and the holding furnace 5.

[0047] A partition wall 13 is provided in the double-chamber furnace 1, which divides the double-chamber furnace 1 into a heating chamber 11 and a waste chamber 12. A circulation channel 131 is provided on the partition wall 13. The circulation channel 131 is located in the middle of the partition wall 13. The height of the circulation channel 131 is higher than the aluminum liquid level in the heating chamber 11 and the waste chamber 12. An electromagnetic pump 14 is provided in the circulation channel 131 to facilitate the circulation of aluminum liquid in the heating chamber 11 and the waste chamber 12.

[0048] The heating chamber 11 is provided with a first furnace door 111 and a high-power burner 6, the waste chamber 12 is provided with a second furnace door 121 and a supplementary heat burner 123, and a furnace bridge 122 is provided in the waste chamber 12. The furnace bridge 122 is arranged close to the second furnace door 121. The area of ​​the furnace bridge 122 is smaller than the cross-sectional area of ​​the waste chamber 12, which is convenient for processing oil-containing, water-containing and film-coated waste aluminum. Specifically, the oil-containing, water-containing and film-coated aluminum waste can be pre-placed on the furnace bridge 122 in the waste chamber 12 for baking, and then pushed into the waste chamber 12 for smelting after the combustibles are completely burned or evaporated, which effectively improves the purity and quality of the aluminum liquid. The first launder 2 is located between the waste chamber 12 and the smelting furnace 3.

[0049] The waste chamber 12 is also connected to the vortex well 8. A vortex channel 81 is provided between the waste chamber 12 and the vortex well 8. The vortex channel 81 is tangent to the inner wall of the vortex well 8. A circulating pump 811 is provided on the vortex channel 81, which is convenient for pumping the high-temperature aluminum liquid in the waste chamber 12 to the vortex well 8 and forming a vortex, thereby realizing efficient mixing and smelting of the aluminum liquid and the scrap aluminum waste in the vortex. A scrap inlet 82 is provided at the top of the vortex well 8, and a conveyor belt (not shown in the figure) is provided outside the vortex well 8. The conveyor belt outlet is directly opposite to the scrap inlet 82 of the vortex well 8, which is convenient for automatic feeding of scrap aluminum waste. An aluminum liquid channel 83 connected to the first flow trough 2 is provided at the bottom of the vortex well 8, which is convenient for the aluminum liquid in the vortex well 8 to enter the smelting furnace 3 through the first flow trough 2.

[0050] The smelting furnace 3 is provided with a third furnace door 31 , the holding furnace 5 is provided with a fourth furnace door 41 and a third flow channel 9 , and a plugging rod 7 is also provided on the end of the third flow channel 9 .

[0051] In the aluminum alloy smelting system for can body materials of this scheme, aluminum alloys for can body materials of different sizes and thicknesses can be smelted in different categories. Specifically, the head and tail cut wastes are put into the heating chamber 11 through the first furnace door 111, and the high-power burner 6 arranged on the heating chamber 11 can melt them into aluminum liquid. The aluminum liquid in the heating chamber 11 is circulated and smelted in the heating chamber 11 and the waste chamber 12 under the action of the electromagnetic pump 14. The packaged waste or block waste is put into the waste chamber 12 through the second furnace door 121, and is heated and melted by the aluminum liquid circulating in the heating chamber 11. If the packaged waste or block waste (including packaged blocks, recycled ingots, and twisted roll aluminum waste) contains oil, water or film, it can be placed on the furnace bridge 122 for baking when feeding, and then pushed into the waste chamber 12 for smelting after the combustibles are completely burned or evaporated, which effectively improves the purity and quality of the aluminum liquid.

[0052] The aluminum liquid in the double-chamber furnace 1 enters the smelting furnace 3 through the first flow channel 2. At this time, the flake or block waste is put into the smelting furnace 3 through the third furnace door 31, mixed with the aluminum liquid entering the smelting furnace 3 through the first flow channel 2, and then enters the holding furnace 5 for refining through the second flow channel 4. In each smelting stage, the first furnace door 111, the second furnace door 121, the third furnace door 31 and the fourth furnace door 51 are used for slag removal, to remove the waste slag generated during the smelting process, improve the smelting quality, and improve the purity and quality of the aluminum liquid.

[0053] The aluminum liquid refined in the holding furnace 5 flows out through the third flow channel 9 after being tested and found to be qualified, and can be directly used for casting aluminum alloy ingots after online purification treatment, or can be mixed with other melts to produce corresponding products as needed.

[0054] This solution also provides a can body aluminum alloy smelting process, such as Figure 3 As shown, the following steps are included:

[0055] (I) In the can body aluminum alloy classification stage, the recycled can body aluminum alloy is classified; the classification method is as follows: Classify the can body aluminum alloy waste types according to the specific treatment of different molten pools:

[0056] (1) Aluminum scraps: Aluminum scraps from the crushing of waste aluminum and milling produced by in-plant machining, with a size less than 5cm2 and a thickness less than 0.1mm, are fed into the vortex well for melting;

[0057] (2) Cutting head and tail waste: Cutting head and tail waste of ingots, the diameter or length of each waste is greater than 100mm and the weight is not less than 10kg, which is fed into the charging chamber of the double-chamber furnace for melting;

[0058] (3) Baled or blocky waste: aluminum waste in the form of baled blocks, recycled ingots, or twisted rolls, with a thickness greater than 0.1 mm, is fed into the waste chamber of a double-chamber furnace for melting;

[0059] (4) Waste in the form of flakes or blocks: recycled ingots, residual rolls without liquid, scraps, thin flakes and baled blocks, some head and tail materials, and aluminum ingots are put into the smelting furnace for melting.

[0060] (ii) The stage of graded feeding and smelting is completed in the graded smelting system, where different types of waste materials are graded and fed into different chambers of the double-chamber furnace and the smelting furnace for smelting. It includes the following steps:

[0061] S1, double-chamber furnace preparation and feeding;

[0062] As a reference, the following steps are included: after feeding the cut head and tail scraps into the heating chamber, start heating; after the scraps in the heating chamber are added from the scrap chamber, start the circulation of aluminum liquid in the heating chamber and the scrap chamber immediately; when the packaged scraps or block scraps contain water, oil and coating, place the feed on the furnace bridge in the heating chamber, use the high temperature of the aluminum liquid to bake until the water and oil evaporate and the coating burns, and then push the feed into the scrap chamber for smelting; the furnace temperature in the heating chamber is 1050-1120°C, and the furnace temperature in the scrap chamber is 750-850°C; in S2, slag removal is carried out when all the raw materials in the double-chamber furnace are melted and the aluminum liquid temperature is ≥720°C.

[0063] S2, double-chamber furnace for stirring, melting and slagging;

[0064] S3, preparing and feeding the smelting furnace;

[0065] As a reference, the order of feeding aluminum scrap into the smelting furnace is as follows: flakes, scraps and baled blocks, residual rolls and heads and tails, recycled ingots and aluminum ingots;

[0066] S4, confirm the composition of aluminum liquid in double-chamber furnace and converter;

[0067] As a reference, after the double-chamber furnace slag removal operation is completed and the aluminum liquid temperature is ≥720℃, the converter is performed after the converter conditions are met. The aluminum liquid temperature in the double-chamber furnace during the converter is 710-740℃. During the converter, part of the aluminum liquid in the double-chamber furnace is directly converted to the melting chamber, and part of the aluminum liquid is pumped tangentially to the vortex well to form a vortex, and aluminum debris is fed into the vortex well, and the aluminum liquid obtained from the mixed smelting is then converted to the melting chamber; the proportion of debris in each furnace of aluminum waste is ≤30%; the remaining aluminum liquid in the double-chamber furnace after the converter is higher than the circulation liquid level line of the electromagnetic pump in the furnace.

[0068] S5, melting and stirring in a smelting furnace;

[0069] As a reference, once the materials are put into the smelting furnace, it can be ignited and melted, and the temperature in the smelting furnace is 950-1100℃.

[0070] S6, refining and slag removal in smelting furnace;

[0071] As a reference, after all the scrap in the smelting furnace is melted, the melt temperature in the smelting furnace is lowered to 720-750°C, and a refining agent of 40-60kg / hundred tons of melt is added to refine the melt for 20-40 minutes. During refining, the refining tube needs to be inserted below 2 / 3 of the aluminum liquid surface, and the position of the refining point should be continuously moved during the refining process.

[0072] S7. Detection and adjustment of aluminum liquid composition in the smelting furnace;

[0073] S8, aluminum liquid converter in smelting furnace;

[0074] As a reference, the temperature of the molten aluminum in the smelting furnace is 720-750℃ when it is converted into a converter.

[0075] S9, refining, standing and slagging in holding furnace;

[0076] As a reference, the holding furnace uses argon refining, the argon flow rate is 200-300L / min, the refining time is not less than 30min, and the standing time is 30-60min.

[0077] (iii) purification treatment stage, including the following steps: S10, grain refinement; S11, online degassing; S12, online filtration, and finally completing casting;

[0078] As a reference, in S12, a double-deep bed filtration device is used for online filtration, and the throughput of the aluminum melt in the small deep bed is 90% or less of the maximum throughput, and the throughput in the large deep bed is 70% or less of the maximum throughput.

[0079] Taking the production of 3104 alloy as an example, the aluminum alloy smelting process of the can body material of this scheme is described in detail. First, the batching engineer prepares waste materials and aluminum ingots according to the production plan and process requirements of 3104 alloy. The waste materials added to the double-chamber furnace include cut heads, cut tails, packing blocks, debris, and residual rolls. Specifically, the heating chamber adds cut heads and cut tails, and the waste chamber adds packing blocks and residual rolls. The packing blocks contain a small amount of waste with oil and water. They need to be piled on the furnace bridge for preheating and baking. After the combustibles are completely burned and the water is completely evaporated, they are pushed into the furnace for melting; small debris is added from the vortex well on the top of the double-chamber furnace directly into the aluminum liquid below the liquid level. The waste materials added to the smelting furnace include thin flakes, residual rolls, and recycled ingots. During the process, while the aluminum liquid in the double-chamber furnace is melting, the smelting furnace prepares and feeds. The batching engineer prepares scrap and aluminum ingots according to the 3104 alloy composition, process requirements, and furnace tonnage, and transfers the aluminum liquid melted in the double-chamber furnace to the smelting furnace after the composition is confirmed. The following specific implementation case will explain in detail the scrap addition and flux purification process for each furnace.

[0080] Example 1

[0081] In this embodiment, since the aluminum liquid in the double-chamber furnace is not completely converted to a converter during each production, there are about 16 tons of aluminum liquid remaining in the furnace. The charging situation in the double-chamber furnace of this furnace is shown in Table 1. While the aluminum liquid in the double-chamber furnace is melting, the smelting furnace is preparing and feeding. The charging situation of the smelting furnace of this furnace is shown in Table 2. According to calculations, in this furnace of aluminum liquid, the proportion of aluminum liquid in the double-chamber furnace converter is 34.6%, the proportion of scrap aluminum added to the smelting furnace is 53.0%, and the proportion of total scrap is 87.6%. The smelting furnace adopts flux refining, the amount of refining agent added is 50kg / hundred tons of melt, the refining time is 30min, and after the refining, slag removal, component analysis and adjustment, and converter are carried out. After the converter is completed, the holding furnace opens the air pressure refining mode, the argon flow rate is set to 260L / min, the refining time is 30min, and the standing time is 45min. The aluminum melt is degassed using a three-rotor degassing device, and the argon flow rate is set to 2.5Nm 3 / h, and the rotor speed is set at 280r / min. The online filtration adopts a double deep bed filtration device, the throughput of aluminum melt in the small deep bed is 600t, and the throughput of aluminum melt in the large deep bed is 1300t. The throughput of both the large and small deep beds is 70% or less of the maximum throughput.

[0082] Table 1 Example 1 Double Chamber Furnace Charging Conditions

[0083]

[0084] Table 2 Example 1 Smelting furnace charging situation

[0085]

[0086] Example 2

[0087] In this embodiment, the charging situation of the double-chamber furnace is basically the same as Table 1. The charging situation of the smelting furnace is shown in Table 3. The ratio of aluminum liquid in the double-chamber furnace of this furnace is 39.2%, the ratio of scrap aluminum added to the smelting furnace is 40.3%, and the total scrap ratio is 79.5%. The smelting furnace adopts flux refining, the amount of refining agent added is 45kg / hundred tons of melt, the refining time is 30min, and slag removal, component analysis and adjustment, and converter are carried out after the refining is completed. After the converter is completed, the holding furnace turns on the air pressure refining mode, the argon flow rate is set to 260L / min, the refining time is 30min, and the standing time is 45min. A three-rotor degassing device is used to degas the aluminum melt, the argon flow rate is set to 2.5Nm3 / h, and the rotor speed is set to 280r / min. The online filtration adopts a double deep bed filtration device. The throughput of the small deep bed aluminum melt is 2000t, and the throughput of the large deep bed aluminum melt is 2700t. The throughput of the large and small deep beds is 70% or less of the maximum throughput.

[0088] Table 3 Smelting furnace charging situation of Example 2

[0089]

[0090] Example 3

[0091] In this embodiment, the charging situation of the double-chamber furnace is basically the same as Table 1. The charging situation of the smelting furnace is shown in Table 4. The ratio of aluminum liquid in the double-chamber furnace of this furnace is 35.6%, the ratio of scrap aluminum added to the smelting furnace is 48.7%, and the total scrap ratio is 84.3%. The smelting furnace adopts flux refining, the amount of refining agent added is 50kg / hundred tons of melt, the refining time is 30min, and slag removal, component analysis and adjustment, and converter are carried out after the refining is completed. After the converter is completed, the holding furnace turns on the air pressure refining mode, the argon flow rate is set to 260L / min, the refining time is 30min, and the standing time is 40min. A three-rotor degassing device is used to degas the aluminum melt, the argon flow rate is set to 2.5Nm3 / h, and the rotor speed is set to 280r / min. The online filtration adopts a double deep bed filtration device. The throughput of the small deep bed aluminum melt is 2800t, and the throughput of the large deep bed aluminum melt is 3600t. The throughput of the large and small deep beds is 70% or less of the maximum throughput.

[0092] Table 4 Smelting furnace charging situation in Example 3

[0093]

[0094]

[0095] Comparative Example 1

[0096] Different from Example 1, this comparative example only uses an ordinary smelting furnace to melt scrap aluminum. The charging conditions are shown in Table 5. The total scrap ratio of this furnace is 70.3%. The scrap types are head-cutting scrap, tail-cutting scrap, thin-sheet scrap, and recycled ingot. The thin-sheet scrap, head-cutting scrap, tail-cutting scrap, and recycled ingot are added to the smelting furnace in the order of thin-sheet scrap, head-cutting scrap, and recycled ingot. There is no small-sized scrap such as residual rolls, packaged blocks, and debris. The smelting furnace, holding furnace, online degassing, and online filtration methods are the same as those in Example 1, wherein the throughput of the small deep bed aluminum melt is 2500t, and the throughput of the large deep bed aluminum melt is 3000t, and the throughput of the large and small deep beds is 70% or less of the maximum throughput.

[0097] Table 5 Charging situation of smelting furnace in comparative example 1

[0098]

[0099] Comparative Example 2

[0100] Different from Example 1, this comparative example only uses an ordinary smelting furnace to melt scrap aluminum. The charging conditions are shown in Table 6. The total scrap ratio of this furnace is 75.3%. The types of scraps are cut heads, cut tail scraps, thin flake scraps, scraps, and recycled ingots. They are added to the smelting furnace in the order of thin flake scraps, cut heads, cut tail scraps, recycled ingots, and aluminum ingots. When the raw materials are melted and the melt temperature reaches above 750°C, the scraps are added from the furnace door. No ultra-thin scraps such as residual rolls and packaged blocks are added to this comparative example. The smelting furnace refining, insulation furnace refining, online degassing, and online filtration methods are the same as those in Example 1, wherein the throughput of the small deep bed aluminum melt is 1600t, and the throughput of the large deep bed aluminum melt is 2200t, and the throughput of the large and small deep beds is 70% or less of the maximum throughput.

[0101] Table 6 Charging situation of smelting furnace in comparative example 2

[0102]

[0103]

[0104] Comparative Example 3

[0105] Different from Example 1, this comparative example only uses an ordinary smelting furnace to melt the scrap aluminum. The charging conditions are shown in Table 7. The total scrap ratio of this furnace is 70.7%. The scrap types are head cutting, tail cutting scrap, flake scrap, debris, and recycled ingots, which are added to the smelting furnace in the order of debris, flake scrap, head cutting, tail cutting scrap, recycled ingot, and aluminum ingot. The smelting furnace refining, insulation furnace refining, online degassing, and online filtration methods are the same as those in Example 1, wherein the throughput of the small deep bed aluminum melt is 2400t, and the throughput of the large deep bed aluminum melt is 2800t, and the throughput of the large and small deep beds is 70% or less of the maximum throughput.

[0106] Table 7 Charging situation of smelting furnace in comparative example 3

[0107]

[0108] Comparative Example 4

[0109] Different from Example 1, the online filtration method of this comparative example adopts double-stage plate filtration. The charging conditions are the same as those of Example 1, the proportion of aluminum liquid after melting the scrap aluminum in the double-chamber furnace is 36.8%, and the proportion of scrap aluminum in the smelting furnace is 42.5%. The refining in the smelting furnace, the refining in the holding furnace, and the online degassing are the same as those in Example 1. The online filtration adopts double-stage plate filtration, the precision of the first-stage filter plate is 30PPI, and the precision of the second-stage filter plate is 50PPI.

[0110] Comparative Example 5

[0111] Different from Example 1, the online filtration method of this comparative example adopts double-stage plate filtration. The charging conditions are the same as those of Example 1, the proportion of aluminum liquid after melting the scrap aluminum in the double-chamber furnace is 39.5%, and the proportion of scrap aluminum in the smelting furnace is 41.2%. The refining in the smelting furnace, the refining in the holding furnace, and the online degassing are the same as those in Example 1. The online filtration adopts double-stage plate filtration, the precision of the first-stage filter plate is 40PPI, and the precision of the second-stage filter plate is 60PPI.

[0112] Experimental Example 1: Performance Testing of Recycled Aluminum Alloy Melt

[0113] The hydrogen content of the melt recovered from smelting in the above-mentioned Examples 1-3 and Comparative Examples 1-5 was tested in the flow channel between the degassing box and the filter box, and the melt recovered from smelting in the above-mentioned Examples 1-3 and Comparative Examples 1-5 was sampled by an offline slag measurement method in the flow channel after the double-deep bed filter device, and the slag content was analyzed by metallographic method. The test results are detailed in Table 8.

[0114] Table 8 Performance test results of the melts recovered from smelting in Examples 1-3 and Comparative Examples 1-5

[0115]

[0116] The results of the melt hydrogen content and slag content of each embodiment are shown in Table 8. As can be seen from Table 8, embodiments 1 to 3 use a double-chamber furnace + a smelting furnace to melt scrap aluminum. The double-chamber furnace consumes different types of scrap aluminum such as cut heads, cut tails, packing blocks, residual rolls, and debris. The smelting furnace consumes scrap aluminum such as cut heads, cut tails, thin sheet waste, and recycled ingots. The total scrap ratio reaches more than 75%, and the final melt hydrogen content is 0.094ml / 100gAl, 0.102ml / 100gAl, and 0.108ml / 100gAl, respectively, and the slag content is 0.008mm 2 / kgAl, 0.006mm 2 / kgAl, 0.007mm 2 / kgAl, which meets the quality control requirements of aluminum alloy melt for can body materials.

[0117] Compared with Examples 1 to 3, Comparative Example 1 only uses a smelting furnace to melt scrap aluminum, and only consumes cut heads, cut tails, thin slices, and recycled ingots, without consuming debris, residual rolls, water-containing, and oily wastes. Although the hydrogen content and slag content of the melt meet the quality control requirements of the tank material melt, the proportion of total waste that can be consumed is only 70.3%, which is lower than the 87.6%, 79.5%, and 84.3% waste amounts that can be consumed in Examples 1 to 3, respectively.

[0118] Compared with Examples 1 to 3, Comparative Example 2 only uses a smelting furnace to melt scrap aluminum. The types of scrap aluminum consumed are similar to those of Examples 1 to 3, including cut heads, cut tails, thin flakes, scraps, and recycled ingots. The scraps are added to the smelting furnace in the order of thin flakes, cut heads, cut tails, recycled ingots, and aluminum ingots. When the raw materials are melted and the melt temperature reaches above 750°C, the scraps are added from the furnace door. The total scrap ratio consumed in Comparative Example 2 is 75.3%, which is lower than the total scrap addition ratio of Examples 1 to 3 (87.6% and 79.5%, respectively), but its final melt hydrogen content and slag content are higher than Examples 1 to 3. This is because Comparative Example 2 melts the scraps in the smelting furnace, and the scrap ratio is relatively high, reaching 16.7%. It is difficult to avoid direct contact with the open flame during melting, and the degree of slag formation of the melt is increased. Although the combined process of flux refining, three-rotor degassing and double deep bed filtration is adopted, the slag content of the melt is 0.015mm 2 / kgAl, which cannot meet the slag content control requirements for high-quality tank materials.

[0119] Compared with Examples 1 to 3, Comparative Example 3 only uses a smelting furnace to melt scrap aluminum. The types of scrap aluminum consumed are similar to those of Examples 1 to 3, including scraps, scraps, flake scraps, scraps, and recycled ingots. However, scraps, flake scraps, scraps, scraps, recycled ingots, and aluminum ingots are added to the smelting furnace in the order of scraps, flake scraps, scraps, scraps, recycled ingots, and aluminum ingots. The total scrap consumed in Comparative Example 2 is 70.7%, and the final melt hydrogen content and slag content are 0.128 ml / 100 gAl and 0.016 mm / 100 gAl, respectively. 2 / kgAl, which is higher than that of Examples 1 to 3. This is because the chips are directly melted into the furnace, the melting rate is very low, the melt slag is serious, and ultimately cannot meet the slag content control requirements of high-quality tank materials.

[0120] Compared with Examples 1 to 3, Comparative Examples 4 and 5 adopt a two-stage plate-type online filtration method. Comparative Example 4 adopts a 30+50PPI filter plate with a filtration accuracy, and the final melt slag content is 0.023mm 2 / kgAl; Comparative Example 5 uses a 40+60PPI filter plate, and the final melt slag content is 0.028mm 2 / kgAl, which are significantly higher than the slag content levels of Examples 1 to 3, and cannot meet the requirement of high-quality tank material for the molten slag content to be less than 0.01mm 2 / kgAl control requirements, indicating that the two-stage plate filtration method cannot effectively control the melt quality of the tank material under the condition of high proportion of waste addition.

[0121] It can be seen that Examples 1 to 3 use a double-chamber furnace + smelting furnace to melt different types and sizes of scrap aluminum according to the characteristics of the furnace. Under the condition that the proportion of scrap aluminum added to the can body material is greater than 75%, the melt purification adopts a combined process of flux refining, online degassing and double deep bed filtration, and the slag content of the melt is less than 0.01 mm2 / kgAl, and the hydrogen content is less than 0.13ml / 100gAl, which meets the quality control requirements of aluminum alloy melt for can body materials. This shows that the aluminum alloy smelting process for can body materials with a high proportion of waste addition can meet the needs of large-scale production.

[0122] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A can body aluminum alloy smelting process, characterized by: The method comprises the following steps: (i) a can body material aluminum alloy classification stage, in which the recycled can body material aluminum alloy is classified; (ii) a graded feeding and smelting stage, in which the following steps are included: S1, double-chamber furnace material preparation and feeding; S2, double-chamber furnace stirring, melting and slag removal; S3, smelting furnace material preparation and feeding; S4, aluminum liquid composition confirmation and converter in the double-chamber furnace; S5, melting and stirring in the smelting furnace; S6, refining and slag removal in the smelting furnace; S7, aluminum liquid composition detection and adjustment in the smelting furnace; S8, aluminum liquid converter in the smelting furnace; S9, refining, standing and slag removal in the holding furnace; and graded feeding of different types of waste obtained by classification into different chambers of the double-chamber furnace and the smelting furnace for smelting; and (iii) an out-of-furnace treatment stage.

2. A can body aluminum alloy smelting process according to claim 1, characterized in that: In the (I) can body aluminum alloy classification stage, the classification method is as follows: Classification is carried out according to the types of can body aluminum alloy scraps processed by different molten pool specificities: (1) Aluminum scraps: Aluminum scraps from the crushing of waste aluminum and milling produced by machining in the factory, with a size less than 5 cm 2 , thickness less than 0.1mm; (2) Cutting head and tail waste: Cutting head and tail waste of ingots, the diameter or length of a single waste is greater than 100mm and the weight is not less than 10kg; (3) Baled or block-shaped waste: aluminum waste in the form of baled blocks, recycled ingots, or twisted rolls, with a thickness greater than 0.1 mm; (4) Waste in the form of flakes or blocks: recycled ingots, residual rolls without liquid, scraps, thin sheets and baled blocks, some heads and tails, and aluminum ingots.

3. A can body aluminum alloy smelting process according to claim 2, characterized in that: (ii) The stage of graded feeding and smelting is completed in a graded smelting system, which includes a double-chamber furnace, a smelting furnace and a holding furnace connected by a flow channel, and plugging rods are provided at both ends of the flow channel to control the inflow and outflow of aluminum liquid in the double-chamber furnace, the smelting furnace and the holding furnace; the double-chamber furnace includes a heating chamber and a waste chamber connected to each other, and the heating chamber, the waste chamber, the smelting furnace and the holding furnace are all provided with furnace doors; the flow channel between the waste chamber and the smelting furnace is the first flow channel, and the flow channel between the smelting furnace and the holding furnace is the second flow channel, and a vortex well is also connected between the waste chamber and the smelting furnace, a debris inlet is provided at the top of the vortex well, and a pipeline at the bottom of the vortex well is connected to the first flow channel.

4. A can body aluminum alloy smelting process according to claim 3, characterized in that: In S1, the following steps are included: feeding the cut head and tail scraps into the heating chamber and then starting the heating; feeding the baled scraps or block scraps into the scrap chamber, and immediately starting the circulation of the aluminum liquid in the heating chamber and the scrap chamber after the scraps are fed into the scrap chamber; when the baled scraps or block scraps contain water or oil, the scraps are first stacked on the furnace bridge in the scrap chamber, and the high temperature of the aluminum liquid is used to bake the scraps until the water and oil evaporate, and then the scraps are pushed into the scrap chamber for smelting; the furnace temperature in the heating chamber is 1050-1120°C, and the furnace temperature in the scrap chamber is 750-850°C; in S2, slag removal is performed when all the raw materials in the double-chamber furnace are melted and the aluminum liquid temperature is ≥720°C.

5. A can body aluminum alloy smelting process according to claim 3, characterized in that: In S3, flake or block waste is fed into the smelting furnace for smelting. The order of feeding aluminum waste into the smelting furnace is as follows: thin flakes, scraps and packaged blocks, residual coils and head and tail materials, recycled ingots and aluminum ingots. In S5, after the feeding is completed, it can be ignited and melted. The furnace temperature in the smelting furnace is 950-1100°C.

6. A can body aluminum alloy smelting process according to claim 3, characterized in that: In S4, in S4, after the double-chamber furnace slag removal operation is completed and the aluminum liquid temperature is ≥720°C, sampling and testing are carried out to meet the converter conditions and then the converter is carried out. During the converter, the aluminum liquid temperature in the double-chamber furnace is 710-740°C. During the converter, part of the aluminum liquid in the double-chamber furnace is directly converted to the smelting chamber, and part of the aluminum liquid is pumped tangentially to the vortex well to form a vortex, and aluminum chips are added to the vortex well, and the aluminum liquid obtained by mixed smelting is then converted to the smelting chamber; the proportion of chips in each furnace of aluminum waste is ≤30%; the remaining aluminum liquid in the double-chamber furnace after the converter is higher than the circulation liquid level line of the electromagnetic pump in the furnace.

7. A can body aluminum alloy smelting process according to claim 3, characterized in that: In S6, after all the scrap in the smelting furnace is melted, the melt temperature in the smelting furnace is lowered to 720-750°C, and a refining agent of 40-60kg / hundred tons of melt is added to refine the melt for 20-40 minutes. During refining, the refining tube needs to be inserted below 2 / 3 of the aluminum liquid surface, and the position of the refining point is continuously moved during the refining process.

8. The aluminum alloy smelting process for can body material according to claim 1, characterized in that: In S8, the temperature of the molten aluminum in the smelting furnace is 720-750°C when the molten aluminum is transferred to the converter.

9. A can body aluminum alloy smelting process according to claim 1, characterized in that: In S9, the holding furnace adopts argon refining, the argon flow rate is 200-300L / min, the refining time is 30min-60min, and the standing time is not less than 30min. If the melt is kept in the furnace for more than 4h, it should be refined again.

10. The aluminum alloy smelting process for can body material according to claim 1, characterized in that: (III) The out-of-furnace treatment stage includes the following steps: S10, grain refinement; S11, online degassing; S12, online filtration, and finally casting. In S12, online filtration adopts a double-deep bed filtration device, and the throughput of the aluminum melt in the small deep bed is 90% or less of the maximum throughput, and the throughput in the large deep bed is 70% or less of the maximum throughput.

Citation Information

Cited By

  • Security recovery method for 7-series aluminum alloy processing aluminum skimmings, regenerated 7-series aluminum alloy cast ingot and application of regenerated 7-series aluminum alloy cast ingot

    CN119320887A