Tungsten particle / Zr-based amorphous composite energetic fragile armor-piercing bullet core, preparation method thereof and application of tungsten particle / Zr-based amorphous composite energetic fragile armor-piercing bullet core in armor-piercing bullet
The tungsten particle/Zr-based amorphous composite energetic fragile armor-piercing projectile core prepared by ball milling and spark plasma sintering solves the problem of uneven tungsten particle distribution, improves the penetration capability and damage effect of the armor-piercing projectile, and reduces costs.
Patent Information
- Application Number
- CN202411081663.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-05
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
AI Technical Summary
Existing preparation methods for tungsten particle-reinforced zirconium-based amorphous alloy composites have defects such as uneven tungsten particle distribution, numerous internal microcracks, and partial crystallization of the BMG matrix, which affect their application in armor-piercing projectiles.
By ball milling spherical tungsten particles and Zr-based amorphous powder together and then combining the mixture with spark plasma sintering, a Zr-based amorphous composite energetic and fragile armor-piercing projectile core with uniformly dispersed tungsten particles was prepared, avoiding stress concentration and achieving good interfacial bonding.
Uniform dispersion of tungsten particles in a Zr-based amorphous matrix was achieved, which improved armor penetration capability and after-effect damage effect, reduced manufacturing cost, and the kinetic energy of the resulting fragments far exceeded 75J, exhibiting strong after-effect damage capability.
Smart Images

Figure CN118957348A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of armor-piercing bullets, and in particular to a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing bullet core, a preparation method thereof, and an application thereof in armor-piercing bullets. Background Art
[0002] Zirconium-based amorphous alloy is a typical metastable material due to its unique microstructure. It can react violently and release energy under high dynamic loads to produce an explosive effect. At the same time, it has excellent physical and chemical properties, such as high hardness, high strength, high elasticity, high fracture toughness, self-sharpening during penetration, and non-toxic and environmentally friendly. It has broad application prospects in the field of armor-piercing energetic fragments. However, during room temperature deformation, zirconium-based amorphous alloys are prone to form highly localized shear bands and catastrophic shear fractures along the shear bands. Therefore, the room temperature plasticity is poor, which seriously limits its application in the field of armor-piercing penetration.
[0003] Tungsten (W) has similar thermal expansion coefficients to zirconium-based amorphous alloys and good wettability, making it an ideal reinforcement phase for Zr-based amorphous composites. The addition of tungsten can not only improve the plasticity and toughness of Zr-based amorphous alloys (Zr-BGMC) and increase the density, but also retain the high strength and shear "self-sharpening" of the amorphous matrix. Therefore, tungsten-reinforced zirconium-based amorphous composites (W / Zr-BGMC) have received widespread attention in armor-piercing materials.
[0004] At present, when tungsten is added to zirconium-based amorphous alloys as a reinforcement phase, its common forms mainly include tungsten powder, tungsten fiber, tungsten rod and tungsten carbide (WC), among which tungsten fiber / BGMC is the most widely studied added phase. Although tungsten particle reinforced BMG-based composites have been studied, the preparation methods used in existing studies are melt infiltration casting or arc melting / copper mold casting. The resulting composites often have defects such as uneven distribution of tungsten particles, many internal microcracks, and partial crystallization of the BMG matrix. Therefore, it is urgent to prepare tungsten particle reinforced zirconium-based energetic fragmentation armor-piercing projectiles with excellent performance through more advanced preparation methods. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core and a preparation method thereof and application in armor-piercing projectiles, so as to overcome the deficiencies in the above-mentioned prior art.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: A method for preparing a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core comprises the following steps:
[0007] S1. Select Zr-based amorphous powder and spherical tungsten particles, weigh the raw materials according to a certain volume fraction, and then mix them by ball milling to obtain a uniform mixture;
[0008] S2. Put the mixture into a mold, pre-press the mixture at a pressure of 39.2KN for 1 minute, and heat the mixture to 678K by spark plasma sintering in a vacuum environment, with a heating rate of 50K / min, keeping warm for 3 minutes, and a sintering pressure of 500MPa. After cooling and demolding, a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing core is obtained.
[0009] Based on the above technical solution, the present invention can also be improved as follows.
[0010] Furthermore, Zr-based amorphous powder is made of Zr 55 Cu 30 Al 10 Ni5 amorphous powder, density 6.85g / cm 3 , particle size ≤53μm.
[0011] Furthermore, the average particle size of the Zr-based amorphous powder is 10 μm to 50 μm.
[0012] Furthermore, the average particle size of the Zr-based amorphous powder is 40 μm.
[0013] Furthermore, the particle size of the spherical tungsten particles is less than or equal to 250 μm and greater than or equal to 30 μm.
[0014] Furthermore, the purity of the spherical tungsten particles is 99.999% and the density is 19.3g / cm 3 .
[0015] Furthermore, the Zr-based amorphous powder and the spherical tungsten particles are weighed so that the volume fraction of the spherical tungsten particles does not exceed 50%.
[0016] Furthermore, the ball milling time is 30 min to 90 min, and the rotation speed is 120 r / min to 200 r / min.
[0017] Based on the above technical solution, the present invention also provides a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core, which is prepared by the above preparation method.
[0018] Based on the above technical solution, the present invention also provides an application of a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing core in an armor-piercing projectile.
[0019] Furthermore, the armor-piercing projectile is an armor-piercing fragmentation projectile or an armor-piercing incendiary projectile.
[0020] The beneficial effects of the present invention are as follows: the reinforcing phase in the present invention selects spherical tungsten particles, and experiments show that the specific surface area of the spherical tungsten particles in contact with the amorphous matrix is the largest, and the volume fraction of the selected spherical tungsten particles does not exceed 50%. At the same time, the skeleton mode is not adopted, but the spherical tungsten particles are mixed with the Zr-based amorphous powder by ball milling. After sintering, the spherical tungsten particles can be evenly dispersed in the Zr-based amorphous matrix to avoid stress concentration, and the interface bonding is good. The spherical tungsten particles are isotropic and can be post-processed according to the required projectile shape without destroying the overall mechanical properties. Therefore, large molds can be used for batch processing to reduce the production cost. When the tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core is used in armor-piercing fragmentation projectiles or armor-piercing incendiary When the incendiary bomb penetrates the target, the tungsten particles can induce more shear bands to be generated and expanded during the armor-piercing process, thereby improving the armor-piercing capability. At the same time, after the armor-piercing is completed, the strength of the Zr-based amorphous matrix drops sharply due to the temperature rise, and it is broken under the action of the unloading wave, and the interface bonding force is reduced, forming many tungsten particle-Zr-based energetic fragments. The tungsten particles penetrate the after-effect target as fragments, and the zirconium-based amorphous matrix releases a large amount of heat, thereby causing greater after-effect damage to the target and igniting the after-effect target. Experiments show that at a penetration speed of 1200m / S, there is a large hole expansion ratio, which can reach 35-67, and the kinetic energy of the fragments formed far exceeds 75J, with a strong after-effect damage capability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a sintering process diagram of the present invention;
[0022] Figure 2 The structure diagram of the sample obtained in the present invention;
[0023] Figure 3 The scanning electron microscope images of the tungsten particle / Zr-based amorphous composite material of three spherical tungsten particles of different sizes in Examples 1, 2, and 3, in which a represents 30 μm, b represents 75 μm, and c represents 250 μm;
[0024] Figure 4 X-ray diffraction spectra of the tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core of three different sizes of spherical tungsten particles in Examples 1, 2, and 3 and the Zr-based amorphous powder without adding spherical tungsten particles;
[0025] Figure 5 This is the overall morphology of the target plate after the armor-piercing projectile core penetrates;
[0026] Figure 6 The cross-sectional morphology of the target plate after penetration by different projectiles are amorphous-858.4m / s, 30μm-882.4m / s, 75μm-875.6m / s, and 250μm-887.2m / s respectively;
[0027] Figure 7 This is the result diagram of the post-target high-energy test;
[0028] Figure 8 This is the result of the target fragmentation test. DETAILED DESCRIPTION
[0029] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0030] Example 1
[0031] A method for preparing a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core comprises the following steps:
[0032] S1. Select Zr-based amorphous powder, whose nominal chemical composition is Zr 55 Cu 30 Al 10 Ni5 (at.%), density 6.85 g / cm 3 The average particle size is 40μm, and the spherical tungsten particles with an average particle size of 30μm are selected, with a purity of 99.999% and a density of 19.3g / cm 3 In view of the need to meet the high density of the armor-piercing core and ensure the density of the material, the raw materials are weighed according to the volume fraction of spherical tungsten particles not exceeding 50%. The raw materials can be weighed by a high-precision balance, and then mixed by ball milling to obtain a uniformly mixed mixture. The ball milling time is 60 minutes and the rotation speed is 120r / min.
[0033] S2. Put the mixture into the alloy mold, pre-press the mixture with a pressure of 39.2KN for 1 minute, and heat the mixture to 678K by spark plasma sintering in a vacuum environment, with a heating rate of 50K / min, holding for 3 minutes, and a sintering pressure of 500MPa. The spark plasma sintering method uses the discharge effect of electric current to quickly sinter the spherical tungsten particles and the Zr-based amorphous powder in a short time, so that the material sintering speed is fast and the material microstructure can be maintained. The specific process is as follows: Figure 1 As shown, after cooling and demolding, a tungsten particle / Zr-based amorphous composite energetic and breakable armor-piercing projectile core is obtained. After sintering, the matrix of the tungsten particle / Zr-based amorphous composite energetic and breakable armor-piercing projectile core is an amorphous phase, the tungsten particles are evenly dispersed in the matrix, and the interface bonding is good.
[0034] Example 2
[0035] A method for preparing a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core comprises the following steps:
[0036] S1. Select Zr-based amorphous powder, whose nominal chemical composition is Zr 55 Cu 30Al 10 Ni5 (at.%), density 6.85 g / cm 3 The average particle size is 40μm, and the spherical tungsten particles with an average particle size of 75μm are selected, with a purity of 99.999% and a density of 19.3g / cm 3 In view of the need to meet the high density of the armor-piercing core and ensure the density of the material, the raw materials are weighed according to the volume fraction of spherical tungsten particles not exceeding 50%. The raw materials can be weighed by a high-precision balance, and then mixed by ball milling to obtain a uniformly mixed mixture. The ball milling time is 60 minutes and the rotation speed is 120r / min.
[0037] S2. Put the mixture into an alloy mold, pre-press the mixture at a pressure of 39.2KN for 1 minute, and heat the mixture to 678K by spark plasma sintering in a vacuum environment, with a heating rate of 50K / min, insulation for 3 minutes, and a sintering pressure of 500MPa. The spark plasma sintering method uses the discharge effect of electric current to quickly sinter the spherical tungsten particles and the Zr-based amorphous powder in a short time, so that the material sintering speed is fast and the material microstructure can be maintained. After cooling and demolding, a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core is obtained.
[0038] Example 3
[0039] A method for preparing a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core comprises the following steps:
[0040] S1. Select Zr-based amorphous powder, whose nominal chemical composition is Zr 55 Cu 30 Al 10 Ni5 (at.%), density 6.85 g / cm 3 The average particle size is 40μm, and the spherical tungsten particles with an average particle size of 250μm are selected, with a purity of 99.999% and a density of 19.3g / cm 3 In view of the need to meet the high density of the armor-piercing core and ensure the density of the material, the raw materials are weighed according to the volume fraction of spherical tungsten particles not exceeding 50%. The raw materials can be weighed by a high-precision balance, and then mixed by ball milling to obtain a uniformly mixed mixture. The ball milling time is 60 minutes and the rotation speed is 120r / min.
[0041] S2. Put the mixture into an alloy mold, pre-press the mixture at a pressure of 39.2KN for 1 minute, and heat the mixture to 678K by spark plasma sintering in a vacuum environment, with a heating rate of 50K / min, insulation for 3 minutes, and a sintering pressure of 500MPa. The spark plasma sintering method uses the discharge effect of electric current to quickly sinter the spherical tungsten particles and the Zr-based amorphous powder in a short time, so that the material sintering speed is fast and the material microstructure can be maintained. After cooling and demolding, a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core is obtained.
[0042] The tungsten particle / Zr-based amorphous composite energetic brittle armor-piercing projectile core obtained in Examples 1, 2, and 3 is in a columnar shape, such as a cylindrical shape. The prepared sample can be processed by a wire cutting system, such as a cylindrical sample with a diameter of 10 mm. Figure 2 As shown, the prepared sample is cut and thinned, and the surface is polished with sandpaper to meet the needs of subsequent test samples. The sample is used as an energetic fragile armor-piercing core in armor-piercing fragmentation bombs or armor-piercing incendiary bombs.
[0043] The scanning electron microscope (SEM) images of the tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile cores of three different sizes of spherical tungsten particles in Examples 1, 2, and 3 are as follows: Figure 3 As shown, the circular light gray area is the tungsten particles, and the dark gray area is the Zr-based amorphous alloy matrix.
[0044] Figure 4 Figure 3 is the X-ray diffraction spectrum of tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core with three different sizes of spherical tungsten particles and Zr-based amorphous powder without adding spherical tungsten particles. It can be seen from the figure that the phase composition of the amorphous composite energetic breakable armor-piercing projectile core with three different spherical tungsten particle sizes is similar. Except for the characteristic peak of tungsten particles and the diffuse scattering peak (2θ=38°) of the Zr-based amorphous alloy matrix, no other crystal phase peaks appear, and the matrix is completely amorphous. Therefore, the tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core with three different sizes of spherical tungsten particles did not crystallize the amorphous alloy matrix during the sintering process.
[0045] When the tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing core is used in an armor-piercing fragmentation projectile, the overall morphology of the target plate after the armor-piercing fragmentation projectile penetrates is as follows: Figure 5 and Figure 6 As shown, Figure 7 This is the result diagram of the post-target high-energy test. Figure 8 This is the result of the target fragmentation test.
[0046] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing projectile core, characterized in that: The steps include: S1. Select Zr-based amorphous powder and spherical tungsten particles, weigh the raw materials according to a certain volume fraction, and then mix them by ball milling to obtain a uniform mixture; S2. Put the mixture into a mold, pre-press the mixture at a pressure of 39.2KN for 1 minute, and heat the mixture to 678K by spark plasma sintering in a vacuum environment, with a heating rate of 50K / min, keeping warm for 3 minutes, and a sintering pressure of 500MPa. After cooling and demolding, a tungsten particle / Zr-based amorphous composite energetic and fragile armor-piercing core is obtained.
2. The method for preparing a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core according to claim 1, characterized in that: The Zr-based amorphous powder is made of Zr 55 Cu 30 Al 10 Ni5 amorphous powder, density 6.85g / cm 3 , particle size ≤53μm.
3. The method for preparing a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core according to claim 1 or 2, characterized in that: The average particle size of the Zr-based amorphous powder is 10 μm to 50 μm.
4. The method for preparing a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core according to claim 1, 2 or 3, characterized in that: The particle size of the spherical tungsten particles is less than or equal to 250 μm and greater than or equal to 30 μm.
5. The method for preparing a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core according to claim 1, characterized in that: The purity of the spherical tungsten particles is 99.999% and the density is 19.3 g / cm 3 .
6. A method for preparing a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core according to any one of claims 1 to 5, characterized in that: The Zr-based amorphous powder and the spherical tungsten particles are weighed so that the volume fraction of the spherical tungsten particles does not exceed 50%.
7. A method for preparing a tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing projectile core according to any one of claims 1 to 5, characterized in that: The ball milling time is 30min~90min, and the rotation speed is 120r / min~200r / min.
8. A tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing core, characterized in that: The method is as described in any one of claims 1 to 7.
9. Use of the tungsten particle / Zr-based amorphous composite energetic breakable armor-piercing core as claimed in claim 8 in armor-piercing bullets.
10. The use according to claim 9, characterized in that: The armor-piercing projectile is an armor-piercing fragmentation projectile or an armor-piercing incendiary projectile.
Citation Information
Cited By
Energy-containing composite connecting piece based on hard alloy and tungsten-containing amorphous alloy and preparation method and application of energy-containing composite connecting piece
CN119737826A