Method for controlling Ti-containing inclusions of seamless stainless steel pipe

Through technical means such as magnesium spray powder desulfurization, top-bottom composite blowing and furnace exterior alloying, combined with specific slag system and argon blowing treatment, the problem of low control efficiency of Ti inclusions in steel is solved, and high-quality seamless stainless steel is achieved The production of pipes improves the yield rate and product competitiveness.

CN118957409APending Publication Date: 2024-11-15NANJING WORLD SPECIAL STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411033870.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art has problems such as low efficiency, complex equipment or easy to cause secondary pollution in the distribution and removal of Ti inclusions in steel, making it difficult to meet the production needs of high-quality seamless stainless steel pipes.

Method used

Using the combined process of magnesium spray powder desulfurization, top-bottom composite blowing, furnace alloying, vacuum treatment and specific slag system, the blast furnace molten iron content, the converter end point C content and alkalinity are controlled, combined with CaC2, special silicide slag and The use of FeMn alloy is carried out through argon blowing and vacuum treatment, forming white slag and adjusting the composition to ensure effective control of Ti inclusions.

Benefits of technology

It significantly improves the material yield and product quality of seamless stainless steel pipes, enhances the competitiveness of products, realizes effective control of Ti inclusions, and avoids secondary pollution of molten steel.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for controlling Ti-containing inclusions of a seamless stainless steel pipe, which comprises the following steps of: selecting less than or equal to 0.03 percent by weight of Ti in blast furnace molten iron, adopting a magnesium powder spraying desulfurization process, controlling less than or equal to 0.005 percent by weight of S in outbound molten iron, and removing desulfurized slag in a tank; during converter smelting, top-bottom combined blowing is adopted, a high-drawing reblowing process is adopted at the end point, the weight percentage content of converter end point C is controlled to be 0.10-0.20%, and the tapping temperature is 1650 DEG C; in the refining process, argon blowing is conducted in the whole process, CaC2 and special silicification slag are added, white slag is formed, and then FeMn alloy is added for component adjustment; the temperature of a soaking section is 1100-1150 DEG C, the head and tail temperature difference is smaller than 50 DEG C, and the heating time is 250 min; during hot continuous rolling, the rolling starting temperature is 1050-1070 DEG C, and the temperature of a finish rolling inlet is 850-900 DEG C; the inlet temperature of the reducing sizing mill is 910-920 DEG C; the spinning temperature is 910-920 DEG C, and the spinning speed is 85 m / s.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of a method for controlling Ti inclusions in a seamless stainless steel pipe. Background Art

[0002] The number, size and distribution of inclusions in steel have a great influence on the quality of steel products. Therefore, controlling non-metallic inclusions in steel is the key to smelting high-quality clean steel and improving product quality. Starting from the properties and sources of non-metallic inclusions in steel, the collision, aggregation growth, floating and removal mechanisms of inclusions are analyzed. At the same time, a comparative analysis of inclusion control technologies such as bubble adsorption, electromagnetic purification, and filtration separation is conducted, and the development status of oxide metallurgical technology is introduced. Studies have shown that the bubble method and filtration method use bubbles and filters as media to adsorb, capture and promote inclusions in molten steel into the slag phase; the electromagnetic purification method uses the centrifugal force of the electromagnetic field to increase the probability of inclusion collision and aggregation growth, but the equipment is relatively complex and its application is limited by the supply of power resources; the inclusion modification technology is to transform high-melting-point inclusions into low-melting-point inclusions to promote the floating of inclusions. Its operation is simple, but it is easy to cause secondary pollution of molten steel. Oxide metallurgy technology pins and inhibits the growth of austenite grains at high temperatures by changing the size, shape and distribution of inclusions, avoiding the formation of coarse grains, thereby achieving the purpose of refining the structure and improving the strength and toughness of steel. Oxide metallurgy technology provides a new idea for the control of inclusions and has important application prospects. Summary of the invention

[0003] The invention provides a method for controlling Ti inclusions in a seamless stainless steel pipe.

[0004] A method for controlling Ti inclusions in a seamless stainless steel pipe comprises the following steps: Hot metal desulfurization: select blast furnace hot metal with a weight percentage content of Ti≤0.03%, adopt magnesium powder spraying desulfurization process, control the weight percentage content of sulfur in the hot metal out of the station S≤0.005%, and clean the desulfurization slag in the tank; Converter smelting adopts top-bottom composite blowing, the end point adopts high-drawing supplementary blowing process, the converter end point C is controlled to have a weight percentage content of 0.10-0.20%, and the tapping temperature is 1650℃; slag blocking tapping, the ladle slag layer thickness is ≤70mm; Refining, blowing argon throughout the process, adding CaC2 and special silicified slag to form white slag, and then adding FeMn alloy to adjust the composition; using CaO-SiO2-Al2O3 slag system, the basicity is between 1.9-2.2, and Al2O3 is controlled at <13%; hanging to VD furnace for vacuum treatment, keep below 65MPa for 10-15min, add quartz sand after the end to reduce the basicity to 1.0-1.1, and then soft blowing argon for 30min; For heating of the billet, the process control requires that the temperature of the soaking section is 1100-1150°C, the temperature difference between the head and the tail is less than 50°C, and the heating time is 250min; during the hot rolling, the starting rolling temperature is 1050-1070°C, the finishing rolling inlet temperature is 850-900°C; the reducing and sizing mill inlet temperature is 910-920°C; the spinning temperature is 910-920°C, and the spinning speed is 85m / s.

[0005] Preferably, during converter smelting, alloying treatment is performed outside the furnace, and ferrosilicon manganese, silicon carbide and carburizer are added with the steel flow; 4.5-5kg lime and 0.8-0.85kg fluorite are added per ton of steel, and new slag is added with the steel flow during the steel tapping process; the argon pressure of the argon station is 0.5MPa, and the argon flow rate is 10Nm 3 / min, measure temperature, take steel and slag samples, and blow argon for 5 minutes.

[0006] Compared with the prior art, the method has a good control effect on Ti inclusions in seamless stainless steel pipes, increases the yield rate, and enhances the competitiveness of products. DETAILED DESCRIPTION

[0007] The production method for controlling titanium inclusions in fine-gauge high-end cord steel of the present invention is further described in detail below in conjunction with specific embodiments. Example

[0008] A method for controlling Ti inclusions in a seamless stainless steel pipe comprises the following steps: The Ti weight percentage of blast furnace molten iron is controlled at 0.03%. For molten iron desulfurization, the magnesium powder spraying desulfurization process is adopted. The sulfur weight percentage of the molten iron outgoing is controlled at 0.004%. The desulfurization slag in the tank must be cleaned. The converter adopts top-bottom composite blowing, and the end point adopts high-drawing supplementary blowing process. The C weight percentage control target of the converter end point is 0.10%, and the steel tapping temperature is 1650℃; slag blocking steel tapping, the thickness of the ladle slag layer is 40mm; alloying outside the furnace is adopted, and when about 1 / 4 of the steel is tapped, silicon manganese iron, silicon carbide and carburizer are added with the steel flow; when the molten steel is tapped to 3 / 4, all alloys must be added, and C, Si, and Mn are controlled at the lower limit of the internal control range; 4.8kg lime and 0.8kg fluorite per ton of steel are added with the steel flow to make new slag during the steel tapping process; the argon pressure of the argon station is 0.5MPa, and the flow rate is 10Nm 3 / min, measure the temperature, take steel and slag samples, blow argon for 3 minutes, and then lift them to the LF furnace; blow argon throughout the process, add CaC2 and special silicified slag to form white slag, and then add FeMn alloy to adjust the composition; use CaO-SiO2-Al2O3 slag system, the basicity is between 1.8, and Al2O3 is controlled at 13%.

[0009] It was hoisted to the VD furnace for vacuum treatment and maintained below 65MPa for 10min. After that, quartz sand was added to reduce the basicity to 1.0. Argon was then soft-blown for 30min and continuous cast into 160*160mm 2 Billet; Rolling process: The billet heating process control requires the temperature of the soaking section: 1100℃, the temperature difference between the head and the tail is less than 50℃, the heating time is 250min, the rolling temperature is 1050℃, and the finishing entrance temperature is 850℃. The entrance temperature of the sizing mill is 910℃. The wire laying temperature is 910℃, and the wire laying speed is 90m / s. The Stelmor controlled cooling line roller speed is 85m / s; the opening volume of the 3, 6, 7, and 8# fans is controlled to be 85% of the rated air volume, the opening volume of the 9 and 10# fans is controlled to be 80% of the rated air volume, and the opening volume of the remaining 1, 2, 4, and 5# fans is controlled to be 100% of the rated air volume; the insulation cover is fully opened. Example

[0010] A method for controlling Ti inclusions in a seamless stainless steel pipe comprises the following steps: The Ti weight percentage of blast furnace molten iron is controlled at 0.023%. For molten iron desulfurization, the magnesium powder spraying desulfurization process is adopted. The sulfur weight percentage of the molten iron outgoing is controlled at 0.003%. The desulfurization slag in the tank must be cleaned. The converter adopts top-bottom composite blowing, and the end point adopts high-drawing supplementary blowing process. The C weight percentage control target of the converter end point is 0.18%, and the steel tapping temperature is 1650℃; slag blocking steel tapping, the thickness of the ladle slag layer is 62mm; alloying outside the furnace is adopted, and when about 1 / 4 of the steel is tapped, silicon manganese iron, silicon carbide and carburizer are added with the steel flow; when the molten steel is tapped to 3 / 4, all alloys must be added, and C, Si, and Mn are controlled at the lower limit of the internal control range; 4.8kg lime and 0.82kg fluorite per ton of steel are added with the steel flow to make new slag during the steel tapping process; the argon pressure of the argon station is 0.5MPa, and the flow rate is 10Nm 3 / min, measure the temperature, take steel and slag samples, blow argon for 5 minutes, and then lift to the LF furnace. Blow argon throughout the process, add CaC2 and special silicide slag to form white slag, and then add FeMn alloy to adjust the composition; use CaO-SiO2-Al2O3 slag system, the basicity is between 2.2, and Al2O3 is controlled at 10%.

[0011] It was hoisted to the VD furnace for vacuum treatment and maintained below 65MPa for 12 minutes. After that, quartz sand was added to reduce the basicity to 1.05. Argon was then blown softly for 30 minutes and the continuous casting was completed into 160*160mm 2 Billet.

[0012] Rolling process: The billet heating process control requirements are as follows: the temperature of the soaking section is 1120℃, the temperature difference between the head and the tail is less than 50℃, the heating time is 250min, the rolling temperature is 1058℃, and the finishing entrance temperature is 865℃. The entrance temperature of the sizing mill is 913℃. The wire laying temperature is 913℃, and the wire laying speed is 85m / s. The Stelmor controlled cooling line roller speed is 55m / s. The opening volume of the 3, 6, 7, and 8# fans is controlled to be 85% of the rated air volume, the opening volume of the 9 and 10# fans is controlled to be 80% of the rated air volume, and the opening volume of the remaining 1, 2, 4, and 5# fans is controlled to be 100% of the rated air volume. The insulation cover is fully opened. Example

[0013] A method for controlling Ti inclusions in a seamless stainless steel pipe comprises the following steps: The Ti weight percentage of blast furnace molten iron is controlled at 0.016%. For molten iron desulfurization, the magnesium powder spraying desulfurization process is adopted. The sulfur weight percentage of the molten iron outgoing is controlled at 0.0047%. The desulfurization slag in the tank must be cleaned. The converter adopts top-bottom composite blowing, and the end point adopts high-pulling supplementary blowing process. The C control target of the converter end point is 0.2%, and the steel-making temperature is 1650℃; slag blocking steel-making, the thickness of the ladle slag layer is 40mm; alloying outside the furnace is adopted, and when about 1 / 4 of the steel is tapped, silicon manganese iron, silicon carbide and carburizer are added with the steel flow; when the molten steel is tapped to 3 / 4, all alloys must be added, and C, Si, and Mn are controlled at the lower limit of the internal control range; 5kg of lime and 0.85kg of fluorite per ton of steel are added with the steel flow to make new slag during the steel-making process; the argon pressure of the argon station is 0.5MPa, and the flow rate is 10Nm 3 / min, measure the temperature, take steel and slag samples, blow argon for 5 minutes, and then hoist to LF furnace. Blow argon throughout the process, add CaC2 and special silicide slag to form white slag, and then add FeMn alloy to adjust the composition; use CaO-SiO2-Al2O3 slag system, the basicity is between 2.23, and Al2O3 is controlled at 12.3%. Hoist to VD furnace for vacuum treatment, keep below 65MPa for 11 minutes, add quartz sand after the end, reduce the basicity to 11.1, and then blow argon for 30 minutes, and continuously cast into 160*160mm 2 Billet.

[0014] Rolling process: The billet heating process control requires the temperature of the soaking section: 1120℃, the temperature difference between the head and the tail is less than 50℃, the heating time is 250min, the rolling temperature is 1060℃, and the finishing entrance temperature is 887℃. The entrance temperature of the sizing mill is 920℃. The wire laying temperature is 920℃, and the wire laying speed is 85m / s. The Stelmor controlled cooling line roller speed is 67m / s. The opening volume of the 3, 6, 7, and 8# fans is controlled to be 85% of the rated air volume, the opening volume of the 9 and 10# fans is controlled to be 80% of the rated air volume, and the opening volume of the remaining 1, 2, 4, and 5# fans is controlled to be 100% of the rated air volume, and the insulation cover is fully opened. Example

[0015] A method for controlling Ti inclusions in a seamless stainless steel pipe comprises the following steps: The Ti weight percentage of blast furnace molten iron is controlled to 0.01%. For molten iron desulfurization, magnesium powder spraying desulfurization process is adopted. The sulfur weight percentage of molten iron outgoing is controlled to 0.005%. The desulfurization slag in the tank must be cleaned. The converter adopts top-bottom composite blowing, and the end point adopts high-drawing supplementary blowing process. The C weight percentage control target of the converter end point is 0.2%, and the steel tapping temperature is 1650℃; The slag layer thickness of the ladle is 43mm. The steel is alloyed outside the furnace. When about 1 / 4 of the steel is discharged, ferrosilicon manganese, silicon carbide and carburizer are added with the steel flow. When the molten steel is discharged to 3 / 4, all the alloys must be added, and C, Si and Mn are controlled at the lower limit of the internal control range. 5kg lime and 0.85kg fluorite per ton of steel are added with the steel flow to make new slag during the steel discharge process. The argon pressure of the argon station is 0.5MPa, and the flow rate is 10Nm 3 / min, measure temperature, take steel and slag samples, blow argon for 5 minutes, and then hoist to LF furnace. Blow argon throughout the process, add CaC2 and special silicide slag to form white slag, and then add FeMn alloy to adjust the composition; use CaO-SiO2-Al2O3 slag system, the basicity is between 1.83, and Al2O3 is controlled at 11%. Hoist to VD furnace for vacuum treatment, keep below 65MPa for 15 minutes, add quartz sand after the end, reduce the basicity to 1.1, and then blow argon for 30 minutes, and continuously cast into 160*160mm 2 Billet.

[0016] Rolling process: The billet heating process control requires the temperature of the soaking section: 1150℃, the temperature difference between the head and the tail is less than 50℃, the heating time is 250min, the rolling temperature is 1070℃, and the finishing entrance temperature is 900℃. The entrance temperature of the sizing mill is 920℃. The wire laying temperature is 920℃, and the wire laying speed is 85m / s. The Stelmor controlled cooling line roller speed is 74m / s. The opening volume of the 3, 6, 7, and 8# fans is controlled to be 85% of the rated air volume, the opening volume of the 9 and 10# fans is controlled to be 80% of the rated air volume, and the opening volume of the remaining 1, 2, 4, and 5# fans is controlled to be 100% of the rated air volume, and the insulation cover is fully opened.

Claims

1. A method for controlling Ti inclusions in seamless stainless steel pipes, characterized in that The steps include: Hot metal desulfurization: select blast furnace hot metal with a weight percentage content of Ti≤0.03%, adopt magnesium powder spraying desulfurization process, control the weight percentage content of sulfur in the hot metal out of the station S≤0.005%, and clean the desulfurization slag in the tank; Converter smelting adopts top-bottom composite blowing, the end point adopts high-drawing supplementary blowing process, the converter end point C is controlled to have a weight percentage content of 0.10-0.20%, and the tapping temperature is 1650℃; slag blocking tapping, the ladle slag layer thickness is ≤70mm; Refining, blowing argon throughout the process, adding CaC2 and special silicified slag to form white slag, and then adding FeMn alloy to adjust the composition; using CaO-SiO2-Al2O3 slag system, the basicity is between 1.9-2.2, and Al2O3 is controlled at <13%; hanging to VD furnace for vacuum treatment, keep below 65MPa for 10-15min, add quartz sand after the end to reduce the basicity to 1.0-1.1, and then soft blowing argon for 30min; For heating of the square billet, the process control requires that the temperature of the soaking section is 1100-1150°C, the temperature difference between the head and the tail is less than 50°C, and the heating time is 250min; during the hot rolling, the starting rolling temperature is 1050-1070°C, the finishing rolling inlet temperature is 850-900°C; the inlet temperature of the sizing mill is 910-920°C; the spinning temperature is 910-920°C, and the spinning speed is 85m / s.

2. The method for controlling Ti inclusions in seamless stainless steel pipe according to claim 1, characterized in that: During the converter smelting, alloying treatment is performed outside the furnace, and ferrosilicon manganese, silicon carbide and carburizer are added with the steel flow; 4.5-5kg lime and 0.8-0.85kg fluorite are added to a ton of steel, and new slag is added with the steel flow during the steel tapping process; the argon pressure of the argon station is 0.5MPa, and the argon flow rate is 10Nm 3 / min, measure temperature, take steel and slag samples, and blow argon for 5 minutes.