500MPa-grade low-yield-ratio hot-rolled weathering-resistant steel strip and preparation method thereof

By optimizing the chemical composition and process of weathering steel, the microstructure of ferrite and granular bainite is formed, which solves the problem that 500MPa-grade hot-rolled weathering steel in the prior art is difficult to achieve low yield and strength ratio, and achieves high strength and low strength It has a high strength ratio and good weather resistance, and is suitable for construction and bridges and other fields.

CN118957445APending Publication Date: 2024-11-15HANDAN IRON & STEEL GROUP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410964680.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing 500MPa-grade hot-rolled weathering steel is difficult to achieve low yield-strength ratio design and manufacturing under the premise of meeting mechanical properties and weathering properties. The excessive Cr content leads to increased smelting and rolling difficulties, and cracking is prone to cold processing.

Method used

Chemical components C: 0.06-0.08, Si: 0.20-0.40, Mn: 0.80-1.30, P: ≤0.020, S: ≤0.005, Als: 0.020-0.030, Nb: 0.010-0.020, Cu: 0.25-0.35, Cr : 0.50-0.90, Ni: 0.12-0.20, alloy element combination relationship 40≤[Cr]/[Nb]≤50 and 5.5≤3[Mn]+4[Cr]≤6.0, through high final rolling, laminar flow cooling and The winding process forms room temperature structure as ferrite and granular bainite, and controls the microstructure to achieve a balance between strength and yield strength ratio.

Benefits of technology

The yield strength is 511~542MPa, tensile strength is 644~677MPa, the yield strength ratio is ≤0.80, the elongation after breaking ≥18%, and the impact work of longitudinal V-shaped notched KV2≥200J in -20℃, and the corrosion rate relative to Q355B is reduced. ≤57%, low alloy cost, easy to control production process, suitable for steel structure construction such as building bridges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957445A_ABST
    Figure CN118957445A_ABST
Patent Text Reader

Abstract

The invention discloses a 500MPa-grade low-yield-ratio hot-rolled weathering-resistant steel strip and a preparation method thereof. The weathering-resistant steel strip comprises the following chemical components: 0.06 to 0.08 percent of C, 0.20 to 0.40 percent of Si, 0.80 to 1.30 percent of Mn, less than or equal to 0.020 percent of P, less than or equal to 0.005 percent of S, 0.020 to 0.030 percent of Als, 0.010 to 0.020 percent of Nb, 0.25 to 0.35 percent of Cu, 0.50 to 0.90 percent of Cr, 0.12 to 0.20 percent of Ni and the balance of Fe and inevitable impurities. The chemical components also satisfy 40 < = [Cr] / [Nb] < = 50, 5.5 < = 3 [Mn] + 4 [Cr] < = 6.0; the preparation method comprises the working procedures of slab heating, hot rolling, laminar cooling and coiling. The yield strength of the weathering resistant steel strip is 511-542 MPa, the tensile strength is 644-677 MPa, and the yield ratio is smaller than or equal to 0.80.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of weathering steel design and manufacturing, and specifically relates to a 500MPa-grade low-yield ratio hot-rolled weathering steel strip and a preparation method thereof. Technical Background

[0002] Weathering steel is widely used in steel structure construction fields such as building bridges, power towers, and railway trucks due to its excellent weather resistance, cost controllability, and easy production and processing. Although the addition of weather-resistant elements Cu, Cr, and Ni results in a slightly higher direct cost than traditional structural steel, weathering steel has a long service life, low maintenance costs, and paint-free use, which indirectly reduces costs. It is suitable for areas that cannot be repaired or are at risk in the future. Considering that the service environment of weathering steel is plateau cliffs, with high altitudes, large spans, and complex natural conditions, higher requirements are placed on the yield strength ratio of weathering steel to ensure safety.

[0003] The invention patent with authorization announcement number CN113201685B discloses an economical low yield ratio hot-rolled weathering steel plate and its manufacturing method. It uses 0.30-0.50% Cr and 0.20-0.60% Mn content, combined with high final rolling and high coiling (680-730°C) processes to obtain ferrite and pearlite structures at room temperature. Although the yield ratio is relatively low, the strength is only at the 345MPa level, which does not have a high strength.

[0004] The invention patent with authorization announcement number CN107460413B discloses a preparation method and application of 550MPa grade ultrafine grain high-strength weathering steel. It utilizes Ti fine grain strengthening and combines high temperature coiling or controlled rolling and then cooling process to regulate Ti precipitation strengthening. The yield strength can reach more than 500MPa, but the yield strength is relatively high and cannot meet the safety design of the structure.

[0005] The invention patent with publication number CN111945065A, "A 500MPa grade high chromium weathering steel, its preparation method and application", and the invention patent CN116288050A, "A weathering steel and its preparation method", respectively use 2.90-3.70% and 1.6-3.0% Cr composition designs, which greatly improve the weather resistance and reduce the yield strength ratio of steel. However, the high Cr content brings difficulties to smelting and rolling, and cold processing is prone to cracking.

[0006] In order to obtain 500MPa-level strength, in addition to adding weathering elements Cu, Cr, and Ni, microalloying elements such as Nb and Ti are usually added to weathering steel, and the strength and toughness of steel are effectively improved by using the fine grain strengthening and precipitation strengthening effects of Nb and Ti; however, grain refinement is not conducive to the control of low yield ratio, and micron-level Ti (C, N) deteriorates plastic toughness; and after adjusting the process to obtain ferrite and pearlite structures, although the yield ratio is significantly reduced, the strength is also reduced, and the strength of 500MPa cannot be achieved. Therefore, how to optimize the composition and process of the existing 500MPa hot-rolled weathering steel strip to achieve the purpose of low yield ratio while meeting the mechanical properties and weathering properties is a key technical problem that needs to be broken through in the current field of weathering structural steel material design and manufacturing technology. Summary of the invention

[0007] The object of the present invention is to provide a 500MPa grade low yield ratio hot-rolled weathering steel strip and a preparation method thereof. The room temperature microstructure of the produced weathering steel is ferrite and granular bainite, the yield strength is 511-542MPa, the tensile strength is 644-677MPa, the yield ratio is ≤0.80, the elongation after fracture is ≥18%, the longitudinal V-notch impact energy KV2 at -20°C is ≥200J, and the corrosion rate relative to Q355B is ≤57%.

[0008] To achieve the above object, the present invention adopts the following technical solutions: A 500MPa grade low yield ratio hot-rolled weathering steel strip, the chemical composition of which is calculated by weight percentage as follows: C: 0.06-0.08, Si: 0.20-0.40, Mn: 0.80-1.30, P: ≤0.020, S: ≤0.005, Als: 0.020-0.030, Nb: 0.010-0.020, Cu: 0.25-0.35, Cr: 0.50-0.90, Ni: 0.12-0.20, and the balance is Fe and unavoidable impurities. In addition, the chemical composition, calculated by weight percentage, must also meet the following conditions: 40≤[Cr] / [Nb]≤50, 5.5≤3[Mn]+4[Cr]≤6.0.

[0009] The design principle of the alloy element combination relationship 40≤[Cr] / [Nb]≤50 in the present invention is: from the analysis of the phase transformation process, Nb has little effect on the phase transformation, while Cr can improve hardenability and promote the transformation of granular bainite; from the analysis of the strengthening method, Nb improves strength by means of fine grain strengthening and precipitation strengthening, while Cr improves strength by solid solution strengthening; from the tensile performance, the grain refinement effect of Nb significantly improves the yield strength, so it is not conducive to the control of low yield ratio, while the solid solution strengthening effect of Cr significantly improves the tensile strength, so it is beneficial to the control of low yield ratio. There is a complementary and competitive relationship between the two, and it is necessary to ensure that the components of Nb and Cr meet the above range, and obtain an ideal microstructure through subsequent processes, thereby achieving a balance between strength, yield ratio and economy in material design.

[0010] The design principle of the alloy element combination relationship 5.5≤3[Mn]+4[Cr]≤6.0 in the present invention is: Mn and Cr can improve the hardenability of steel, reduce the transformation temperature from austenite to ferrite, increase the phase transformation supercooling, and create dynamic conditions for the transformation of ferrite and granular bainite; at the same time, Mn and Cr are also key elements for solid solution strengthening, which can significantly improve the tensile strength of steel. If 3[Mn]+4[Cr] is too small, pearlite structure is likely to appear in the cooled structure, resulting in a decrease in tensile strength; if 3[Mn]+4[Cr] is too large, lath bainite or even lath martensite structure is likely to appear in the cooled structure. Although the strength is improved, the increase in hardened structure in the steel will reduce the elongation of the steel and cause processing cracking.

[0011] The 500MPa grade low yield ratio hot-rolled weathering steel strip of the present invention has a room temperature microstructure of ferrite and granular bainite, a yield strength of 511-542MPa, a tensile strength of 644-677MPa, a yield ratio of ≤0.80, an elongation after fracture of ≥18%, a longitudinal V-notch impact energy KV2 of ≥200J at -20°C, and a corrosion rate of ≤57% relative to Q355B.

[0012] The method for preparing the 500MPa-grade low-yield ratio hot-rolled weathering steel strip of the present invention comprises the steps of slab heating, hot rolling, laminar cooling and coiling.

[0013] Preferably, in the method for preparing the 500 MPa grade low yield ratio hot-rolled weathering steel strip of the present invention, in the slab heating process, the soaking temperature is controlled at 1210-1250°C to ensure that the alloy elements can be completely dissolved in the steel.

[0014] Preferably, in the method for preparing the 500 MPa grade low yield ratio hot-rolled weathering steel strip of the present invention, the hot rolling process includes rough rolling and finish rolling, and the final rolling temperature of the finish rolling is 890-910°C.

[0015] Preferably, in the method for preparing the 500 MPa grade low yield ratio hot-rolled weathering steel strip of the present invention, the laminar cooling process adopts a cooling mode of first slow cooling and then fast cooling.

[0016] Furthermore, in the preparation method of the 500MPa grade low yield ratio hot-rolled weathering steel strip described in the present invention, the specific operation of the cooling mode of slow cooling followed by fast cooling in the laminar cooling process is as follows: the 2nd and 4th water spray headers are opened in the 7 groups of laminar cooling groups from front to back along the rolling direction, and the 1st and 3rd water spray headers are closed, which are used for the transformation of ferrite and the precipitation of the microalloying element Nb; the water spray headers in the 8th to 12th groups of laminar cooling groups are fully opened for the transformation of granular bainite.

[0017] Preferably, in the method for preparing the 500 MPa grade low yield ratio hot-rolled weathering steel strip of the present invention, in the coiling step, the coiling temperature is 380-420°C.

[0018] The design principle of the present invention is as follows: In order to achieve the purpose of low yield ratio, there are usually two ideas: one is to adjust the grain size to a lower grain size. Since grain refinement is the most effective way to increase yield strength, coarsening the grain size can reduce the yield strength and thus reduce the yield ratio, but there may be a risk of strength mismatch; the second is to adjust the organization into a two-phase structure of "soft phase" and "hard phase". During the stretching process, since both phases are elastic-plastic bodies and the elastic-plastic behaviors of the two phases are very different, the yield strength is the result of the joint action of the two phases. The coordinated deformation between the "soft phase" and the "hard phase" can reduce the yield ratio. The present invention is based on the "hard phase" granular bainite steel, by adjusting the cooling rate, introducing a certain amount of ferrite "soft phase", thereby obtaining a two-phase organization of ferrite and granular bainite.

[0019] During the supercooled austenite phase transformation of steel, a wider temperature transformation range is required because the transformation ranges of ferrite and granular bainite are 600-800℃ and 400-600℃ respectively. Therefore, the control of high final rolling temperature of 890-910℃ provides a prerequisite for the subsequent laminar cooling, while also reducing the deformation resistance of the steel; the control of low coiling temperature of 380-420℃ provides a larger temperature gradient for laminar cooling, and also avoids the temperature range (300-350℃) where the convective heat transfer coefficient increases sharply.

[0020] The slow cooling and fast cooling in the laminar cooling process are to promote the transformation of ferrite and granular bainite respectively. The formation temperature of ferrite is relatively high (600-800℃) and the degree of supercooling is relatively small, so it is necessary to slow cool in the high temperature section at the beginning of the laminar cooling process to provide thermodynamic conditions for the transformation of ferrite; the formation temperature of granular bainite is relatively high (400-600℃) and the degree of supercooling is relatively large, so it is necessary to fast cool in the low temperature section at the end of the laminar cooling process to provide thermodynamic conditions for the transformation of granular bainite.

[0021] Compared with the prior art, the present invention has the following beneficial effects: 1. The alloy cost is low, and the weather-resistant element Cr is used to reduce the amount of Nb added, which improves the hardenability, provides the basic conditions for the transformation of ferrite and granular bainite, improves weather resistance, and significantly reduces the yield strength ratio; 2. The production process is easy to control. The process design of high final rolling and low coiling, slow cooling first and then fast cooling not only reduces the deformation resistance of steel, but also avoids the temperature range where the convective heat transfer coefficient increases sharply. Conventional hot rolling production lines can achieve stable industrialized mass production; 3. The microstructure and performance are stable. Through the comprehensive regulation of Cr alloy composition and hot rolling process, the microstructure obtained at room temperature is composed of ferrite and granular bainite. The coordinated deformation of the two significantly reduces the yield strength ratio of steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the metallographic structure of the weathering steel of Example 6.

[0023] Figure 2 This is the metallographic structure of the weathering steel of comparative example 1.

[0024] Figure 3 This is the metallographic structure of the weathering steel of comparative example 2.

[0025] Figure 4 This is the metallographic structure of the weathering steel of comparative example 3.

[0026] Figure 5 This is the metallographic structure of the weathering steel of comparative example 4.

[0027] Figure 6 This is the metallographic structure of the weathering steel of comparative example 5. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with specific examples and comparative examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Unless otherwise specified, the examples are all based on conventional experimental conditions. In addition, for those skilled in the art, without departing from the essence and scope of the present invention, various modifications or improvements to the material composition and dosage in these embodiments all belong to the scope of protection claimed in the present invention. Examples 1 to 6 and Comparative Examples 1 to 5

[0029] The chemical compositions of the weathering steel strips of various embodiments and comparative examples are shown in Table 1.

[0030] Table 1 Chemical composition and content of weathering steel strips in various embodiments and comparative examples (%)

[0031] The weather-resistant steel strips in each embodiment and comparative example adopt the preparation method of slab heating → hot rolling → laminar cooling → coiling, with an absorptive temperature of 1210-1250°C. The slabs are descaled and width-fixed after being taken out of the furnace and then enter rough rolling. The rough rolling adopts a double-stand reversible type, which consists of 2 separately arranged reversible rough rolling mills. R1 rolls 3 passes and R2 rolls 5 passes. After the rough rolling is completed, the slabs pass through the flying shear and the descaling machine in turn via the conveyor roller and enter the finishing rolling. After 7 passes of finishing rolling, the final rolling temperature of each embodiment is ensured to be 890-910°C.

[0032] The laminar cooling process of the weathering steel strip in each embodiment and comparative example 1 adopts a cooling mode of slow cooling followed by fast cooling, that is, the 2nd and 4th water spray headers are opened in the 7 groups of laminar cooling groups from front to back along the rolling direction, and the 1st and 3rd water spray headers are closed, which are used for the transformation of ferrite and the precipitation of the micro-alloying element Nb; the water spray headers in the 8th to 12th groups of laminar cooling groups are fully opened for the transformation of granular bainite; then they enter the 13th to 20th groups of laminar cooling groups for air cooling, and are cooled to the coiling temperature of 380 to 420°C in the 21st to 22nd groups of fine-tuning zones.

[0033] In the laminar cooling process of the weathering steel strip in comparative example 2, a sparse cooling mode is adopted (the 2nd and 4th water spray headers of the laminar cooling group are opened, and the 1st and 3rd water spray headers are closed), and the coiling temperature is 558°C.

[0034] The laminar cooling process of the weathering steel strip in comparative example 3 adopts the second slow cooling + fast cooling layer cooling mode. The first water spray header is opened in the 7 layers of cooling groups from front to back along the rolling direction, and the 2nd, 3rd and 4th water spray headers are closed. The water spray headers in the 8th to 14th layers of cooling groups are fully opened, and then enter the 15th to 20th layers of cooling groups for air cooling, and are cooled to the coiling temperature of 481°C in the 21st to 22nd groups of fine-tuning areas.

[0035] In comparative example 4, the laminar cooling process of the weathering steel strip adopts a cooling mode of intensive cooling (the water spray headers of the laminar cooling group are fully open), and the coiling temperature is 305°C.

[0036] The laminar cooling process of the weathering steel strip in comparative example 5 adopts the third slow cooling + fast cooling layer cooling mode. The 1st, 2nd and 3rd water spray headers are opened in the 7 layers of cooling groups from front to back along the rolling direction, the 4th water spray header is closed, and the water spray headers in the 8th to 10th layers of cooling groups are fully opened. Then, the 11th to 20th layers of cooling groups are air cooled, and the strip is cooled to the coiling temperature of 333°C in the fine-tuning zone of 21st to 22nd groups.

[0037] The actual control process parameters of each embodiment and comparative example and the room temperature structure of the steel strip are shown in Table 2.

[0038] Table 2 Process parameters and room temperature microstructure of steel strips in various embodiments and comparative examples

[0039] The mechanical properties of the weathering steel strips of various embodiments and comparative examples are shown in Table 3.

[0040] Table 3 Performance of steel strips in various embodiments and comparative examples

[0041] It can be seen from Table 2 and Table 3 that, by using the composition and preparation process of the present invention, the room temperature structure of the steel strip is composed of ferrite and granular bainite, such as Figure 1 As shown, the yield strength is 511-542MPa, the tensile strength is 644-677MPa, the yield strength ratio is ≤0.80, the elongation after fracture is ≥18%, and the -20℃ impact test meets KV2≥200J; according to TB / T 2375 "Cyclic immersion corrosion test method for weathering steel for railways", the corrosion rate relative to Q355B is ≤57%; Comparative Example 1 contains a relatively high Nb element. By adopting the production process of the present invention, fine ferrite and granular bainite structures are obtained. Figure 2 As shown, the toughness is good, but the yield strength ratio is high and the corrosion resistance is poor. Comparative Example 2 uses the weathering steel composition provided by the present invention, and the process adopts sparse cooling and high-temperature coiling process. The microstructure is ferrite and pearlite, such as Figure 3 As shown, the strength is relatively low and fails to meet the strength requirements of the weathering steel of the present invention.

[0042] Comparative Example 3 uses the weathering steel composition provided by the present invention, and adopts a cooling mode of first slow cooling and then fast cooling and a high-temperature coiling process that are not described in the present invention. The microstructure is ferrite and pearlite, such as Figure 4 As shown, the strength is relatively low and fails to meet the strength requirements of the weathering steel of the present invention.

[0043] Comparative Example 4 adopts the weathering steel composition provided by the present invention, and adopts intensive cooling and ultra-low temperature coiling process in the process, and the microstructure is granular and lath bainite, such as Figure 5 As shown, the yield strength is relatively high and the elongation and toughness are poor.

[0044] Comparative Example 5 adopts the weathering steel composition provided by the present invention, and adopts a cooling mode of first slow cooling and then fast cooling and an ultra-low temperature coiling process that are not described in the present invention. The microstructure is granular bainite, such as Figure 6 As shown, the yield strength ratio is relatively high and the elongation after fracture is relatively low, which fails to meet the yield strength ratio requirement of the weathering steel of the present invention.

[0045] In summary, the 500MPa grade low yield ratio hot-rolled weathering steel strip provided by the present invention has low alloy cost, easy-to-control production process, stable organizational performance, and can achieve stable batch industrial production. It can be widely used in steel structure construction fields such as building bridges, power towers, and railway freight cars.

Claims

1. A 500MPa grade low yield ratio hot-rolled weathering steel strip, characterized in that: The chemical composition of the weathering steel strip is calculated by weight percentage: C: 0.06-0.08, Si: 0.20-0.40, Mn: 0.80-1.30, P≤0.020, S≤0.005, Als: 0.020-0.030, Nb: 0.010-0.020, Cu: 0.25-0.35, Cr: 0.50-0.90, Ni: 0.12-0.20, and the balance is Fe and unavoidable impurities; in addition, the chemical composition must also meet the following requirements by weight percentage: 40≤[Cr] / [Nb]≤50, 5.5≤3[Mn]+4[Cr]≤6.

0.

2. A 500MPa grade low yield ratio hot-rolled weathering steel strip according to claim 1, characterized in that: The room temperature microstructure of the weathering steel strip is ferrite and granular bainite.

3. The 500MPa grade low yield ratio hot-rolled weathering steel strip according to claim 1, characterized in that: The weathering steel strip has a yield strength of 511-542 MPa, a tensile strength of 644-677 MPa, a yield strength ratio of ≤0.80, an elongation after fracture of ≥18%, a longitudinal V-notch impact energy KV2 of ≥200 J at -20°C, and a corrosion rate of ≤57% relative to Q355B.

4. A method for preparing a 500MPa grade low yield ratio hot-rolled weathering steel strip according to any one of claims 1 to 3, characterized in that: The process comprises slab heating, hot rolling, laminar cooling and coiling; the hot rolling process comprises rough rolling and finish rolling, and the final rolling temperature of the finish rolling is 890-910°C.

5. The method for preparing a 500MPa grade low yield ratio hot-rolled weathering steel strip according to claim 3, characterized in that: In the slab heating process, the soaking temperature is controlled at 1210-1250°C.

6. The method for preparing a 500MPa grade low yield ratio hot-rolled weathering steel strip according to claim 3, characterized in that: The laminar cooling process adopts a cooling mode of first slow cooling and then fast cooling.

7. The method for preparing a 500MPa grade low yield ratio hot-rolled weathering steel strip according to claim 5, characterized in that: The specific operation of the cooling mode of slow cooling followed by fast cooling is as follows: the 2nd and 4th water spray headers are opened in the 7 layers of cooling groups from front to back along the rolling direction, and the 1st and 3rd water spray headers are closed; the water spray headers in the 8th to 12th layers of cooling groups are fully opened.

8. The method for preparing a 500MPa grade low yield ratio hot-rolled weathering steel strip according to claim 3, characterized in that: In the coiling process, the coiling temperature is 380-420°C.