Construction of an electrochemical cell

By using a porous sintered body as the anode and cathode material of the electrochemical cell, it is directly in contact with the film and reduces the catalyst layer, and the efficient and energy-saving preparation of hydrogen and oxygen is achieved, solving the problems of large space occupation and high production costs in the prior art.

CN118957616AInactive Publication Date: 2024-11-15EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410599300.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-15
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing electrochemical batteries have problems such as large space occupation, high production costs and low energy efficiency during the process of water electrolysis. Especially when preparing hydrogen and oxygen on industrial scale, it is difficult to achieve high efficiency and energy saving while reducing costs.

Method used

The porous sintered body is used as the anode and cathode material. The sintered body is composed of grains fused at the grain boundary and has a porous structure that is directly in contact with the film. It assumes the functions of electrodes and porous transport layers, reduces the use of the catalyst layer, and passes through Gradient porosity design optimizes electrochemical reactions.

Benefits of technology

It realizes operation without additional porous transport layers, reduces the internal resistance of the cell, improves the efficiency and cost-effectiveness of the electrochemical cell, and can efficiently and energy-saving large quantities of hydrogen and oxygen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957616A_ABST
    Figure CN118957616A_ABST
Patent Text Reader

Abstract

The invention relates to an electrochemical cell (0) comprising an anode (1), a cathode (2) and an anion-conducting membrane (3) arranged between the anode (1) and the cathode (2). The invention also relates to the use of an electrochemical cell (0) in a method for producing hydrogen (H2) and oxygen (O2) by electrochemical decomposition of water (H2O). The invention also relates to an electrolytic cell (6) having a plurality of cells (0) and to a method for producing an electrolytic cell (6). An object of the invention is to provide an electrochemical cell (0) with which AEM water electrolysis can be carried out on an industrial scale. The production cost of the cell is reduced, the cell is constructed in a space-saving manner and allows high-efficiency and energy-saving production of hydrogen and oxygen in large quantities. This object is achieved by partially or entirely implementing the anode as a first porous sintered body (1) comprising grains fused together at the grain boundaries thereof and by bringing the first porous sintered body into direct contact with a film (3).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrochemical cell comprising an anode, a cathode and an anion conducting membrane arranged between the anode and the cathode. The present invention also relates to the use of the electrochemical cell in a method for producing hydrogen and oxygen by electrochemical decomposition of water. The present invention also relates to an electrolyser having a plurality of cells and a method for producing the electrolyser. Background Art

[0002] Electrochemical cells are used to carry out electrochemical processes. There are many electrochemical processes with very different goals. An important electrochemical process is the decomposition of chemical compounds. This process is called electrolysis.

[0003] An industrial implementation of an electrochemical cell for performing electrolysis is called an electrolysis cell. An electrolysis cell typically comprises a plurality of interconnected electrochemical cells.

[0004] An electrochemical cell has at least two electrodes: an anode and a cathode. An electrochemical cell is usually divided into two compartments by an electrically insulating separator. The anode is present in a first, or "anode" compartment, and the cathode is present in a second, or "cathode" compartment. The two electrodes or compartments are electrically isolated from each other by the separator. The electrochemical cell is filled with an electrolyte.

[0005] An important electrochemical process is the production of hydrogen and oxygen by the electrochemical decomposition of water. A variant of water electrolysis is characterized by the use of an anion-conducting membrane (anion exchange membrane, AEM) as a diaphragm. This is usually referred to as AEM water electrolysis (AEMWE). Since the reaction takes place in an alkaline medium, AEM water electrolysis is also often referred to as alkaline membrane water electrolysis.

[0006] In AEM water electrolysis, an electrochemical cell is filled with water or an alkaline water-based electrolyte and a voltage is applied between the anode and cathode. On the cathode side, water (H2O) is decomposed into hydrogen gas (H2) and hydroxide ions (OH - )(Equation C). The anion exchange membrane transports the hydroxide ions to the anode side where they are oxidized to oxygen (O2) (Equation A). This results in the release of oxygen on the anode side and simultaneous release of hydrogen on the cathode side. Therefore, the anode side is also referred to as the oxygen side, while the cathode side is also referred to as the hydrogen side.

[0007] 2H2O+2e - →H2+2OH - (C) Reduction / cathode reaction

[0008] 2OH - →1 / 2O2+H2O+2e - (A) Oxidation / anodic reaction

[0009] In order to achieve the described effect, the membrane must conduct hydroxide ions between the anode and cathode. At the same time, the membrane must be electrically insulating so that no electrical short circuit occurs between the anode and cathode. Finally, if possible, the anion conducting membrane must be gas-tight so that there is no back mixing of the evolved gases. In addition, the anion conducting membrane must withstand the alkaline conditions present in AEM water electrolysis. These properties are achieved by special anion conducting polymers (also called anion conducting ionomers).

[0010] To accelerate the reaction, catalytically active substances (also called electrocatalysts) are incorporated both on the cathode side and on the anode side. This is achieved by introducing catalytically active layers. These catalytically active layers can be present on a substrate material specially introduced into the cell for this purpose or on a porous transport layer (catalyst-coated substrate, CCS), or the membrane can be directly coated with the catalytically active material (catalyst-coated membrane, CCM).

[0011] In AEM water electrolysis, water or electrolyte must flow through the cell and gases must flow out of the cell in order to supply fresh water for electrolysis and to discharge hydrogen and oxygen, or water or electrolyte enriched with hydrogen and oxygen in turn. This is usually ensured by a porous transport layer (PTL), which is firstly adjacent to the catalytically active layer in order to ensure good electrical contact; secondly, the porous transport layer (PTL) is conductive and has sufficient porosity to transport gases outward and to supply water and electrolyte. In order to improve the transport of water or electrolyte through the cell, a specific channel structure (called flow field) is incorporated into the cell. This structure must be in electrical contact with the porous transport layer, have conductivity and establish electrical contact with the bipolar plate (BPP). The bipolar plate electrically connects two adjacent cells. The specific channel structure is usually directly incorporated into the bipolar plate, for example by mechanical deformation. For efficient water electrolysis, it is particularly important that the contact resistance at the contact surfaces of (i) the catalytically active layer and the porous transport layer, (ii) the porous transport layer and the flow field, and (iii) the flow field and the bipolar plate is kept as low as possible and does not increase during operation of the electrolyzer due to oxidation of the contact surfaces. Otherwise, the increased contact resistance will lead to an increase in the cell voltage, a decrease in efficiency and an increase in energy consumption.

[0012] The following is an excellent review of the architecture and materials of electrochemical cells currently used in AEM water electrolysis: Miller, Hamish Andrew et al.: Green hydrogen from anion exchange membrane water electrolysis: a review of recent developments in critical materials and operating conditions, Sustainable Energy Fuels, 2020, 4, 2114 DOI: 10.1039 / c9se01240k.

[0013] The overall goal of developing electrolyzers for water electrolysis is to increase the efficiency of the process and to reduce the manufacturing costs of the electrolyzers.

[0014] Nickel foam is mentioned as an electrode material in the review cited by Miller et al. The foam is a porous structure.

[0015] EP 3453785 A1 describes an electrochemical cell for alkaline water electrolysis. It discloses in paragraph

[0022] an anode having a supply layer (17) which is partially made of a metal nonwoven or metal foam. The material specified in paragraph

[0023] is nickel or stainless steel. A further catalyst layer (15) is arranged between the nonwoven and the membrane (13); see FIG. 1 and paragraphs

[0015] and

[0027] . The electrode-catalyst layer-membrane-catalyst layer-electrode sandwich structure of the electrochemical cell (see paragraph

[0053] ) is very space-consuming. This is particularly disadvantageous when many such cells are to be connected in an electrolytic cell. In this case, not only does the space occupied by the electrolytic cell increase, but also the internal resistance of the cell stack increases. This reduces the energy efficiency of the method. A good feature of the electrochemical cell shown in EP 3453785 A1 is fluid management: in order to improve the flow of water into the compartment and the flow of gas out of the compartment, the membrane is provided with channels; paragraph

[0054] . The electrochemical cell thus appears to be suitable in principle for industrial water electrolysis. Disadvantages are the space-consuming layer structure and the high production costs due to the incorporation of catalyst layers: these contain expensive metals which serve as electrocatalysts; see paragraph

[0029] .

[0016] WO 2020260370 A1 describes an electrochemical cell in which one compartment can be operated dry. CCS on nickel nonwovens or foams is mentioned on page 5. However, CCS does always have a catalyst layer. WO 2020260370 A1 page 6 recommends the use of metal oxides (e.g. copper-cobalt oxides) as electrocatalysts for the anode. However, for cost reasons, WO 2020260370 A1 page 6 recommends not using Pt catalysts.

[0017] WO 2016142382 A1 discloses in FIG. 2 an embodiment I of a (photo) electrochemical cell having a cathode (corrosion protection layer 15 of the photoelectrode 2), an anion conducting membrane (2) and an anode (counter electrode 3). Disposed between the anode (3) and the membrane (2) is a porous nickel-containing structure (5A). The porous nickel-containing structure (5A) can be composed of nickel fibers or stainless steel fibers. Nickel foam is also conceivable (page 12). As shown in FIG. 2 and described on page 17, the anode (counter electrode 3) is separated from the membrane. The porous nickel-containing structure (5A) is arranged in between. A disadvantage of this cell is its bulky layer structure.

[0018] A more streamlined solution is Implementation II of WO 2016142382 A1, which does not require a porous nickel-containing structure. The porosity required for fluid conduction is achieved in the membrane. Since the photoelectrochemical cell has an integrated voltage source (i.e., a photoelectrode), the electrical energy available for water electrolysis is limited. When driven by pure light, the electrolysis capacity is low. In industrial water electrolysis using external electrical energy, a large amount of gaseous hydrogen and oxygen will be produced, and these gaseous hydrogen and oxygen must be exported from the pool. The porous structure integrated in the membrane in Implementation II is not designed for this amount of gas. However, the construction in Implementation II is too large for the compact design of an industrial-scale electrolyzer.

[0019] EP 4181240 A1, which was not yet published at the time of filing, also relates to an electrochemical cell for water electrolysis, which has a textile electrode comprising nickel. The textile electrode is directly adjacent to the membrane.

[0020] With regard to this prior art, the object of the present invention is to provide an electrochemical cell with which AEM water electrolysis can be carried out on an industrial scale. The cell reduces production costs, is constructed in a space-saving manner and allows the energy-efficient and large-scale production of hydrogen and oxygen. Summary of the invention

[0021] This object is achieved by the electrochemical cell according to the invention.

[0022] Therefore, the present invention provides an electrochemical cell for alkaline membrane water electrolysis, which comprises an anode, a cathode and an anion conducting membrane arranged between the anode and the cathode, wherein the anode is partially or completely implemented as a first porous sintered body, the first porous sintered body comprises grains fused together at their grain boundaries, and wherein the first porous sintered body is in direct contact with the membrane. A fundamental discovery of the present invention is that the porous structure in the form of a sintered body is not only suitable as an electrode, but can also simultaneously assume the function of a porous transport layer for electrolyte and / or gas evolution: the sintered body is essentially porous because there are cavities between the individual particles. This is because the particles are irregularly shaped and sometimes fused together in certain places. Water or electrolyte can penetrate into these cavities and thus come into contact with the electrode material. This allows the reactants to reach the catalytically active centers directly through the porous cavities in the sintered body. The evolved gases can also escape through the cavities. Therefore, the sintered body not only realizes the electrochemical function, but also the flow function. The fluid conductivity of the porous electrode enables it to be in direct contact with the membrane. This means that the sintered body is directly adjacent to the membrane in a planar manner. Therefore, no catalyst layer is arranged between the anode and the membrane. Therefore, there is direct mechanical contact between the membrane and the sintered body, preferably over the entire interface between the membrane and the electrode. However, since the membrane is not conductive, there is no contact problem in the electrical sense. By virtue of the fluid conducting properties of the sintered body, the electrochemical cell of the present invention can operate without an additional porous transport layer. This reduces the internal resistance of the cell, since there is no contact resistance between the various components that are usually used. However, it may be necessary to incorporate a flow field in the electrochemical cell that is in contact with the electrolyte and the gas entering and leaving the cell. However, the flow field is arranged away from the membrane; preferably, the flow field is incorporated into the bipolar plate or the end plate. The flow field has a much larger flow cross section than the pores of the sintered body.

[0023] Sintered bodies differ from known textile structures in that they are not constructed from linear textile structures, ie fibers, yarns, filaments or threads. Instead, sintered bodies are formed from grains.

[0024] Sintered bodies differ from known metal foams in that they are formed from grains that are connected at least in some places at grain boundaries. Sintered bodies are therefore not monolithic. Metal foams, on the other hand, have a monolithic metal dispersion phase in which a gas phase is dispersed. The pores of sintered bodies are generally much smaller than the individual grains. In contrast, metal foams have relatively large pores relative to their metal phase.

[0025] In a particularly preferred embodiment, the grains of the sintered body consist of or at least comprise a catalytically active material. "Catalytic activity" in this context means that the material is capable of accelerating an electrochemical reaction carried out in an electrochemical cell. The catalytically active material is thus an electrocatalyst.

[0026] The use of catalytically active sintered materials allows the reactants to come into particularly close contact with the catalytically active centers present in the grains of the sintered material. As a result, the electrochemical reaction can be carried out very close to the membrane, which means that the ions formed are able to pass directly through the membrane into the opposite compartment.

[0027] Materials with electrocatalytic activity usually contain transition metals. For the purposes of the present invention, transition elements are: Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Ac, Rf, Db, Sg, Bh, Hs, Mt, Ds, Rg. Sintered materials containing transition elements have a higher electrocatalytic activity than sintered materials without transition elements. In addition, the relatively good electrical conductivity of transition metals reduces the internal resistance of the electrochemical cell.

[0028] Very particularly preferably, nickel is used as the electrocatalytically active material. Therefore, in a preferred embodiment of the invention, the grains of the sintered body contain nickel or consist of nickel. The grains themselves are then electrocatalytically active.

[0029] Nickel is a relatively cheap transition metal with good catalytic properties, especially in water electrolysis. In addition, there are some nickel-containing materials that can be easily sintered into anodes. These materials include pure nickel, nickel-containing alloys such as, in particular, Hastelloy, Chronin, Monel, Inconel, Incoloy, Invar, Kovar; nickel-containing steels, nickel-containing stainless steels, and steels of grades AISI 301, AISI 301L, AISI 304, AISI 304L, AISI 310, AISI 310L, AISI 316, AISI 316L, AISI 317, AISI 317L and AISI 321.

[0030] In a particularly preferred embodiment of the invention, the anode is therefore at least partially embodied as a first sintered body, the grains of which consist of a nickel-containing material.

[0031] An additional advantage of the electrochemical cell of the present invention is that an ionomer (often also called a binder) for fixing the electrocatalyst on a substrate or electrode (CCS) or directly on a membrane (CCM) is not absolutely required. The oxygen formed during electrolysis is highly reactive and chemically attacks (oxidizes) the ionomer, which leads to impairment of the mechanical properties of the ionomer and may also cause the electrocatalyst to fall off. This then leads to an increase in the required cell voltage and to increased energy consumption. However, when the sintered body itself is electrocatalytically active, the risk of catalyst falling off is smaller. As a result, the structure of the proposed electrochemical cell reduces its manufacturing costs and, due to the low electrical resistance, allows an energy-efficient process.

[0032] In view of the advantages of the sintered structure, the anode is preferably completely embodied in the form of a porous sintered body. However, it is also conceivable to use an anode which is only partially embodied in the form of a porous sintered body and the rest consists of non-sintered material. Non-sintered here means that there are no identifiable grain boundaries. Therefore, the sintered body can also be mounted on a solid plate or on a flat or shaped metal sheet or on different porous structures such as metal foam, expanded metal or expanded metal mesh.

[0033] Preferably, the first sintered body contains no catalytically active coating of a material different from that of the sintered body. In this case, the catalysis of the anode reaction is achieved exclusively by the electrocatalytically active material present in the sintered body or constituting the grains of the sintered body.

[0034] The porosity P of the first porous sintered body used as the anode should be between 5% and 60% or between 15% and 45%. The porosity P here is determined according to the following formula:

[0035] P=1-ρ V / ρ M

[0036] In this formula, ρ V is the volume density of the porous sintered body, ρ M is the solid density of the grain. V describes the macroscopic density of the entire sintered body, while ρ M Describes the microscopic density of the sintered material that makes up the grains.

[0037] Compared with the foam, the porosity of the sintered body is quite low: the porosity of nickel foam typically varies between 80% and 90%; see Table 1 in the following literature: Rocha Fernando et al.: Effect of pore size and electrolyte flow rate on the bubble removal efficiency of 3D pure Ni foam electrodes during alkaline water electrolysis, Journal of Environmental Chemical Engineering, Volume 10, Issue 3, April 1, 2022 (2022-04-01), Page 107648, ISSN: 2213-3437, DOI: 10.1016 / 3.jece.2022.107648.

[0038] In the simplest case, the porosity is the same everywhere in the first sintered body. Preferably, the porosity in the first sintered body can be changed, specifically along a (hypothetical) gradient perpendicular to the interface between the first porous sintered body and the membrane. The porosity P should be reduced in the direction of the membrane so that the first sintered body has a lower porosity at the interface with the membrane than at the side of the anode away from the membrane. This means that the catalytically active centers are concentrated at the membrane, with the result that the electrochemical reaction there is particularly intense. This shortens the path of the ions generated at the anode.

[0039] Preferably, the pores of the first porous sintered body are smaller than the grains of the first porous sintered body. This is a major difference compared to foams, where the pores are larger than solid materials. The size difference can be easily estimated by optical microscopy, i.e. by examining a section through the first porous sintered body. The pore sizes of the sintered body are randomly distributed. The pore sizes are typically between 1 μm and 200 μm. The pore sizes of the sintered body are also much smaller than typical flow cross sections of a flow field, which are in the range of 1 mm.

[0040] The grain size of the sintered body is also randomly distributed. The difference between pore size and grain size is evaluated not by comparing the extreme values, but by comparing the median values: if the single largest pore is larger than the smallest grain, this is harmless as long as the median pore size is smaller than the median grain size. The property of a sintered body with a pore size smaller than its grain size statistically means that the median pore size is smaller than the median grain size.

[0041] The first porous sintered body can also be formed by at least two layers, wherein the two layers have different porosities or are composed of grains of different particle sizes. The layer with lower porosity or composed of finer particles must be arranged closer to the membrane than the layer with higher porosity or composed of coarser particles. The effect is that the porosity of the electrode decreases toward the membrane, in other words, the electrode becomes denser and consists of finer grains. This is desirable because a greater density of catalytic active sites is required near the membrane, and a greater permeability of water or electrolyte and formed gas is required away from the membrane. The sintered body can also be formed by more than two layers, for example, by three or four or five or six layers. Then, the porosity of each layer or the sintered grain size is reduced layer by layer in the direction of the membrane. This realizes the gradient already mentioned above. The sintered layers can be bonded to each other by grain boundaries, and as a result, the sintered body can be handled as a single component regardless of the layer structure. This is conducive to the assembly of the cell.

[0042] Since the nickel-containing sintered bodies described herein are also suitable as cathodes, it is conceivable that both the anode and the cathode are produced from sintered catalytically active materials. Therefore, in a preferred development of the electrochemical cell, its cathode is partially or completely embodied as a second porous sintered body comprising grains fused together at their grain boundaries.

[0043] In order to distinguish between a sintered body used as a cathode and a sintered body used as an anode, the term "first porous sintered body" is used for the anode, and the term "second porous sintered body" is used for the cathode.

[0044] On the cathode side, it is not absolutely necessary to integrate the catalytic activity into the sintered material. However, it is preferred that the second sintered body also uses a catalytically active material. The same material as on the anode side is suitable here. In the simplest case, the same material is used on both the anode side and the cathode side. However, this is not necessarily necessary. Therefore, it is appropriate to distinguish between a first sintered body and a second sintered body. Preferably, the cathode is completely embodied as a porous sintered body.

[0045] The second porous sintered body, in addition to its electrochemical function as a cathode, also realizes the function of a porous transport layer.

[0046] The cathode side of the electrochemical cell can be constructed in two variants.

[0047] In a first variant, the cathode (hydrogen side, in particular implemented as a second porous sintered body) is in direct contact with the membrane. In this case, the membrane itself is not coated with any catalytically active material (electrocatalyst), which requires that the catalytically active substance has been applied to the cathode or that the cathode material itself has catalytic activity.

[0048] In a second variant, the catalytically active layer (electrocatalyst) is arranged between the cathode (hydrogen side, in particular implemented as a second porous sintered body) and the membrane. The particles forming the second sintered body do not necessarily have to be catalytically active or coated with a catalytically active substance. In this case, the grains of the second sintered body must only be conductive in order to allow electrical contact between the catalytically active layer (electrocatalyst) and the flow field or the bipolar plate. This structure is advantageous when the electrocatalyst to be used cannot be integrated into the grains, or cannot be produced therefrom, or cannot be applied to the second porous sintered body in a manner with permanent stability, or its catalytic activity is higher than that of the sintered material itself or of the catalytically active substances formed on the surface of the grains during operation of the electrolyzer.

[0049] As described above, the variant of the invention having a catalyst layer between the cathode and the membrane has the advantage that it can contain electrocatalysts that cannot be easily applied to the second sintered body. Thus, the catalyst layer can contain catalytically active particles (electrocatalysts) containing elements such as Pt, Ru, Pd, C, Ni, Mn, Mo, Co, Cu, Fe, Cr.

[0050] It is particularly advantageous when the catalytically active particles of the electrocatalyst are embedded in an anion-conducting polymer. In this case, the catalyst layer consists at least of the catalytically active particles and the anion-conducting polymer. Ion-conducting polymers are called ionomers. Embedding the catalytically active particles in the anion-conducting ionomer ensures that the hydroxide ions formed during the water reduction at the cathode can be conducted into the membrane immediately after the reaction. It is very particularly preferred when the anion-conducting polymer has very good adhesion to the membrane surface and conducts hydroxide ions very well. In this case, the catalyst particles are particularly effectively integrated with the membrane and the catalyst particles are particularly well ionically bonded to the membrane.

[0051] However, in contrast to known CCM designs (membranes coated with electrocatalysts on both sides), the membranes of the present structure are provided with a catalyst layer at most on the cathode hydrogen-producing side. The anode oxygen-producing side does not have any catalyst layer; the electrocatalyst is located on the oxygen side integrated into the sintered anode material. Therefore, the variant with a catalyst layer exclusively on the cathode side can be regarded as a "semi-CCM cell".

[0052] The separation-active material forming the anion-conducting membrane is also an anion-conducting ionomer. In principle, all anion-conducting ionomers can be incorporated into the electrochemical cell according to the invention and hereby assume the function of separation-active membrane material and / or serve to immobilize catalytically active particles.

[0053] In a preferred embodiment of the invention, the membrane comprises the same anion-conducting polymer as the catalytically active coating which fixes the catalyst on the hydrogen side. The ionomer in the catalyst layer and the ionomer in the membrane should have at least the same repeating units in the anion-conducting polymer; the chain length may differ.

[0054] Particular preference is given to using anion-conducting polymers which correspond to the formula (I) or (II) or (III).

[0055] The common advantages of the ionomers of formula (I), (II) or (III) are their good ionic conductivity, high resistance to swelling in alkaline media and low synthesis cost.

[0056] The ionomers of formula (I) or (II) or (III) can be used for the preparation of membranes or as binders for fixing electrocatalysts in catalytically active layers or on inactive sintered materials.

[0057] The anion conducting polymer of formula (I) is defined as follows:

[0058]

[0059] Where X is a structural element containing a positively charged nitrogen atom attached to C 1 and C 2 and is connected to one or two hydrocarbon groups containing 1 to 12, preferably 1 to 6, more preferably 1 or 5 carbon atoms through two bonds, and wherein Z is a hydrocarbon group containing a hydrocarbon group connected to C 3 and C 4 The present invention relates to a structural element having carbon atoms and containing at least one aromatic six-membered ring directly connected to one of the oxygen atoms, wherein the aromatic six-membered ring may be substituted by one or more halogen groups and / or one or more C1 to C4 alkyl groups.

[0060] The preparation of ionomers of formula (I) is described in WO 2021 / 013694 A1.

[0061] The anion conducting polymer of formula (II) is defined as follows:

[0062]

[0063] Where X is a structural element containing a positively charged nitrogen atom attached to C 1 and C 2 and is connected to one or two hydrocarbon groups containing 1 to 12, preferably 1 to 6, more preferably 1 or 5 carbon atoms through two bonds, and wherein Z is a hydrocarbon group containing a hydrocarbon group connected to C 3 and C 4 The invention relates to a structural element having at least one aromatic six-membered ring which has carbon atoms and which is directly connected to one of the oxygen atoms, wherein the aromatic six-membered ring may be substituted in the 3- and 5-positions by identical or different C1-C4-alkyl groups, in particular by methyl, isopropyl or tert-butyl groups, preferably by methyl groups.

[0064] The preparation of ionomers of formula (II) is described in EP 4 032 934 A1.

[0065] The anion conducting polymer of formula (III) is defined as follows:

[0066]

[0067] Wherein X is a ketone or a sulfone group;

[0068] wherein Z is a structural element containing at least one tertiary carbon atom and at least one aromatic six-membered ring, wherein the aromatic six-membered ring is directly attached to one of the two oxygen atoms;

[0069] wherein Y is a structural element containing at least one positively charged nitrogen atom, wherein the nitrogen atom is connected to the structural element Z.

[0070] The preparation of ionomers of formula (III) is described in EP 4 059 988 A1.

[0071] Regardless of whether the electrochemical cell is equipped with one or two porous sintered bodies (electrodes), it is advantageous when the first sintered body and / or the second sintered body is in contact with the bipolar plate on its side away from the membrane. "Contact" here means not only in a mechanical sense, but also in an electrical sense, since the bipolar plate is electrically conductive. The contact is preferably made over the entire area. More preferably, direct contact is envisaged, in which no additional material is incorporated into the cell between the electrode and the bipolar plate. This makes the cell particularly compact and cost-effective. The fluid conduction function of the porous sintered body is then optimally utilized. The bipolar plate can be used to establish electrical contact with adjacent electrochemical cells. This makes it possible to save space by stacking a plurality of electrochemical cells connected in series; see below.

[0072] The bipolar plates are preferably composed of one of the following materials: nickel; nickel-containing alloys such as Hastelloy, Chronin, Monel, Inconel, Incoloy, Invar, Kovar; nickel-containing steel, nickel-containing stainless steel, steel of the types AISI 301, AISI 301L, AISI304, AISI 304L, AISI 310, AISI310L, AISI316, AISI 316L, AISI 317, AISI 317L and AISI321; nickel-plated steel, nickel-plated stainless steel, nickel-plated titanium, nickel-plated brass, nickel-plated aluminum, nickel-plated acrylonitrile-butadiene-styrene copolymer and carbon.

[0073] The electrochemical cell presented herein is optimized for use in alkaline water electrolysis (AEM water electrolysis). Thus, the present invention provides for the production of hydrogen and oxygen by electrochemical decomposition of water, having the following process steps:

[0074] a) providing at least one electrochemical cell comprising an anode, a cathode and an anion conducting membrane arranged between the anode and the cathode, wherein the anode is at least partially embodied as a first porous sintered body comprising grains fused together at their grain boundaries, and wherein the first porous sintered body is in direct contact with the membrane;

[0075] b) providing an aqueous electrolyte having a pH of 7 to 15;

[0076] c) providing a voltage source;

[0077] d) contacting the first sintered body and / or the cathode with an electrolyte;

[0078] e) applying a voltage obtained from a voltage source to the anode and the cathode;

[0079] f) exhausting oxygen and / or an electrolyte in which oxygen is dissolved from the first porous sintered body;

[0080] g) exhausting hydrogen gas and / or electrolyte in which hydrogen gas is dissolved from the electrochemical cell;

[0081] h) optionally separating oxygen from the electrolyte discharged from the first porous sintered body;

[0082] i) optionally separating hydrogen from the electrolyte discharged from the cell.

[0083] The electrolyte used here contains water to be electrolyzed. The pH of the electrolyte is adjusted to an alkaline region (pH 7 to pH 15) by adding an alkaline substance such as NaOH or KOH to the water. Therefore, the water in the electrolyte is decomposed in the water electrolysis, and thus water is continuously supplied to the electrolyte.

[0084] The method can be operated in two variants: wet and semi-dry. In the wet variant, both compartments are loaded with electrolyte. In the semi-dry operating mode, only one of the two compartments is loaded with electrolyte, either on the anode side (case 1) or on the cathode side (case 2).

[0085] In the wet variant, both compartments on either side of the membrane are immersed in an aqueous alkaline electrolyte. Hydrogen accumulates in the aqueous electrolyte on the cathode side and oxygen on the anode side. If the gases do not bleed out of the electrolyte on their own, the electrolyte is vented from both compartments and the desired gases are released.

[0086] In practice, mixed forms may also exist in which a portion of the gas formed escapes on its own from the porous sintered body and a further portion remains dissolved in the water and has to be separated therefrom in a separate operation.

[0087] Unlike the wet variant, in the semi-dry variant, only the anode side (anode, case 1) or the cathode side (cathode, case 2) is immersed in an alkaline electrolyte. The cathode or anode chamber remains dry. From there, hydrogen or hydrogen-rich alkaline electrolyte or oxygen or oxygen-rich alkaline electrolyte is discharged from the second porous sintered body (cathode) or from the first porous sintered body (anode). In case 1, oxygen accumulates in the anode chamber filled with alkaline electrolyte, as in the case of the wet variant. In case 2, hydrogen accumulates in the cathode chamber filled with alkaline electrolyte, as in the case of the wet variant.

[0088] The advantage of these two semi-dry variants is that there is no need to separate the alkaline electrolyte and hydrogen (case 1) or oxygen (case 2), since the respective electrodes are not immersed in the alkaline electrolyte and the gases formed therefore contain very little water. The basic idea of ​​the semi-dry AEM process (case 1) using water only on the anode side is described in WO 2011 / 004343 A1.

[0089] Therefore, in the semi-dry method (Case 1), there is no need to soak the second porous sintered body and there is no need to separate the hydrogen. The formed hydrogen directly exists in the cathode chamber in a gaseous form.

[0090] In fact, in case 1, there can also be a mixed form, in which part of the oxygen escapes from the first porous sintered body on its own, while another part of the oxygen remains dissolved in the water and must be separated therefrom in a separate operation. However, if hydrogen recovery is the only purpose, the step of separating oxygen from the electrolyte taken from the first porous sintered body can be omitted. The oxygen remains in the electrolyte. This process is particularly energy-saving because it is not necessary to separate hydrogen and oxygen from the electrolyte.

[0091] When the electrolysis is carried out in such a way that only the cathode side (cathode, case 2) is immersed in an alkaline electrolyte, a separate oxygen separation can be omitted.

[0092] In fact, in case 2, there can also be a mixed form, in which a portion of the hydrogen escapes from the first porous sintered body on its own, while another portion of the hydrogen remains dissolved in the electrolyte and must be separated therefrom in a separate operation.

[0093] The common point of all method variants presented herein is to utilize the porous structure of sintered body to guide reactants to the catalytic active center of electrocatalyst. According to the present invention, porous sintered body realizes fluid conduction function in all cases. Depending on the embodiment (wet, semi-dry situation 1, semi-dry situation 2), the fluid conducted in porous sintered body is liquid electrolyte, liquid electrolyte with hydrogen dissolved therein, liquid electrolyte with oxygen dissolved therein, oxygen or hydrogen. In addition, fluid can comprise multiple phases consisting of mentioned gas and liquid.

[0094] A particular advantage of the electrochemical cell structure presented herein is that it can be used for different process variants without any structural changes. Therefore, the manufacturer of the electrochemical cell only needs to design one cell, and then the user of the cell can decide which process variant (wet, semi-dry, etc.) is the most cost-effective for his / her application. The reduction in complexity makes the production cost of the cell significantly reduced.

[0095] All method variants presented herein are preferably implemented continuously. This means that the aqueous alkaline electrolyte is continuously supplied and the gas or oxygen-rich and / or hydrogen-rich electrolyte is continuously discharged. The continuous supply of electrolyte compensates for the loss of water present therein due to electrolysis. Otherwise, over time, water would be completely electrolyzed and electrolyte would be lost. The electrochemical reaction would then stop. Although it is conceivable that an intermittent process in which the electrochemical cell is completely filled with electrolyte or at least its anode compartment is filled with electrolyte and is electrolyzed until the cell or anode compartment becomes empty is not preferred on an industrial scale.

[0096] The method of the invention is preferably carried out in an electrolyser comprising at least two electrochemical cells of the invention which share a common bipolar plate. This means that the bipolar plate is in contact with the anode of the first electrochemical cell of the electrolyser and the cathode of the second electrochemical cell of the electrolyser at the same time. In this case, the two adjacent cells are connected in series. The invention also provides such an electrolyser.

[0097] The advantage of an electrolyser in which adjacent cells each share a bipolar plate is its compact stacking construction and thus its small construction size. Preferably, the electrolyser comprises more than two adjacent cells sharing a common bipolar plate. Depending on the size of the individual electrochemical cells and the desired output, up to 250 cells can be stacked in one electrolyser by means of the bipolar plates.

[0098] Another advantage of the electrolyser of the invention is that it can be manufactured with a high degree of automation: this is because the individual components of the electrochemical cell can be stacked very efficiently by robots. This enables the production costs of the electrolyser to be further reduced.

[0099] The invention also provides a method for preparing an electrolytic cell comprising at least two electrochemical cells of the invention, which share a common bipolar plate when the following components are stacked directly one after the other in this order during the preparation process.

[0100] In this method, the order of stacking events is from anode to cathode:

[0101] a) a first porous sintered body;

[0102] b) anion conducting membrane;

[0103] c) an optional catalyst layer;

[0104] d) cathode;

[0105] e) bipolar plates;

[0106] f) a first porous sintered body;

[0107] g) anion conducting membrane;

[0108] h) an optional catalyst layer;

[0109] i) Cathode.

[0110] The same can be done from cathode to anode. In that case, the stacking order is as follows:

[0111] a) cathode;

[0112] b) an optional catalyst layer;

[0113] c) anion conducting membrane;

[0114] d) a first porous sintered body;

[0115] e) bipolar plates;

[0116] j) cathode;

[0117] k) an optional catalyst layer;

[0118] 1) anion conducting membrane;

[0119] m) A first porous sintered body.

[0120] Both stacking sequences produce identical electrolyzers. In order to bring more than two adjacent cells of the invention into contact with each other through a common bipolar plate according to the invention, the stacking sequence can be run repeatedly. After each run, the bipolar plates should be inserted.

[0121] For example, when three cells are stacked from anode to cathode, the stacking order is as follows:

[0122] a) a first porous sintered body;

[0123] b) anion conducting membrane;

[0124] c) an optional catalyst layer;

[0125] d) cathode;

[0126] e) bipolar plates;

[0127] f) a first porous sintered body;

[0128] g) anion conducting membrane;

[0129] h) an optional catalyst layer;

[0130] i) cathode;

[0131] j) bipolar plates;

[0132] k) a first porous sintered body;

[0133] 1) anion conducting membrane;

[0134] m) an optional catalyst layer;

[0135] n) cathode.

[0136] All stacks may be provided with end plates at either end of the stack, which are similar in structure to the bipolar plates, but connected in a monopolar manner.

[0137] The stacking is preferably automated, in particular using a robot.

[0138] The preparation of the electrolyser is particularly efficient when the first and second sintered bodies consist of the same material. It is particularly preferred to use the same sintered body for both anode and cathode. In this case, the number of different parts is smaller, which increases the assembly speed and reduces the cost of the electrolyser. In this case, the stacking process can also be better performed by a robot, because the robot does not need to distinguish between anode and cathode, but only needs to install one sintered body as electrode. It then does not matter whether the stacking is from cathode to anode or from anode to cathode.

[0139] The present invention also provides the intended use of the electrochemical cell in alkaline membrane water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0140] The present invention will now be described by working examples. In this regard, the accompanying drawings show:

[0141] Figure 1a : A schematic diagram of a first embodiment of an electrochemical cell;

[0142] Figure 1b : A first embodiment of an electrochemical cell ( Figure 1a ) is a schematic diagram of the operation in the wet process variant;

[0143] Figure 1c : A first embodiment of an electrochemical cell ( Figure 1a ) Schematic diagram of operation in a semi-dry variant (Case 1 - "dry cathode");

[0144] Figure 1d : A first embodiment of an electrochemical cell ( Figure 1a ) Schematic diagram of operation in a semi-dry variant (Case 2 - "dry anode");

[0145] Figure 2a : A schematic diagram of a second embodiment of an electrochemical cell;

[0146] Figure 2b : A second embodiment of the electrochemical cell ( Figure 2a ) is a schematic diagram of the operation in the wet variant;

[0147] Figure 2c : A second embodiment of the electrochemical cell ( Figure 2a ) Schematic diagram of operation in a semi-dry variant (Case 1 - "dry cathode");

[0148] Figure 2d : A second embodiment of the electrochemical cell ( Figure 2a ) Schematic diagram of operation in a semi-dry variant (Case 2 - "dry anode");

[0149] Figure 3 : comprising two according to the first embodiment ( Figure 1a ) is a schematic diagram of an operating variant of an electrolytic cell of an electrochemical cell;

[0150] Figure 4 : comprising two according to the second embodiment ( Figure 2a ) is a schematic diagram of the design of the electrolytic cell of an electrochemical cell.

[0151] Figure 5 : Current-voltage curve in Example 1

[0152] Figure 6 : Current-voltage curves of Example 2 and Example 1 DETAILED DESCRIPTION

[0153] Figure 1a A cross section of a first embodiment of an electrochemical cell 0 is shown in schematic form. The electrochemical cell 0 comprises an anode 1, a cathode 2 and an anion conducting membrane 3 arranged between the anode 1 and the cathode 2. Both the anode 1 and the cathode 2 are implemented as porous sintered bodies. The porosity is, for example, 38%. The pores can be distributed uniformly in the sintered body, or can be distributed following a gradient, so that the porosity increases with increasing distance from the membrane 3.

[0154] The membrane 3 is a flat membrane made of an anion-conducting polymer. The membrane 3 divides the electrochemical cell 0 into two compartments: an anode compartment on the anode 1 side and a cathode compartment on the cathode 2 side. Both the anode 1 and the cathode 2 are directly adjacent to the membrane 3. The sides of the anode 1 and the cathode 2 facing away from the membrane 3 are each in contact with an end plate 4.

[0155] The active areas of the anode 1 and the cathode 2 extend perpendicularly to the plane of the drawing.

[0156] Figure 1aThe embodiment of the electrochemical cell 0 shown in does not have a separate flow distributor or a separate porous transport layer (PTL) or a separate catalytically active catalyst layer. The anode 1 and the cathode 2 themselves assume the function of the PLT, since they consist of a porous sintered body that is also fluid conductive. However, the flow distributor can be incorporated into the end plate 4 (not shown). Therefore, the compartments of the cell only include the corresponding sintered bodies 1, 2. The sintered material includes nickel and iron. In the simplest case, the material constituting the grains is stainless steel, which generally includes nickel and iron. In the operation of the cell, the oxidation of nickel and iron forms a catalytically active mixed Ni-Fe oxide or mixed Ni-Fe hydroxide. Therefore, the sintered material is catalytically active; no additional catalyst layer is required.

[0157] The electrochemical cell 0 allows three operation modes: wet, semi-dry case 1 and semi-dry case 2.

[0158] Figure 1b Schematically shows Figure 1a The operation of the electrochemical cell in the wet process variant. Here, in the electrolytic operation, the anode 1 and the cathode 2 are immersed in water or an alkaline electrolyte and permeated therewith.

[0159] Figure 1c A semi-dry variant is shown, in which only the Figure 1a The anode 1 of the electrochemical cell 0 is immersed in water or an alkaline electrolyte and permeated therewith (semi-dry case 1). The cathode 2 remains dry.

[0160] Figure 1d A semi-dry variant is shown, in which only the Figure 1a The cathode 2 of the electrochemical cell 0 is immersed in water or an alkaline electrolyte and infiltrated therewith (semi-dry case 2). The anode 1 remains dry.

[0161] Figure 2a A cross section of a design of a second embodiment of an electrochemical cell 0 is shown in schematic form. The electrochemical cell 0 comprises an anode 1, a cathode 2 and an anion conducting membrane 3 arranged between the anode 1 and the cathode 2. Both the anode 1 and the cathode 2 are implemented as porous sintered bodies consisting of nickel-containing grains. The membrane 3 is a flat membrane made of an anion conducting ionomer, which divides the cell 0 into two compartments. The two electrodes (anode 1 and cathode 2) are directly adjacent to the membrane 3. The sides of the anode 1 and the cathode 2 away from the membrane 3 are each in contact with an end plate 4.

[0162] The second embodiment is characterized in that a catalyst layer 5 is arranged between the cathode 2 and the membrane 3. The catalyst layer 5 may be applied to the cathode 2 and / or to the cathode side of the membrane 3. The catalyst layer 5 is therefore present in the cathode compartment. The catalyst layer 5 comprises catalytically active particles (electrocatalysts) fixed on the cathode 2 or the membrane 3 with an ionomer. The catalytically active particles are metal particles or alloys or coatings or compounds containing Au, Pt, Rh, Ru, Pd, Ag, Ni, Co, Cu, Fe, Mn, Mo, such as sulfides, selenides, oxides, mixed oxides, hydroxides, mixed hydroxides, spinels or perovskites, with a certain particle size or coating thickness of 1 nm to 10 μm. The catalytically active particles present in the catalyst layer 5 may be unloaded or loaded on a carbonaceous material, such as carbon black or charcoal, or loaded on an oxide, such as CeO2, TiO2 or WO3. Based on the membrane or electrode area (cathode 2), the concentration of the electrocatalyst is 0.01 mg / cm 2 Up to 25mg / cm 2 , preferably 0.05 mg / cm 2 Up to 5mg / cm 2 The thickness of the particle-containing catalyst layer is 1 μm to 500 μm, preferably 5 μm to 100 μm. The ionomer is the same material from which the membrane 3 is made. When the catalyst layer 5 is applied to the membrane 3, the resulting structure is a "catalyst-coated membrane" (CCM). If the catalyst layer 5 is applied to the cathode 2, the resulting structure is a "catalyst-coated substrate" (CCS). Figure 2a In the schematic presentation, it is not possible to determine whether a CCM or CCS variant is depicted.

[0163] Figure 2a The electrochemical cell 0 also allows three operation modes: wet, semi-dry case 1 and semi-dry case 2.

[0164] Figure 2b A wet variant is shown, in which the anode 1 and the cathode 2 are immersed in water or an alkaline electrolyte and impregnated with it in electrolytic operation.

[0165] Figure 2c A semi-dry variant is shown, in which only the anode 1 is immersed in water or an alkaline electrolyte and permeated therewith during electrolysis operation (semi-dry case 1). The cathode 2 remains dry.

[0166] Figure 2d A semi-dry variant is shown, in which only the cathode 2 is immersed in water or an alkaline electrolyte and permeated therewith during electrolysis operation (semi-dry case 2). The anode 1 remains dry.

[0167] Figure 3A first embodiment of a wet-operating electrolysis cell 6 is shown in schematic form. The electrolysis cell 6 comprises two adjacent electrochemical cells 0 according to the first embodiment, which are of identical construction and are contacted via a common bipolar plate 7 .

[0168] In order to carry out water electrolysis with the first electrolyzer 6, all electrodes are continuously immersed in water or alkaline electrolyte and infiltrated with it during the electrolysis operation. This mode of operation corresponds to the above-mentioned "wet" method variant, because all sintered bodies are immersed in water or alkaline electrolyte and infiltrated with it. Then a voltage acting between the anode 1 and the cathode 2 is applied to each cell. According to the above-mentioned principle, the effect is water electrolysis and the associated release of hydrogen (H2) in the porous sintered body forming the cathode 2 and the release of oxygen (O2) in the porous sintered body forming the anode 1. Oxygen (O2), hydrogen (H2) and undecomposed water (H2O) or alkaline electrolyte are discharged from the anode 1 and the cathode 2 accordingly, and water or alkaline electrolyte is continuously pumped through the anode 1 and the cathode 2.

[0169] Figure 4 A second embodiment of an electrolysis cell 8 in operation is shown in schematic form. The second electrolysis cell 8 comprises two adjacent electrochemical cells 0 according to the second embodiment, which have the same construction and are contacted via a common bipolar plate 7 .

[0170] In order to carry out water electrolysis with the second electrolyzer 8, all electrodes are immersed in water or alkaline electrolyte and infiltrated with it during the electrolysis operation. This mode of operation corresponds to the above-mentioned "wet" method variant, because the two sintered bodies are immersed in water or alkaline electrolyte. Then, a voltage acting between the anode 1 and the cathode 2 is applied to each cell. According to the above-mentioned principle, the effect is water electrolysis and the associated release of hydrogen (H2) in the porous sintered body forming the cathode 2 and the release of oxygen (O2) in the porous sintered body forming the anode 1. Oxygen (O2), hydrogen (H2) and undecomposed water (H2O) or alkaline electrolyte are discharged from the anode 1 and the cathode 2, respectively, and water or alkaline electrolyte is continuously pumped through the anode 1 and the cathode 2.

[0171] experiment

[0172] The effects achieved by the present invention will now be demonstrated with reference to experimental data. For this purpose, a porous sintered body was used as the anode material in an electrolysis test cell for AEM water electrolysis. For comparison, nickel foam was used as the anode material.

[0173] 1. Preparation of ionomers (not part of this invention)

[0174] The anion conducting polymer was synthesized according to Example 3 of EP3770201A1.

[0175] 2. Preparation of anion conducting membranes (not part of the present invention)

[0176] Then, membranes were prepared using the anion-conducting polymer synthesized in 1 as described in Example 4 of EP 3770201 A1. A fresh piece of membrane was used for each experiment, which had been ion-exchanged in 1 M KOH at 60° C. for 24 hours.

[0177] 3. Preparation of active test cathodes (not part of this invention)

[0178] The ink was prepared from platinum-coated carbon (60 wt. % platinum on carbon support, product number AB204745, abcr GmbH, Germany). This was achieved by first adding 44 parts of water, then 44 parts of ethanol and finally 5 parts of ionomer solution (5% solution of the ionomer prepared in 1. in DMSO) per part by weight of platinum-based catalyst, and then shaking the ink and dispersing it by ultrasonic treatment for 30 minutes.

[0179] To prepare the cathode, a carbon fiber nonwoven (TGP-H120, thickness = 370 μm, porosity = 78%, sample name "carbon fiber nonwoven", Toray Industries Inc., Japan) was selected as the substrate. The substrate was coated with the Pt / C-containing ink prepared as described above using a Prism 400 ultrasonic sprayer (from Ultrasonic Systems, Inc, Haverhill, MA, USA). The loading of platinum (Pt) was 0.6 mg / cm 2 .

[0180] 4. Determination of electrolytes in test cells

[0181] The schematic diagram of the electrolyte test cell is as follows Figure 2a All working examples are implemented in an electrochemical cell 0, which consists of an anode 1, a cathode 2, a membrane 3 and two active areas of 16 cm 2 The cathode 3 is composed of an end plate 4. One component of the cathode 3 is the above-mentioned catalyst coating 5. Therefore, the cathode 3 is a catalyst-coated substrate (CCS).

[0182] The end plate 4 has a flow field in the form of elongated channels 1.5 mm wide, each channel having an inlet and an outlet ( Figure 2a not shown).

[0183] The electrolyte used was 1 M KOH, which was pumped at a rate of 50 mL / min through the anode 1 and cathode 2. All experiments were performed at 60° C. after the electrolyte reached thermal equilibrium. Each specific feature of the corresponding working example is explained separately.

[0184] Embodiment 1 (present invention)

[0185] Here, a porous sintered body (steel SAE 316L, thickness = 1.57 mm, porosity = 38%, sample name "sintered body") was used as anode without further catalyst coating. The sintered body simultaneously served as porous transport layer and active (anode) catalyst material. Figure 5 The current-voltage curve recorded when using the electrolytic test cell is shown.

[0186] Figure 5 : Current-voltage curve in Example 1

[0187] It can be seen that using the sintered body without an additional anode-side catalyst coating enables a maximum current of 1.5 A / cm2 at a voltage below 1.9 V. 2 This implies high efficiency for industrial use.

[0188] Example 2. (Not the present invention)

[0189] For this purpose, a nickel foam (product code: NI00-FA-000152, thickness = 1.6 mm, porosity = 95%, Goodfellow, USA, sample name "Foam") was used as anode without further catalyst coating. This sintered body simultaneously serves as porous transport layer and active (anode) catalyst material. Figure 6 The current-voltage curve recorded when the nickel foam anode is used is shown as a dotted line. The solid line is the current-voltage curve recorded when the sintered steel anode is used. Figure 5 The current-voltage curve.

[0190] Figure 6 : Current-voltage curves of Example 2 and Example 1

[0191] It can be seen that significantly higher voltages are achieved when using nickel foam (dashed line) than when using a sintered body (solid line). For example, here 1.5 A / cm is not reached until 2.15 V. 2 The current density is relatively high. This relatively high voltage means that the efficiency in use is very low. In industry, this means that more energy (>10%) is required to produce the same amount of hydrogen.

[0192] in conclusion

[0193] It is clear from the comparison of these two examples that the efficiency is significantly improved using the sintered body as anode material for AEM water electrolysis compared to the foam electrode.

[0194] Reference numerals list

[0195] 0 Electrochemical Cell

[0196] 1. First porous sintered body (anode)

[0197] 2. Second porous sintered body (cathode)

[0198] 3 Anion Conducting Membrane

[0199] 4 End plate

[0200] 5 Catalyst layer

[0201] 6 An electrolytic cell according to a first embodiment comprising two adjacent electrochemical cells contacted by a common bipolar plate 7

[0202] 7 Bipolar Plate

[0203] 8 An electrolytic cell according to a second embodiment comprising two adjacent electrochemical cells contacted by a common bipolar plate 7

[0204] H2O Water or alkaline electrolyte

[0205] H2 Hydrogen

[0206] O2 Oxygen

Claims

1. An electrochemical cell (0) for alkaline membrane water electrolysis, comprising an anode (1), a cathode (2) and an anion conducting membrane (3) arranged between the anode (1) and the cathode (2), characterized in that: The anode (1) is partially or completely implemented as a first porous sintered body (1), which contains grains fused together at their grain boundaries, and the first porous sintered body (1) is in direct contact with the membrane (3).

2. The electrochemical cell (0) according to claim 1, characterized in that The grains of the first porous sintered body (1) contain or consist of a catalytically active material, wherein the catalytically active material contains at least one transition metal selected from the list consisting of the following transition metals: Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Ac, Rf, Db, Sg, Bh, Hs, Mt, Ds, Rg.

3. The electrochemical cell (0) according to claim 1 or 2, characterized in that The crystal grains of the first porous sintered body (1) contain nickel.

4. The electrochemical cell (0) according to claim 3, characterized in that The grains of the first porous sintered body (1) are composed of a material selected from the group consisting of nickel, nickel-containing alloys, Hastelloy, Chronin, Monel, Inconel, Incoloy, Invar, Kovar; nickel-containing steel, nickel-containing stainless steel, and steels of AISI 301, AISI 301L, AISI 304, AISI 304L, AISI310, AISI310L, AISI316, AISI 316L, AISI 317, AISI 317L and AISI 321 grades.

5. The electrochemical cell (0) according to any one of claims 1 to 4, characterized in that No catalyst layer is provided between the first porous sintered body (1) and the membrane (3).

6. The electrochemical cell (0) according to any one of claims 1 to 5, characterized in that The porosity P of the first porous sintered body (1) is 5% to 60% or 15% to 45%, wherein the porosity P is determined according to the following formula: P=1-ρ V / r M where ρ V is the volume density of the first porous sintered body (1), ρ M is the solid density of the grains of the first porous sintered body (1).

7. The electrochemical cell (0) according to claim 6, characterized in that The porosity P varies along a gradient, wherein the gradient is arranged perpendicular to the interface between the first porous sintered body (1) and the membrane (3) and wherein the porosity P decreases in the direction of the membrane (3).

8. The electrochemical cell (0) according to claims 1 to 7, characterized in that As evaluated in a cross-sectional view by an optical microscope, the pores of the first porous sintered body (1) are smaller than the grains of the first porous sintered body (1).

9. The electrochemical cell (0) according to claims 1 to 8, characterized in that The cathode (2) is partially or completely implemented as a second porous sintered body (2), which contains grains fused together at their grain boundaries.

10. The electrochemical cell (0) according to claim 9, characterized in that The grains of the second porous sintered body (2) contain or consist of a catalytically active material, wherein the catalytically active material contains at least one transition metal selected from the list consisting of the following transition metals: Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Ac, Rf, Db, Sg, Bh, Hs, Mt, Ds, Rg.

11. The electrochemical cell (0) according to claim 9 or 10, characterized in that The crystal grains of the second porous sintered body (2) contain nickel.

12. The electrochemical cell (0) according to claim 11, characterized in that The grains of the second porous sintered body (2) are composed of a material selected from the group consisting of nickel, nickel-containing alloys, Hastelloy, Chronin, Monel, Inconel, Incoloy, Invar, Kovar; nickel-containing steel, nickel-containing stainless steel, and steels of AISI 301, AISI 301L, AISI 304, AISI 304L, AISI310, AISI310L, AISI316, AISI 316L, AISI 317, AISI 317L and AISI 321 grades.

13. The electrochemical cell (0) according to any one of claims 1 to 12, characterized in that A catalyst layer (5) is arranged between the cathode (2) and the membrane (3).

14. The electrochemical cell (0) according to claim 13, characterized in that The catalyst layer (5) comprises at least one element selected from the group consisting of the following elements or a compound of the elements: Pt, Ru, Pd, C, Ni, Mo, Co, Cu, Fe, Cr.

15. The electrochemical cell (0) according to claim 13 or 14, characterized in that The catalyst layer (5) comprises an anion-conducting polymer.

16. The electrochemical cell (0) according to claim 15, characterized in that The anion-conducting polymer comprises repeating units which are also comprised in the membrane (3).

17. The electrochemical cell (0) according to any one of the preceding claims 1 to 16, characterized in that The first porous sintered body (1) and / or the second porous sintered body (2) is in contact with the bipolar plate (7) at a side away from the membrane (3).

18. The electrochemical cell (0) according to claim 17, characterized in that The bipolar plate (7) is composed of a material selected from the following: nickel; nickel-containing alloys, Hastelloy, Chronin, Monel, Inconel, Incoloy, Invar, Kovar; nickel-containing steel, nickel-containing stainless steel, steel of AISI 301, AISI 301L, AISI 304, AISI 304L, AISI 310, AISI310L, AISI316, AISI 316L, AISI 317, AISI 317L and AISI 321 grades; nickel-plated steel, nickel-plated stainless steel, nickel-plated titanium, nickel-plated brass, nickel-plated aluminum, nickel-plated acrylonitrile-butadiene-styrene copolymer, and carbon.

19. A method for producing hydrogen (H2) and oxygen (O2) by electrochemical decomposition of water (H2O), comprising the following steps: a) providing at least one electrochemical cell (0) according to any one of claims 1 to 18; b) providing an aqueous electrolyte having a pH of 7 to 15; c) providing a voltage source; d) bringing the first porous sintered body (1) and / or the cathode (2) into contact with the electrolyte; e) applying a voltage obtained from the voltage source to the anode (1) and the cathode (2); f) discharging oxygen (O2) and / or an electrolyte in which oxygen (O2) is dissolved from the first porous sintered body (1); g) discharging hydrogen gas (H2) and / or an electrolyte in which hydrogen gas (H2) is dissolved from the electrochemical cell (0); h) optionally separating oxygen (O2) from the electrolyte discharged from the first porous sintered body (1); i) optionally separating hydrogen (H2) from the electrolyte discharged from the electrochemical cell (0).

20. Electrolysis cell (6, 8) for carrying out the method according to claim 19, comprising at least two electrochemical cells (0) according to claim 17 sharing a common bipolar plate (7).

21. A method for producing an electrolytic cell (6, 8) according to claim 20, in which the following components are stacked directly one after the other in the following order: a) a first porous sintered body (1); b) anion conducting membrane (3); c) an optional catalyst layer (5); d) cathode (2); e) bipolar plate (7); f) a first porous sintered body (1); g) anion conducting membrane (3); h) an optional catalyst layer (5); i) Cathode (2).

22. A method for producing an electrolytic cell (6, 8) according to claim 20, in which the following components are stacked directly one after the other in the following order: a) cathode (2); b) an optional catalyst layer (5); c) anion conducting membrane (3); d) a first porous sintered body (1); e) bipolar plate (7); f) cathode (2); g) an optional catalyst layer (5); h) anion conducting membrane (3); j) A first porous sintered body (1).

23. Use of the electrochemical cell (0) according to any one of claims 1 to 16 in alkaline membrane water electrolysis.