Anode catalyst for proton exchange membrane electrolytic cell as well as synthesis method and application of anode catalyst
By optimizing the reaction conditions between iridium precursor and alkaline substances, a highly active and easily dispersed iridium oxide catalyst was prepared, which solved the problems of slow kinetics and high cost of the anode catalyst, improved the electrolytic activity and specific surface area, and promoted the protons Commercialization of exchange membrane electrolytic cell technology.
Patent Information
- Application Number
- CN202411011793.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
AI Technical Summary
The kinetics of existing proton exchange membrane electrolytic cell anode catalysts are slow, resulting in high voltage and expensive cost. In particular, the scarcity and high price of iridium oxide catalysts have become technical bottlenecks in commercialization.
By optimizing the reaction conditions of the iridium precursor and alkaline substances, including adjusting the pH value, adding small molecule solvents and calcining temperature, a uniform, small particle size and easy dispersion iridium oxide catalyst is prepared to improve its specific surface area and electrolytic activity.
It reduces the cost of the catalyst, improves its dispersion and electrolytic activity, overcomes the problem of slow kinetics, and promotes the commercialization of proton exchange membrane electrolytic cell technology.
Smart Images

Figure CN118957632A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of proton exchange membrane (PEM) electrolyzers, and in particular relates to an anode catalyst for a proton exchange membrane electrolyzer, a synthesis method and application thereof. Background Art
[0002] The PEM electrolyzer is a device that converts electrical energy into chemical energy. The water on the anode side undergoes an oxidation reaction with water on the surface of the proton exchange membrane through the voltage of the external circuit to generate oxygen, which is called the oxygen evolution reaction (OER). At the same time, the protons or hydrated protons generated migrate to the cathode to undergo a reduction reaction to generate hydrogen, which is called the hydrogen evolution reaction (HER). This method of preparing hydrogen by electrolyzing water has the advantages of rapid response, high current density, good self-consistency with renewable energy, and high purity of the generated gas, and has therefore received widespread attention from the society.
[0003] At present, the membrane electrode is one of the core components of the PEM electrolyzer. The membrane electrode is composed of a cathode, an anode catalyst layer and a proton exchange membrane. Since the anode OER is a four-electron reaction process, the kinetics are slow, resulting in a high anode voltage, which has also become a technical bottleneck for the PEM electrolyzer. Commonly used PEM water electrolysis anode catalysts include iridium oxide and ruthenium oxide. Due to the poor stability of ruthenium oxide, current commercial catalysts usually use iridium oxide. The abundance of iridium oxide is very small, which makes it expensive, which is also an important factor limiting the commercialization of PEM electrolyzers. Therefore, the OER activity of the anode catalyst is extremely important. Only by preparing a catalyst with a small particle size and easy dispersion can the specific surface area be increased, more active sites can be exposed, and the intrinsic activity of the catalyst can be exerted, which plays a key role in the potential of the entire PEM electrolyzer. Summary of the invention
[0004] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a proton exchange membrane electrolysis cell anode catalyst and a synthesis method and application thereof. The purpose of the present invention is to propose a highly active and easily dispersible synthesis method for a proton exchange membrane water electrolysis anode catalyst, which can not only obtain a uniform, small particle size, and high intrinsic activity iridium oxide catalyst, but also has a simple method and low cost.
[0005] In order to achieve the above technical objectives, the technical solution adopted by the embodiment of the present invention is:
[0006] In a first aspect, an embodiment of the present invention provides a method for synthesizing an anode catalyst of a proton exchange membrane electrolyzer, comprising the following steps:
[0007] Step S1, adding an iridium precursor to a mixture of deionized water and a small molecule solvent to obtain an iridium precursor solution;
[0008] Step S2, adding a certain amount of alkaline substance to the iridium precursor solution of step S1, adjusting the pH value to 8-14, heating to 50-100° C. and stirring evenly;
[0009] Step S3, drying the mixture in step S2, and placing it in a muffle furnace for calcination;
[0010] Step S4, repeatedly washing the solid obtained in step S3 for multiple times, and drying to obtain an iridium oxide catalyst.
[0011] Further, the small molecule solvent includes one or more of ethanol, isopropanol, acetic acid, ethylene glycol and n-propanol;
[0012] The volume content of the small molecule solvent in the solvent of step S1 is 10-30%.
[0013] Furthermore, in step S3, the drying time is 3-10 hours, the calcination temperature is 200-600° C., and the calcination time is 0.5-3 hours.
[0014] Furthermore, the alkaline substance includes one or more of sodium hydroxide, potassium hydroxide or lithium hydroxide.
[0015] In a second aspect, an embodiment of the present invention provides an anode catalyst for a proton exchange membrane electrolyzer, which is prepared by the synthesis method described in the first aspect.
[0016] In a third aspect, an embodiment of the present invention provides use of the catalyst described in the second aspect in an anode of a proton exchange membrane electrolyzer.
[0017] The technical solution provided by the embodiment of the present invention has the following beneficial effects:
[0018] (1) The present invention optimizes the synthesis process of iridium oxide catalyst: by regulating the reaction conditions of alkali solution and sodium chloroiridate, including feed ratio, solvent composition, reaction temperature, etc., the dispersibility and electrolytic water activity of iridium oxide catalyst are improved, and the cost is reduced. This optimization is to overcome the scarcity and high price of expensive materials such as iridium oxide, thereby promoting the commercialization of proton exchange membrane electrolyzer technology.
[0019] (2) The present invention optimizes the reaction temperature: After adding a small molecule solvent to water, the reaction temperature of the catalyst can be increased and the dispersibility of the catalyst can be improved.
[0020] (3) Control of catalyst particle size: Different solvents have different effects on the prepared catalyst particle size.
[0021] (4) Impact on catalyst yield: When the reaction temperature increases, the catalyst yield also increases to a certain extent.
[0022] (5) Research on solvents: In addition to water, one or more solvents including ethanol, isopropanol, acetic acid, ethylene glycol, and n-propanol were added during the catalyst synthesis process. It was found that this had an impact on improving catalyst activity, reaction efficiency, and dispersibility. This idea may provide a new direction and reference for improving other catalyst synthesis processes in the future.
[0023] (6) Improving the OER activity of the catalyst: By preparing a catalyst with a small particle size and easy dispersion, the specific surface area of the catalyst is increased, exposing more active sites, thereby exerting the intrinsic activity of the catalyst. This method plays an important role in overcoming the problem of slow OER kinetics and reducing the anode voltage.
[0024] Overall, these innovative practices and research directions provide new ideas and approaches for solving key problems in proton exchange membrane electrolyzer technology, and are expected to promote scientific research and technological development in this field. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a linear scan diagram of Examples 1-4 of the present invention tested in a three-electrode system.
[0026] Figure 2 This is a high-resolution transmission electron microscopy image of the iridium oxide catalyst obtained in Example 2 of the present invention.
[0027] Figure 3 It is a linear scanning diagram of comparative examples 1-4 of the present invention tested in a three-electrode system. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0029] Example 1
[0030] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer comprises the following steps:
[0031] Step S1, adding 0.01 mol of sodium chloroiridate into 100 mL of a solvent formed by deionized water and ethylene glycol, wherein the volume of the ethylene glycol solution is 10 mL;
[0032] Step S2, adding 3 g of sodium hydroxide to the sodium chloroiridate solution of step S1, heating to 80° C. and stirring evenly;
[0033] Step S3, drying the mixture in step S2, placing it in a muffle furnace and calcining it at 200° C. for 2 hours;
[0034] Step S4: The solid obtained in step S3 was repeatedly washed 5 times with deionized water and dried in an oven at 80° C. to obtain 2.1 g of iridium oxide catalyst.
[0035] Example 2
[0036] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer comprises the following steps:
[0037] Step S1, adding 0.02 mol of sodium chloroiridate into 200 mL of a solvent formed by deionized water, ethanol, n-propanol and acetic acid, wherein the volumes of ethanol, n-propanol and acetic acid are all 20 mL;
[0038] Step S2, adding 5 g of sodium hydroxide to the sodium chloroiridate solution of step S1, heating to 80° C. and stirring evenly;
[0039] Step S3, drying the mixture in step S2, placing it in a muffle furnace and calcining it at 300° C. for 1.5 h;
[0040] Step S4: Wash the solid in step S3 repeatedly with deionized water for 5 times, and dry it in an oven at 80° C. to obtain 4.3 g of iridium oxide catalyst.
[0041] Example 3
[0042] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer comprises the following steps:
[0043] Step S1, adding 0.03 mol of sodium chloroiridate into 300 mL of a solvent formed by deionized water, ethylene glycol, isopropanol and n-propanol, wherein the volumes of ethylene glycol, isopropanol and n-propanol are all 30 mL;
[0044] Step S2, adding 8 g of sodium hydroxide to the sodium chloroiridate solution of step S1, heating to 80° C. and stirring evenly;
[0045] Step S3, drying the mixture of step S2, placing it in a muffle furnace and calcining it at 400° C. for 1 hour;
[0046] Step S4: Wash the solid in step S3 repeatedly with deionized water for 5 times, and dry it in an oven at 80° C. to obtain 6.5 g of iridium oxide catalyst.
[0047] Example 4
[0048] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer comprises the following steps:
[0049] Step S1, adding 0.04 mol of sodium chloroiridate into 400 mL of a solvent formed by deionized water, acetic acid and ethylene glycol, wherein the volume of the acetic acid and the volume of the ethylene glycol are both 40 mL;
[0050] Step S2, adding 10 g of sodium hydroxide to the sodium chloroiridate solution of step S1, heating to 80° C. and stirring evenly;
[0051] Step S3, drying the mixture obtained in step S2, placing it in a muffle furnace and calcining it at 500° C. for 1 hour;
[0052] Step S4: The solid in step S3 was repeatedly washed 5 times with deionized water and dried in an oven at 80° C. to obtain 8.8 g of iridium oxide catalyst.
[0053] Comparative Example 1
[0054] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer is disclosed. Except that ethylene glycol is not added in step S1, the remaining steps are the same as those of the corresponding embodiment 1, and 1.9 g of the catalyst is obtained.
[0055] Comparative Example 2
[0056] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer comprises the following steps:
[0057] Step S1, adding 0.02 mol of sodium chloroiridate into 200 mL of a solvent formed by deionized water, ethanol, n-propanol and acetic acid, wherein the volumes of ethanol, n-propanol and acetic acid are all 50 mL;
[0058] The other steps were the same as in Example 2 to obtain 4 g of catalyst.
[0059] Comparative Example 3
[0060] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer comprises the following steps:
[0061] Step S1, adding 0.03 mol of sodium chloroiridate into 300 mL of a solvent formed by deionized water, ethanol, isopropanol and acetone, wherein the volume of ethanol, isopropanol and acetone is 30 mL each;
[0062] The other steps were the same as those in Example 3, and 6.2 g of iridium oxide catalyst was obtained.
[0063] Comparative Example 4
[0064] A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer is provided. 5 g of sodium hydroxide is added in step S2, and the other steps are the same as those in Example 4, to obtain 7 g of iridium oxide catalyst.
[0065] The physical properties and electrochemical tests of the catalysts prepared in Examples 1-4 and Comparative Examples 1-4 were carried out. The electrochemical tests were carried out in a three-electrode system, and the activity was mainly observed at a current density of j = 10 mA cm -2 The overpotential η, the specific values are shown in Table 1. The smaller η is, the higher the oxygen evolution activity of the catalyst is, which is more conducive to improving the efficiency of water electrolysis. It can be seen from Table 1 that compared with Comparative Examples 1-4, the iridium oxide catalysts prepared in Examples 1-4 of the present invention have higher oxygen evolution activity in water electrolysis.
[0066] Table 1 Oxygen evolution overpotential and yield values of catalysts in Examples 1-4 and Comparative Examples 1-4
[0067]
[0068] like Figure 1 As shown, by comparing Examples 1-4, it is found that when one or more of ethanol, isopropanol, acetic acid, ethylene glycol, and n-propanol are added to the solvent in addition to water, the oxygen evolution overpotential of iridium oxide is between 270-280 mV, and the activity does not change significantly. Figure 2 The high-resolution transmission electron microscopy image shows that the particle size of the catalyst is about 3nm and is evenly dispersed. When no solvent other than water is added in Comparative Example 1, the activity of the catalyst decreases, which shows that one or more solvents selected from ethanol, isopropanol, acetic acid, ethylene glycol, and n-propanol have a positive effect on the synthesis of iridium oxide. At the same time, in Comparative Example 2, when an excess of additional solvent is added, the oxygen evolution activity of the iridium oxide catalyst will decrease. Comparative Example 3 can prove that acetone does not have a positive effect on catalyst synthesis compared to several other solvents. When the amount of alkali in Comparative Example 4 is appropriately decreased, the catalyst activity is slightly improved, but the output will decrease, which may be due to the insufficient reaction of the iridium precursor, which leads to an increase in cost.
[0069] In summary, when adding appropriate amounts of one or more ethanol, n-propanol, isopropanol, ethylene glycol and acetic acid, the yield of the iridium oxide catalyst and its water electrolysis activity can be effectively improved, the catalyst particle size can be reduced, and the exposure of the catalyst active sites can be increased to improve the oxygen evolution activity of iridium oxide.
[0070] The iridium oxide catalyst of the present invention is obtained by reacting alkali solution with sodium chloroiridate and then calcining. During the reaction, the reaction conditions of the alkali solution and sodium chloroiridate have a great influence on the synthesis of iridium oxide, such as the feed ratio of alkali to iridium, the solvent composition during the reaction, the reaction temperature, etc. The present invention improves the OER activity and yield of the catalyst by optimizing the appropriate reaction conditions, and can effectively reduce the cost of electrolyzing water.
[0071] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for synthesizing an anode catalyst for a proton exchange membrane electrolyzer, It is characterized in that The following steps are involved: Step S1, adding an iridium precursor to a mixture of deionized water and a small molecule solvent to obtain an iridium precursor solution; Step S2, adding a certain amount of alkaline substance to the iridium precursor solution of step S1, adjusting the pH value to 8-14, heating to 50-100° C. and stirring evenly; Step S3, drying the mixture in step S2, and placing it in a muffle furnace for calcination; Step S4, repeatedly washing the solid obtained in step S3 for multiple times, and drying to obtain an iridium oxide catalyst.
2. The method for synthesizing the anode catalyst of the proton exchange membrane electrolyzer according to claim 1, It is characterized in that The small molecule solvent includes one or more of ethanol, isopropanol, acetic acid, ethylene glycol and n-propanol; The volume content of the small molecule solvent in the solvent mixture of step S1 is 10-30%.
3. The method for synthesizing the anode catalyst of the proton exchange membrane electrolyzer according to claim 1, It is characterized in that In step S3, the drying time is 3-10 h, the calcination temperature is 200-600° C., and the calcination time is 0.5-3 h.
4. The method for synthesizing the anode catalyst of the proton exchange membrane electrolyzer according to claim 1, It is characterized in that The alkaline substance includes one or more of sodium hydroxide, potassium hydroxide or lithium hydroxide.
5. A proton exchange membrane electrolyzer anode catalyst, It is characterized in that The compound is prepared by the synthesis method according to any one of claims 1 to 4.
6. Use of the catalyst according to claim 5 in an anode of a proton exchange membrane electrolyzer.