Composite iridium oxide / iridium carrier type oxygen evolution electrocatalyst and preparation method thereof

By loading a composite iridium oxide/iridium support-type oxygen precipitation electrocatalyst with conductive metal nanoiridium layer and iridium oxide layer on the nanoparticle support, the problems of high cost of precious metal iridium and poor catalyst stability are solved, and high conductivity and excellent Electrocatalytic oxygen evolution performance, suitable for large-scale application of PEM hydrogen production technology.

CN118957657APending Publication Date: 2024-11-15BEIJING DYNAMIC HYDROGEN NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411012265.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the existing PEM hydrogen production technology, the high cost of precious metal iridium and its high load in the membrane electrode oxygen evolution catalytic layer seriously limits the rapid development and large-scale application of the technology, especially in a highly acidic and high voltage oxidation environment. Under the following, the catalyst is prone to irreversible deep surface reconstruction, resulting in problems of loss of active components and low conductivity.

Method used

Using a composite iridium oxide/iridium support type oxygen precipitation electrocatalyst, the conductive metal nanoiridium layer and iridium oxide layer are uniformly supported on the nanoparticle support, the iridium loading is 20 wt.% to 80 wt.%, and the conductive metal nanoiridium layer is composed of 2 The iridium metal nanoparticles of ~3 nm are composed of titanium dioxide, titanium nitride, etc. The conductivity and stability of the catalyst are improved by specific preparation methods.

Benefits of technology

Achieve high conductivity composite iridium oxide/iridium support type oxygen precipitation electrocatalyst, which significantly improves the conductivity and stability of the catalyst, reduces ohmic impedance loss, has excellent electrocatalytic oxygen evolution performance, has a wide range of applications, and is suitable for many This type of carrier has simple synthesis technology and high repeatability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957657A_ABST
    Figure CN118957657A_ABST
Patent Text Reader

Abstract

The invention discloses a composite iridium oxide / iridium carrier type oxygen evolution electrocatalyst and a preparation method thereof, and belongs to the technical field of hydrogen production by electrocatalytic decomposition of water. The oxygen evolution electrocatalyst structurally comprises a nano-particle carrier, a conductive metal nano-iridium layer coated on the surface of the carrier and an active iridium oxide layer further coated on the surface of the carrier. A hydrate chloroiridic acid and a carrier are fully mixed in an organic solvent, and controllable growth of a conductive metal nano iridium layer on the surface of the carrier is realized under heating and stirring conditions; and further fully mixing with iridium chloride hydrate and sodium hydroxide according to a certain proportion, and obtaining the high-conductivity composite iridium oxide / iridium carrier type oxygen evolution electrocatalyst under the reaction conditions of heating, stirring and subsequent calcination. The oxygen evolution electrocatalyst shows excellent electrocatalytic oxygen evolution reaction performance in an acidic electrolyte, the preparation method is simple in process and high in universality, and the oxygen evolution electrocatalyst is suitable for various carriers and has huge application potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrocatalytic water decomposition to produce hydrogen, relates to a catalyst for oxygen evolution by water electrolysis, and specifically relates to a composite iridium oxide / iridium carrier type oxygen evolution electrocatalyst and a preparation method thereof. Background Art

[0002] As the consumption of fossil fuels leads to a decrease in their reserves, and environmental pollution and climate warming become increasingly prominent, there is an urgent need to develop new clean energy with abundant reserves that does not rely on fossil fuels. Hydrogen energy, as a green and zero-carbon secondary energy source, is an important carrier for achieving carbon neutrality and carbon peak and building a low-carbon clean energy field. Proton exchange membrane water electrolysis (PEM) hydrogen production technology has the advantages of high efficiency, environmental protection, high current density, high hydrogen purity and high flexibility, and easy coupling with renewable energy power. It has gradually become a key technology in the field of green hydrogen preparation. PEM hydrogen production mainly includes two types of electrode half reactions, namely the anode side oxygen evolution reaction (OER) and the cathode side hydrogen evolution reaction (HER). Among them, the OER reaction occurs in a strongly acidic and high-voltage oxidative working environment. At present, only iridium-based catalysts (generally iridium dioxide catalysts) can achieve relatively balanced activity and stability under these harsh conditions, becoming the commercial anode catalyst for the current PEM water electrolysis technology. However, the high cost of precious metal iridium and its high loading in the membrane electrode oxygen evolution catalytic layer have seriously restricted the rapid development and large-scale application of PEM hydrogen production technology.

[0003] Developing supported catalysts is an effective strategy to reduce the amount of precious metal iridium and improve its OER catalytic mass activity. The support helps to disperse the catalytic active components to reduce the loading. At the same time, the electronic synergy between the two helps to stabilize the anchoring behavior of the catalyst layer on the support surface and improve the stability of the catalyst. These supports usually have extremely low electrical conductivity, and the active catalytic layer needs to be evenly and completely coated on its surface to improve the conductivity and reduce the ohmic impedance loss in the PEM hydrogen production device. However, under the operating conditions of the electrolyzer, the catalyst is prone to irreversible deep surface reconstruction, resulting in the loss of active components and then converted into a low-activity and low-conductivity oxide deactivated material.

[0004] Therefore, how to controllably load the highly stable active iridium oxide component evenly on the carrier surface and significantly improve the catalyst conductivity becomes a difficulty in developing low-loading and high-performance anode catalyst materials. Summary of the invention

[0005] In view of this, the present invention intends to provide a high-conductivity composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst and a preparation method thereof.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] A composite iridium oxide / iridium carrier type oxygen evolution electrocatalyst is used for the anode reaction of electrolyzing water to produce hydrogen. The electrocatalyst comprises a nanoparticle carrier with a stable structure in a strongly acidic and oxidizing environment, a conductive metal nano-iridium layer coated on the surface of the carrier and an iridium oxide layer further coated on the surface thereof, wherein the iridium loading is 20wt.% to 80wt.%, that is, the iridium element occupies 20% to 80% of the total mass of the oxygen evolution electrocatalyst.

[0008] Furthermore, the conductive metal nano-iridium layer is composed of iridium metal nano-particles with a size of about 2 to 3 nm, and is preferably a single-layer structure, that is, the conductive metal nano-iridium layer has a thickness of 2 to 3 nm.

[0009] Furthermore, the carrier is at least one of titanium dioxide, titanium nitride, niobium pentoxide and tantalum pentoxide, and the carrier is usually in the form of rod-shaped or spherical nanoparticles with a particle size of 20 to 100 nm.

[0010] Preferably, the iridium oxide layer has a thickness of 2 to 3 nm.

[0011] The composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst has high electrical conductivity, which is due to the fact that the composite components of highly conductive metal iridium and active iridium oxide are uniformly loaded on the carrier surface without any independent carrier exposure.

[0012] The present invention also provides a method for preparing the composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst, which specifically comprises the following steps:

[0013] (1) Preparation of the first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier

[0014] The hydrated chloroiridic acid (H 2 IrCl 6 6H 2 O) and carrier powder are uniformly mixed in an organic solvent, then heated to a reaction temperature of 150-200° C. and stirred for reaction for 2-20 hours. After the reaction is completed, the mixture is cooled to room temperature, centrifuged and precipitated, and washed to obtain a first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier.

[0015] (2) Preparation of the second precursor of the electrocatalyst of iridium oxyhydroxide coated with a conductive metal nano-iridium layer carrier

[0016] The first electrocatalyst precursor prepared in step (1) is mixed with hydrated iridium tetrachloride (IrCl 4 ·xH 2O), sodium hydroxide (or potassium hydroxide) are dispersed in deionized water and stirred at room temperature for 1 to 12 hours; then the mixture is heated to a reaction temperature of 70 to 100°C and stirred for 4 to 24 hours, and then the heating and stirring are stopped; after the mixture is cooled to room temperature, it is centrifuged and precipitated, and washed to obtain the second precursor of the electrocatalyst of the iridium hydroxide-coated conductive metal nano-iridium layer carrier.

[0017] (3) Preparation of high conductivity composite iridium oxide / iridium support type oxygen evolution electrocatalyst

[0018] The second electrocatalyst precursor prepared in the above step (2) is mixed with sodium nitrate powder in proportion, and then fully ground; the ground mixture is further calcined at a temperature of 350 to 550° C. for 1 to 3 hours, and then cooled to room temperature; the obtained product is washed with deionized water, and dried to obtain a high-conductivity composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst.

[0019] Furthermore, the specific surface area of ​​the carrier selected in step (1) is preferably 10 m 2 / g~50m 2 / g.

[0020] Furthermore, in the above step (1), the organic solvent may be an alcohol solvent, such as diethylene glycol, benzyl alcohol, or ethylene glycol.

[0021] Furthermore, in the above step (1), the mass ratio of the hydrated chloroiridic acid to the carrier powder is preferably 2:1 to 1:11.

[0022] Furthermore, in the above step (1), after the reaction is completed and cooled, the mixture is centrifuged at 6000-10000 r / min, the precipitate is separated and washed twice with a mixed solution of water and ethanol to obtain the first electrocatalyst precursor.

[0023] Furthermore, in the above step (2), the mass ratio of the first electrocatalyst precursor to hydrated iridium tetrachloride is 3:1 to 1:5; the mass ratio of hydrated iridium tetrachloride to sodium hydroxide or potassium hydroxide is 3:1 to 4:1.

[0024] Furthermore, in the above step (2), after the reaction is completed and cooled, the mixture is centrifuged at 6000-10000 r / min, the precipitate is separated and washed twice with a mixed solution of water and ethanol to obtain the second electrocatalyst precursor.

[0025] Furthermore, in the above step (3), the second electrocatalyst precursor is mixed with sodium nitrate powder in a mass ratio of 1:10 to 1:50.

[0026] Furthermore, in the above step (3), the temperature is preferably raised to 350-550°C at a heating rate of 2-10°C / min for calcination. It should be noted that in the above step (2), under the conditions of the presence of hydroxide and heating and stirring, the iridium oxyhydroxide nanolayer can be controllably grown on the surface of the carrier.

[0027] Furthermore, the present invention provides an application of the above-mentioned high-conductivity composite iridium oxide / iridium support type oxygen evolution electrocatalyst in the anode oxygen evolution reaction of electrocatalytic water decomposition to produce hydrogen. According to experiments, it exhibits excellent electrocatalytic oxygen evolution (OER) performance in acidic electrolyte.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] (1) The composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst of the present invention has high conductivity, and its conductivity is 10.72S / cm at an implementation pressure of 30MPa. Its preparation method has good universality, is applicable to various types of carriers, has a simple synthesis process, high repeatability, and has a wider range of catalyst preparation applications.

[0030] (2) The composite iridium oxide / iridium carrier oxygen evolution electrocatalyst of the present invention has good catalytic activity, which is superior to the current commercial iridium oxide catalyst and can reach 10 mA / cm at an overpotential of 251 mV. 2 The current density is high and has great application potential. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a transmission electron microscope (TEM) image of the first precursor of the electrocatalyst prepared in Example 1, the surface of the carrier being coated with a conductive metal nano-iridium layer.

[0032] Figure 2 This is a transmission electron microscope (TEM) image of the composite iridium oxide / iridium support type oxygen evolution electrocatalyst prepared in Example 1.

[0033] Figure 3 This is the X-ray diffraction (XRD) spectrum of the composite iridium oxide / iridium support type oxygen evolution electrocatalyst prepared in Example 1.

[0034] Figure 4 This is the conductivity test result of the composite iridium oxide / iridium support type oxygen evolution electrocatalyst prepared in Example 1.

[0035] Figure 5 The polarization curve of the water electrolysis oxygen evolution reaction of the composite iridium oxide / iridium support type oxygen evolution electrocatalyst prepared in Example 1 and its comparison with the commercial IrO 2 comparison. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solutions and advantages of the present invention more clearly and completely described, they will be explained in detail in conjunction with exemplary embodiments below, but the protection scope required by the present invention is not limited to the following embodiments.

[0037] Embodiment 1

[0038] (1) Preparation of the first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier

[0039] 1.5 g of chloroiridic acid hydrate H 2 IrCl 6 6H 2 O and 1.2 g of titanium dioxide powder carrier were mixed in 400 mL of diethylene glycol solvent, wherein the specific surface area of ​​the titanium dioxide powder was 30 m 2 / g, can be subjected to ultrasonic and stirring treatment to prepare a metal precursor mixed solution; then, the stirred homogenized solution is heated to 180°C and continued to be stirred for 8h; after the solution is cooled to room temperature, it is centrifuged at 8000r / min for 10min, and then washed twice with water and ethanol solution in a volume ratio of 1:1, so as to obtain the first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier.

[0040] The TEM image of the prepared first electrocatalyst precursor is as follows: Figure 1 As shown, it can be seen that the surface of the carrier is composed of a uniformly coated single layer of metal iridium nanoparticles, and the particle size is uniform, showing a distribution of 2-3nm.

[0041] (2) Preparation of the second precursor of the electrocatalyst of iridium oxyhydroxide coated with a conductive metal nano-iridium layer carrier

[0042] Take 1.2 g of the first electrocatalyst precursor prepared in step (1) above and 0.8 g of hydrated iridium tetrachloride IrCl 4 ·xH 2 O, 0.6g sodium hydroxide NaOH is dispersed in deionized water, and the mixed solution is stirred at room temperature for 3h; then the mixture is heated to a reaction temperature of 80°C and stirred for 8h; after the solution is cooled to room temperature, it is centrifuged at 8000r / min for 10min, and then washed twice with water and ethanol solution in a volume ratio of 1:1 to obtain the second precursor of the electrocatalyst of the iridium hydroxide-coated conductive metal nano iridium layer carrier.

[0043] (3) Preparation of high conductivity iridium oxide / iridium support type oxygen evolution electrocatalyst

[0044] The second electrocatalyst precursor prepared in the above step (2) is mixed with sodium nitrate powder in a mass ratio of 1:10, and then fully ground; the ground mixture is heated to 375°C at a heating rate of 3°C / min and calcined for 1 hour, and then cooled to room temperature; the obtained product is washed with deionized water, and dried to obtain a high-conductivity iridium oxide / iridium titanium oxide support-type oxygen evolution electrocatalyst, wherein the mass of iridium element accounts for 50wt.% of the total mass of the electrocatalyst.

[0045] The TEM image of the prepared high conductivity composite iridium oxide / iridium support oxygen evolution electrocatalyst is shown in Figure 2 As shown in Figure 1, an active iridium oxide layer is uniformly loaded on the surface. The XRD pattern of the electrocatalyst is shown in Figure 1. Figure 3 As shown, the obtained material presents a coexistence state of the diffraction peak of the carrier (rutile titanium dioxide), the diffraction peak of metal nano-iridium and the broadened diffraction peak of the active iridium oxide layer, indicating the successful preparation of the composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst.

[0046] The conductivity test experiment was measured by a four-probe resistivity tester. First, the catalyst powder sample was pressed into a sheet, and the pressure range was set to 2.0MPa to 30.0MPa. Four electrodes were placed on the catalyst material and current was injected into the material. The resistivity was measured by measuring the voltage difference. The resistivity of the composite iridium oxide / iridium support type oxygen evolution electrocatalyst was measured to be 0.093Ωcm to 0.302Ωcm, and the conductivity was measured to be 3.31S / cm to 10.72S / cm. Figure 4 As shown, it exhibits high electrical conductivity and has excellent electrical conductivity.

[0047] The electrochemical linear sweep voltammetric polarization curve performance was obtained under a three-electrode test system by 2 SO 4 The prepared composite iridium oxide / iridium carrier oxygen evolution electrocatalyst was tested in an electrolyte. The catalyst was dispersed in a mixed solution of isopropanol / deionized water (volume ratio of 1:1) and 5wt.% perfluorosulfonic acid Nafion solution (25μL / mL). After ultrasonic dispersion for 1h, a uniform catalyst slurry with a concentration of 2mg / mL was obtained. 100μL of the above slurry was dropped on a carbon paper electrode and dried as a working electrode (1cm×1cm), and tested with a carbon rod as a counter electrode and Ag / AgCl as a reference electrode. The measured potentials were converted into reversible hydrogen electrode potentials (RHE).

[0048] from Figure 5 The polarization curve of the electrolytic oxygen evolution reaction is shown in Figure 2, which is similar to that of commercial IrO 2Compared with the catalyst, the catalytic performance of the composite iridium oxide / iridium carrier oxygen evolution electrocatalyst prepared in this example is significantly improved, and it can reach 10mA / cm 2 of current density.

[0049] Embodiment 2

[0050] (1) Preparation of the first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier

[0051] 1.5 g of chloroiridic acid hydrate H 2 IrCl 6 6H 2 O and 1.2 g of titanium nitride powder carrier were mixed in 400 mL of diethylene glycol solvent, wherein the specific surface area of ​​the titanium nitride powder was 35 m 2 / g, can be subjected to ultrasonic and stirring treatment to prepare the metal precursor mixed solution; then, the stirred homogenized solution is heated to 180°C and continued to be stirred for 8h; after the solution is cooled to room temperature, it is centrifuged at 8000r / min for 10min, and then washed twice with water and ethanol solution in a volume ratio of 1:1, so as to obtain the first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier.

[0052] (2) Preparation of the second precursor of the electrocatalyst of iridium oxyhydroxide coated with a conductive metal nano-iridium layer carrier

[0053] 1.2 g of the first electrocatalyst precursor prepared in step (1) above was mixed with 0.8 g of hydrated iridium tetrachloride IrCl 4 ·xH 2 O, 0.6g sodium hydroxide NaOH is dispersed in deionized water, and the mixed solution is stirred at room temperature for 3h; then the mixture is heated to a reaction temperature of 80°C and stirred for 8h; after the solution is cooled to room temperature, it is centrifuged at 8000r / min for 10min, and then washed twice with water and ethanol solution in a volume ratio of 1:1 to obtain the second precursor of the electrocatalyst of the iridium hydroxide-coated conductive metal nano iridium layer carrier.

[0054] (3) Preparation of high conductivity iridium oxide / iridium support type oxygen evolution electrocatalyst

[0055] The second electrocatalyst precursor prepared in the above step (2) is mixed with sodium nitrate powder in a mass ratio of 1:10, and then fully ground; the ground mixture is heated to 375°C at a heating rate of 3°C / min and calcined for 1 hour, and then cooled to room temperature; the obtained product is washed with deionized water and dried to obtain a high-conductivity iridium oxide / iridium titanium nitride support-type oxygen evolution electrocatalyst.

[0056] The performance of the composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst material prepared in this embodiment for electrocatalytic decomposition of water to produce hydrogen and oxygen is similar to that in the first embodiment.

[0057] Embodiment 3

[0058] (1) Preparation of the first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier

[0059] 1.5 g of chloroiridic acid hydrate H 2 IrCl 6 6H 2 O and 1.2 g of titanium dioxide powder carrier were mixed in 400 mL of diethylene glycol solvent, wherein the specific surface area of ​​the titanium dioxide powder was 30 m 2 / g, can be subjected to ultrasonic and stirring treatment to prepare the metal precursor mixed solution; then, the stirred homogenized solution is heated to 180°C and continued to be stirred for 8h; after the solution is cooled to room temperature, it is centrifuged at 8000r / min for 10min, and then washed twice with water and ethanol solution in a volume ratio of 1:1, so as to obtain the first precursor of the electrocatalyst with a conductive metal nano-iridium layer coated on the surface of the carrier.

[0060] (2) Preparation of the second precursor of the electrocatalyst of iridium oxyhydroxide coated with a conductive metal nano-iridium layer carrier

[0061] 1.2 g of the first electrocatalyst precursor prepared in step (1) above and 1.7 g of hydrated iridium chloride IrCl 4 ·xH 2 O, 1g sodium hydroxide NaOH is dispersed in deionized water, and the mixed solution is stirred at room temperature for 4h; then the mixture is heated to a reaction temperature of 80°C and stirred for 8h; after the solution is cooled to room temperature, it is centrifuged at 8000r / min for 10min, and then washed twice with water and ethanol solution in a volume ratio of 1:1 to obtain the second precursor of the electrocatalyst of the iridium hydroxide-coated conductive metal nano-iridium layer carrier.

[0062] (3) Preparation of high conductivity iridium oxide / iridium support type oxygen evolution electrocatalyst

[0063] The second electrocatalyst precursor prepared in the above step (2) is mixed with sodium nitrate powder in a mass ratio of 1:10, and then fully ground; the ground mixture is heated to 375°C at a heating rate of 3°C / min and calcined for 1 hour, and then cooled to room temperature; the obtained product is washed with deionized water, and dried to obtain a high-conductivity iridium oxide / iridium titanium oxide support type oxygen evolution electrocatalyst with a precious metal iridium loading of 70wt.%.

[0064] The performance of the composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst material prepared in this embodiment for electrocatalytic decomposition of water to produce hydrogen and oxygen is similar to that in the first embodiment.

[0065] The above is only a partial embodiment of the present invention, and its description is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. For ordinary technicians in this field, various forms of changes and improvements can still be made to the technical solutions in the embodiments based on the above description. It is not necessary and impossible to list all implementation methods here. Any modification, change, replacement, etc. made on the basis of the technical content disclosed by the present invention are equivalent to equivalent implementation cases and should be included in the protection scope of the present invention.

Claims

1. A composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst, comprising a nanoparticle carrier, a conductive metal nano-iridium layer coated on the surface of the carrier, and an iridium oxide layer further coated on the surface of the conductive metal nano-iridium layer, wherein the iridium loading is 20 to 80 wt.%.

2. The composite iridium oxide / iridium support type oxygen evolution electrocatalyst according to claim 1, characterized in that: The conductive metal nano-iridium layer is composed of iridium metal nano-particles with a size of 2 to 3 nm.

3. The composite iridium oxide / iridium support type oxygen evolution electrocatalyst according to claim 1, characterized in that: The carrier is rod-shaped or spherical nanoparticles with a particle size of 20 to 100 nm and composed of at least one of titanium dioxide, titanium nitride, niobium pentoxide and tantalum pentoxide.

4. The composite iridium oxide / iridium support type oxygen evolution electrocatalyst according to claim 1, characterized in that: The thickness of the conductive metal nano-iridium layer is 2-3 nm, and the thickness of the iridium oxide layer is 2-3 nm.

5. The method for preparing the composite iridium oxide / iridium carrier-type oxygen evolution electrocatalyst according to any one of claims 1 to 4, comprising the following steps: 1) preparing a first electrocatalyst precursor: uniformly mixing hydrated chloroiridic acid and carrier powder in an organic solvent, heating to 150-200° C. and stirring for reaction, cooling to room temperature after the reaction is completed, centrifuging and precipitating, washing, and obtaining a first electrocatalyst precursor having a conductive metal nano-iridium layer coated on the carrier surface; 2) preparing a second electrocatalyst precursor: dispersing the first electrocatalyst precursor, hydrated iridium tetrachloride, and sodium hydroxide or potassium hydroxide in deionized water, stirring at room temperature for a period of time, then heating the mixture to 70-100° C. and continuing to stir the reaction, cooling to room temperature after the reaction is completed, centrifuging and separating the precipitate, washing, and obtaining an electrocatalyst second precursor having an iridium hydroxide-coated conductive metal nano-iridium layer carrier; 3) Preparation of a composite iridium oxide / iridium support type oxygen evolution electrocatalyst: The second electrocatalyst precursor is mixed with sodium nitrate powder, fully ground and calcined at a temperature of 350 to 550° C., then cooled to room temperature, the product is washed with deionized water, and dried to obtain the composite iridium oxide / iridium support type oxygen evolution electrocatalyst.

6. The preparation method according to claim 5, characterized in that: The specific surface area of ​​the carrier powder in step 1) is 10 to 50 m 2 / g, the mass ratio of the hydrated chloroiridic acid to the carrier powder is 2:1-1:11, and the organic solvent is an alcohol solvent.

7. The preparation method according to claim 5, characterized in that: In step 2), the mass ratio of the first electrocatalyst precursor to hydrated iridium tetrachloride is 3:1 to 1:5; the mass ratio of hydrated iridium tetrachloride to sodium hydroxide or potassium hydroxide is 3:1 to 4:

1.

8. The preparation method according to claim 5, characterized in that: In step 3), the second electrocatalyst precursor is mixed with sodium nitrate powder in a mass ratio of 1:10 to 1:

50.

9. The preparation method according to claim 5, characterized in that: The organic solvent in step 1) is selected from diethylene glycol, benzyl alcohol, and ethylene glycol; the centrifugal speed in step 1) and step 2) is 6000-10000 r / min, and the separated precipitate is washed with a mixed solution of water and ethanol; in step 3), after grinding, the mixture is heated to 350-550° C. at a heating rate of 2-10° C. / min for calcination.

10. Use of the composite iridium oxide / iridium support type oxygen evolution electrocatalyst according to any one of claims 1 to 4 in the anodic oxygen evolution reaction for electrocatalytic water decomposition to produce hydrogen.

Citation Information

Cited By

  • Nano iridium / iridium oxide composite catalyst with three-dimensional porous network structure and preparation method of nano iridium / iridium oxide composite catalyst

    CN121183372A

  • A three-dimensional porous network structure nano-iridium / iridium oxide composite catalyst and its preparation method

    CN121183372B