Preparation method of nickel-based agilawood particle composite electrodeposition layer on surface of AZ91D magnesium alloy

By using variable frequency power ultrasonic pulse electrodeposition technology to add agarwood particles on the surface of magnesium alloy, agarwood particles composite electrodeposition layer is formed, which solves the corrosion and hardness problems of magnesium alloy, and achieves the improvement of high hardness and corrosion resistance. The environmental hazards of ceramic particles and the easy degradation of biomass particles in traditional technology are avoided.

CN118957694APending Publication Date: 2024-11-15DALIAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411241887.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Due to its active chemical properties and low hardness, magnesium alloys are prone to corrosion and have poor corrosion resistance. The ceramic particles added in traditional composite electrodeposition technology are costly and harmful to the environment. Biomass particles are prone to degradation under high temperature and extreme pH conditions, affecting deposition. Uniform and denseness of the layer.

Method used

The agarwood particles are added to the surface of the magnesium alloy by using variable frequency power ultrasonic pulse electrodeposition technology. The hardness and corrosion resistance are improved by combining the nickel-based agarwood particles with layer by layer. The agarwood particles are protected as heterogeneous nucleation sites and hydrophobicity. layer, enhance the performance of the deposited layer.

Benefits of technology

It significantly improves the hardness and corrosion resistance of the surface of AZ91D magnesium alloy, with a hardness of 14 to 22 times, and the self-corrosion current density decreases by 3 to 4 orders of magnitude. The deposited layer is uniform and dense, with a flat appearance, and agarwood particles are environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029535770000131
    Figure BDA0005029535770000131
  • Figure BDA0005029535770000141
    Figure BDA0005029535770000141
  • Figure HDA0005029535780000011
    Figure HDA0005029535780000011
Patent Text Reader

Abstract

The invention belongs to the technical field of metal-based micro-nano biomass particle composite electrodeposition, and discloses a preparation method of a nickel-based agilawood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy. According to the method, agilawood particles are added into a basic plating solution, a variable-frequency power ultrasonic pulse electrodeposition mode is adopted, and finally the nickel-based agilawood particle composite electrodeposition layer is prepared on the surface of the AZ91D magnesium alloy. The prepared nickel-based agilawood particle composite electro-deposition layer on the surface of the AZ91D magnesium alloy is flat in appearance, compact and uniform, the hardness is improved by 14-22 times compared with that of the AZ91D magnesium alloy, the hardness is improved by 1.1-1.8 times compared with that of an electro-deposition pure nickel layer on the surface of the AZ91D magnesium alloy, the self-corrosion current density is reduced by 3-4 orders of magnitude compared with that of the AZ91D magnesium alloy, and the self-corrosion current density is reduced by 1 order of magnitude compared with that of the electro-deposition pure nickel layer on the surface of the AZ91D magnesium alloy. And high hardness and excellent corrosion resistance are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of metal-based micro-nano biomass particle composite electrodeposition, and the present invention relates to a method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of an AZ91D magnesium alloy. Background Art

[0002] Magnesium alloy is one of the lightest structural metals, with advantages such as high specific strength and stiffness, good thermal and electrical conductivity, damping and vibration reduction, electromagnetic shielding, easy processing and forming, good biocompatibility and easy recycling. It has been applied in aerospace, transportation and information fields in Europe, America, Japan and other countries and regions. my country is a country with abundant magnesium resources, and the development and utilization of magnesium alloy is of great strategic significance. Although magnesium alloy has many advantages, magnesium alloy is anode to almost all metals, and its α phase chemical property is very active, with a large potential difference with the second phase or impurity elements, which can induce corrosion when in contact; magnesium alloy can spontaneously form Mg(OH) in the air. 2 The protective film is loose and porous, and due to poor thermodynamic stability, it is unstable when the pH is less than 11, and it is difficult to play a protective role. Secondly, the hardness of magnesium alloy is relatively low, usually between 60 and 120 HV. This is because the crystal form and crystal structure characteristics of magnesium element lead to its relatively soft physical properties. Specifically, the crystal structure of magnesium alloy is a hexagonal closest packing structure, which makes it easier to produce plastic deformation and also reduces its hardness.

[0003] Composite electrodeposition refers to the technology of using electrochemical deposition technology to co-deposit one or more solid particles with the matrix metal to form a composite deposition layer. The addition of micron and nanometer-level particles in composite electrodeposition can serve as heterogeneous nucleation sites, increase the density of grain nucleation, promote grain refinement, and effectively improve the hardness and strength of the deposited layer. Traditional composite electrodeposition technology often adds ceramic particles, which can effectively improve the wear resistance and corrosion resistance of the composite deposited layer, but these ceramic particles are often expensive and difficult to reproduce once used. Therefore, considering adding sustainable biomass particles, depositing them on the surface of composite materials, and observing the performance improvement of the deposited layer is a breakthrough.

[0004] Biomass refers to organic matter fixed during the growth of plants, animals and microorganisms, including plant and animal waste, crops, trees, microbial cells and algae. It is a very important renewable resource, and most biomass materials can be decomposed by microorganisms in the natural environment, returning to the material cycle of nature and reducing environmental pollution. However, biomass particles may degrade or change their structure in the electroplating solution, especially under high temperature and extreme pH conditions, affecting the uniformity and density of the deposited layer. In addition, biomass particles often agglomerate during the electrodeposition process, resulting in an uneven deposited layer and a decrease in the deposition rate.

[0005] Agarwood, as a special biomass material, is formed gradually by the healthy white agarwood tree under the influence of natural factors (lightning, fire, microbial invasion, etc.) or human factors (cutting, drilling, inoculation, etc.), and mainly includes sesquiterpenes and 2-(2-phenylethyl) chromones. At present, there are many studies on the preparation of nickel-based composite deposition layers by single addition of ceramic particles through composite electrodeposition, but ceramic particles may cause certain harm to human health, pollute the environment, and are expensive. The nickel-based composite electrodeposition layer with single addition of agarwood particles as the reinforcement phase has not yet been studied.

[0006] Patent No. CN116065208 A discloses a method for preparing a nano-nickel-based composite electrodeposition layer on a magnesium alloy surface by variable frequency power ultrasonic electrodeposition. However, after adding TiN and GO (graphene oxide), the hardness can only reach 600-744.9 HV, which is 8.5-10.8 times higher than that of AZ91D magnesium alloy, and the maximum self-corrosion current density reaches 7.517×10 -7 A.cm -2 , its hardness and corrosion resistance need to be improved. Summary of the invention

[0007] In order to overcome the shortcomings of the prior art, the present invention provides a method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy; the present invention adds agarwood particles to a basic plating solution, adopts a variable frequency power ultrasonic pulse electrodeposition method, and finally prepares a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy.

[0008] The nickel-based agarwood particle composite electrodeposited layer on the surface of the AZ91D magnesium alloy prepared by the present invention has a smooth appearance, is dense and uniform, has a hardness 14 to 22 times higher than that of the AZ91D magnesium alloy, and is 1.1 to 1.8 times higher than that of the electrodeposited pure nickel layer on the surface of the AZ91D magnesium alloy, and has a self-corrosion current density 3 to 4 orders of magnitude lower than that of the AZ91D magnesium alloy, and is 1 order of magnitude lower than that of the electrodeposited pure nickel layer on the surface of the AZ91D magnesium alloy, and has high hardness and excellent corrosion resistance.

[0009] The above object of the present invention is achieved through the following technical solutions:

[0010] A composite electrodeposition layer of nickel-based agarwood particles on the surface of a magnesium alloy, characterized in that it is composed of three layers, which work together to enhance the performance of the AZ91D magnesium alloy substrate. The first layer is an alkaline chemical plating layer, which is directly attached to the AZ91D magnesium alloy substrate as the first layer of the composite electrodeposition layer; the second layer is an acidic chemical plating layer, which is located above the first alkaline chemical plating layer and is the middle layer of the composite electrodeposition layer; the third layer is an electrodeposition layer, which is located at the outermost layer of the entire composite electrodeposition layer. Each layer is deposited on the basis of the previous layer, forming a layer-by-layer progressive structure.

[0011] The above-mentioned method for preparing a composite electrodeposition layer of nickel-based agarwood particles on the surface of AZ91D magnesium alloy, the cathode is a chemically plated AZ91D magnesium alloy, and the anode is a nickel plate with a mass fraction greater than 99%, the two are respectively connected to the negative electrode and the positive electrode of a pulse power supply, immersed in a pre-prepared electroplating solution and placed in an ultrasonic generator for electrodeposition, and the agarwood particles and metallic nickel are co-deposited on the surface of AZ91D magnesium alloy by using the electrochemical principle to prepare a composite electrodeposition layer of nickel-based agarwood particles on the surface of AZ91D magnesium alloy;

[0012] The electroplating solution is composed of nickel sulfate as the main salt, ammonium citrate and ammonium bifluoride as the main additional salts, sodium saccharin and sodium dodecyl sulfate are added to achieve the purpose of refining grains and reducing pores, and Tween 20 and agarwood particles are added at a weight ratio of 5-15:1-9.

[0013] The preparation method of the nickel-based agarwood particle composite electrodeposition layer on the surface of the AZ91D magnesium alloy is specifically performed as follows:

[0014] S1. Grinding and polishing: Grinding and polishing the surface of AZ91D magnesium alloy, and then using anhydrous ethanol ultrasonic cleaning and deionized water cleaning;

[0015] S2. Alkaline washing and degreasing: using the saponification of alkaline solution to remove the oil stains on the surface of the AZ91D magnesium alloy after polishing in step S1, the composition of the alkaline solution is 30-50 g / L of sodium hydroxide, 30-35 g / L of sodium phosphate, and 10-12 g / L of sodium carbonate, and the alkaline washing is carried out at 60-70°C for 15-20 min and then washed with deionized water;

[0016] S3. Pickling: Pickle the AZ91D magnesium alloy after alkali washing and degreasing in step S2, 80-90wt%, concentration 580-620cm 3 / L phosphoric acid solution pickling for 35 to 45 seconds to remove oxides on the surface of AZ91D magnesium alloy, and then rinse with deionized water;

[0017] S4. Surface conditioning: Surface conditioning the pickled AZ91D magnesium alloy at 65-70°C for 2-2.5 min using a pyrophosphate system to remove the oxides produced in step S3 and slightly etch the β phase of the AZ91D magnesium alloy to level the surface, so that the AZ91D magnesium alloy is fully exposed, the surface conditioning solution includes 150-170 g / L potassium pyrophosphate, 18-22 g / L sodium carbonate, and 8-12 g / L potassium fluoride, and the surface conditioning is followed by washing with deionized water;

[0018] S5. Activation: Activate the AZ91D magnesium alloy after surface conditioning in step S4; place the AZ91D magnesium alloy after surface conditioning in a mixed solution of phosphoric acid and ammonium bifluoride and activate it at room temperature for 1 to 2 minutes, the volume ratio of phosphoric acid to ammonium bifluoride being 2 to 3:1 to 2; remove oxides and generate a magnesium fluoride protective film layer, and wash with deionized water after activation; the phosphoric acid is preferably 170 to 190 mL / L; the ammonium bifluoride is preferably 90 to 100 g / L.

[0019] S6. Alkaline chemical plating: the AZ91D magnesium alloy activated in step S5 is subjected to alkaline chemical plating, the alkaline chemical plating solution comprises: nickel sulfate 20-25g / L, sodium hypophosphite 20-25g / L, sodium citrate 18-22g / L, ammonium bifluoride 10-12g / L, sodium carbonate 18-22g / L; the plating process is: the plating temperature is 70-75°C, the pH is adjusted to 9.20-9.60 with appropriate amount of ammonia water, the plating time is 40-50min, and the magnetic stirring rate is 210-280r / min;

[0020] S7. Acid chemical plating: Acid chemical plating is performed on the AZ91D magnesium alloy after the alkaline chemical plating in step S6, and the acid chemical plating solution includes: 20-25 g / L nickel sulfate, 20-25 g / L sodium hypophosphite, 4-6 g / L citric acid, and 18-22 g / L ammonium bifluoride; the plating process is: the plating temperature is 80-85°C, the pH is adjusted to 6.00-6.25 with an appropriate amount of ammonia water, the plating time is 40-50 min, and the magnetic stirring rate is 210-280 r / min;

[0021] S8. Prepare a basic plating solution: the basic plating solution components are: nickel sulfate 100-160g / L, ammonium citrate 6-15g / L, ammonium bifluoride 30-50g / L, saccharin sodium 1-3g / L, sodium dodecyl sulfate 0.1-0.2g / L;

[0022] S9. Ultrafine grinding: The diameter of the agarwood particles reaches 200nm~500nm after being processed by a high-speed intelligent grinder;

[0023] S10. Prepare the electroplating solution: mix the ultrafinely crushed agarwood particles and Tween20 in step S9 with deionized water to obtain a mixed solution, and apply magnetic stirring, mechanical stirring and ultrasonic waves to fully disperse the mixed solution, and add the dispersed mixed solution to the basic plating solution prepared in step S8; after mixing, place it in an ultrasonic field again and add mechanical stirring to continue dispersing, and obtain the electroplating solution required for preparing the nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy;

[0024] S11. Electrodeposition: The anode nickel plate and the AZ91D magnesium alloy after the acid chemical plating in step S7 are immersed in the electroplating solution prepared in step S10 as cathodes, and then a pulse power supply and an ultrasonic generator are connected between the cathode and the anode for electroplating; the electroplating process is: voltage 2 to 4V, current density 1.5 to 3A·cm -2 , duty cycle 35-80%, ultrasonic power 150-240W, ultrasonic frequency 45KHZ and 80KHZ alternating for 10-20s, mechanical stirring speed 150r / min-400r / min, deposition temperature 45-50℃, deposition time 20-70min, and finally prepare a nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added agarwood particles.

[0025] Preferably, in the alkaline degreasing in step S2, the composition of the alkaline solution is 35 g / L sodium hydroxide, 30 g / L sodium phosphate, and 11 g / L sodium carbonate, and the alkaline washing conditions are temperature 65° C. and time 20 min.

[0026] Preferably, in step S3, the pickling conditions are 85wt% and 600cm 3 / L phosphoric acid solution, pickling temperature room temperature, pickling time 40s.

[0027] Preferably, in step S4, the surface conditioning solution is 160 g / L potassium pyrophosphate, 20 g / L sodium carbonate, and 11 g / L potassium fluoride, and the surface conditioning conditions are a surface conditioning temperature of 70° C. and a time of 2.5 min.

[0028] Preferably, in step S5 activation, the activation solution is 180 mL / L phosphoric acid, 95 g / L ammonium bifluoride, and the activation time is 1.5 min.

[0029] Preferably, in the alkaline chemical plating in step S6, the alkaline chemical plating solution is 20 g / L nickel sulfate, 25 g / L sodium hypophosphite, 20 g / L sodium citrate, 10 g / L ammonium bifluoride, and 20 g / L sodium carbonate; the plating temperature is 75°C, the pH is 9.40, and the plating time is 45 min.

[0030] Preferably, in the acid chemical plating in step S7, the acid chemical plating solution is 20 g / L nickel sulfate, 20 g / L sodium hypophosphite, 5 g / L citric acid, and 20 g / L ammonium bifluoride; the plating temperature is 80° C., the pH is 6.20, and the plating time is 45 min.

[0031] Preferably, in step S8, the basic plating solution is prepared, and the basic plating solution is 120 g / L nickel sulfate, 10 g / L ammonium citrate, 40 g / L ammonium bifluoride, 3 g / L sodium saccharin, and 0.1 g / L sodium dodecyl sulfate.

[0032] Preferably, in step S10, the concentration of agarwood particles is 1 g / L, 3 g / L, 5 g / L, 7 g / L, 9 g / L; and the concentration of Tween 20 is 10 mL / L.

[0033] Preferably, in step S10, magnetic stirring, mechanical stirring and ultrasonic waves are applied to the mixture of the agarwood particles and Tween 20 to fully disperse them, and the process conditions are: magnetic stirring rate is 300r / min, action time is 10min; mechanical stirring speed is 300r / min, ultrasonic power is 210W, and action time is 20min.

[0034] Preferably, in step S10, the dispersed mixed solution is added to the basic plating solution prepared in step S8, mixed, and then placed in an ultrasonic field again with mechanical stirring to continue dispersion. The process conditions are: mechanical stirring speed of 300 r / min, ultrasonic power of 210 W, and action time of 10 min.

[0035] Preferably, in step S11, the anode and cathode are immersed in the electroplating solution, the anode and cathode area ratio is 1-2:2-3, and the inter-electrode distance is 25 mm.

[0036] Preferably, in step S11, the electrodeposition process is performed at a current density of 2A·cm -2 , duty cycle 80%, ultrasonic power 210W, ultrasonic frequency 45KHZ and 80KHZ alternating action time 10s and 20s, mechanical stirring speed 300r / min.

[0037] The beneficial effects of the present invention compared with the prior art are:

[0038] The present invention provides a method for preparing a composite electrodeposition layer of nickel-based agarwood particles on the surface of an AZ91D magnesium alloy. Traditional composite electrodeposition often adds micron and nanometer-level ceramic particles, which may cause certain harm to human health, pollute the environment, and are costly. With the increasing demand for sustainability and environmental friendliness, the present invention adds micron-level biomass agarwood particles as second-phase particles into a basic plating solution, which is not only beneficial to human health but also environmentally friendly, and improves the comprehensive properties of the AZ91D magnesium alloy, such as hardness and corrosion resistance, and has potential applications in the fields of medicine, food packaging, and the environment.

[0039] The invention adds agarwood particles to the basic plating solution and determines the maximum hardness and the maximum corrosion resistance of the agarwood particles. The agarwood particles can be combined with Ni by a variable frequency power ultrasonic composite electrodeposition process. 2+ Co-deposition, on the one hand, agarwood particles can become heterogeneous nucleation sites, for Ni 2+It provides a large number of nucleation centers, which plays a role in fine crystal strengthening; on the other hand, the agarwood particles are dispersed in the sediment layer, which can hinder the movement of dislocations and improve the hardness and uniformity of the sediment layer. The agarwood particles contain sesquiterpenoid compounds, which can form a hydrophobic protective layer on the surface of the sediment layer, reduce the penetration of corrosive media into the matrix, and slow down the corrosion rate; in addition, the sesquiterpenoid compounds contain easily oxidized components, which can act as sacrificial anodes in corrosive environments, protect the sediment layer from corrosion through their own oxidation, and improve corrosion resistance. In addition, Tween20 is used as a dispersant, which can form a thin film on the surface of the agarwood particles, reduce the attraction between particles, and avoid agglomeration.

[0040] The present invention provides a method for preparing a nickel-based agarwood particle composite electrodeposited layer on the surface of an AZ91D magnesium alloy. The deposition layer prepared by the method is uniform and dense, has a smooth appearance, and has a hardness that is 14 to 22 times higher than that of the AZ91D magnesium alloy, and 1.1 to 1.8 times higher than that of the electrodeposited pure nickel layer on the surface of the AZ91D magnesium alloy (without adding agarwood particles). The self-corrosion current density is 3 to 4 orders of magnitude lower than that of the AZ91D magnesium alloy, and is 1 order of magnitude lower than that of the electrodeposited pure nickel layer on the surface of the AZ91D magnesium alloy. When the amount of agarwood particles added is 5 g / L, the hardness reaches a maximum of 1600.7 HV; when the amount of agarwood particles added is 9 g / L, the corrosion resistance is the best, the self-corrosion potential is -0.018 V, and the self-corrosion current density is 7.426×10 -8 A.cm -2 . BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The present invention is further described below in conjunction with the accompanying drawings and embodiments:

[0042] Figure 1 The surface metallographic structures of the deposited layers prepared in Examples 1-5 are magnified 800 times. (a) Example 1, (b) Example 2, (c) Example 3, (d) Example 4, (e) Example 5.

[0043] Figure 2 The cross-sectional metallographic morphology images of the deposited layers prepared in Examples 1-5 are magnified 560 times. (a) Example 1, (b) Example 2, (c) Example 3, (d) Example 4, (e) Example 5.

[0044] Figure 3 The surface SEM microstructure images of the deposited layers prepared in Examples 1-5, magnified 2000 times, are (a) Example 1, (b) Example 2, (c) Example 3, (d) Example 4, and (e) Example 5.

[0045] Figure 4 This is a cross-sectional SEM microstructure image of the deposited layer of Example 5 magnified 4000 times.

[0046] Figure 5 This is the EDS spectrum analysis diagram of the deposited layer in Example 3.

[0047] Figure 6 It is the XRD diffraction pattern of the deposited layers prepared in Examples 1-5 and Comparative Example 1.

[0048] Figure 7 is a microhardness graph of the deposited layers prepared in Examples 1-5.

[0049] Figure 8 1 is a polarization curve diagram of the deposited layer prepared in Example 1-5.

[0050] Fig. 9 This is a diameter size distribution diagram of the agarwood particles of the present invention. DETAILED DESCRIPTION

[0051] The present invention is described in detail below by specific examples, but the protection scope of the present invention is not limited. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial channels.

[0052] In one or more examples of this implementation mode, the specific preparation process is as follows:

[0053] S1. Grinding and polishing: the surface of the AZ91D magnesium alloy is grinded with 320 mesh, 600 mesh, 800 mesh, 1000 mesh, 1200 mesh, 1500 mesh and 2000 mesh water-abrasive sandpaper respectively, and the ground surface of the AZ91D magnesium alloy is polished with 1.5 μm alumina polishing paste.

[0054] S2. After the polishing in step S1, the AZ91D magnesium alloy is cleaned, alkaline degreasing, pickled, surface conditioned, and activated to remove possible dust, grease, and oxides and generate a protective magnesium fluoride film. Cleaning: Clean with anhydrous ethanol for 10 to 20 minutes in an ultrasonic wave of 60 to 80 KHZ and 150 to 200 W, and rinse with deionized water; Alkaline degreasing: Place the AZ91D magnesium alloy in a 60 to 70 ° C degreasing alkali solution for 15 to 20 minutes to clean the grease that may exist on the surface. The degreasing alkali solution is composed of 30 to 50 g / L of sodium hydroxide, 30 to 35 g / L of sodium phosphate, 10 to 12 g / L of sodium carbonate, and water as the balance. Rinse with deionized water after alkaline washing; Pickling: Pickle the AZ91D magnesium alloy at room temperature for 35 to 45 seconds to remove surface oxides. The main components of the pickling solution are 85% by mass and 580 to 620 cm 3 / L of phosphoric acid, and rinse with deionized water after pickling; surface conditioning: surface conditioning the AZ91D magnesium alloy at 65-70°C for 2-2.5min to remove the pickling corrosion products adsorbed on the surface after pickling, and slightly etch the β phase of the AZ91D magnesium alloy to level the surface, the surface conditioning solution includes 150-170g / L of potassium pyrophosphate, 18-22g / L of sodium carbonate, 8-12g / L of potassium fluoride, and water as the balance, and rinse with deionized water after surface conditioning; activation: activating the AZ91D magnesium alloy at room temperature for 1-2min to further dissolve the oxide to expose the active metal interface and generate a magnesium fluoride protective film, the activation solution includes 170-190mL / L of phosphoric acid, 90-100g / L of ammonium bifluoride, and water as the balance, and rinse with deionized water after activation; and obtaining a sample.

[0055] S3. Immediately place the AZ91D magnesium alloy after the surface treatment in step S2 in a constant temperature water bath for alkaline chemical plating. The alkaline chemical plating solution comprises 20-25 g / L nickel sulfate, 20-25 g / L sodium hypophosphite, 18-22 g / L citrate, 10-12 g / L ammonium bifluoride, and 18-22 g / L sodium carbonate. During the alkaline chemical plating process, the temperature is 70-75°C, the alkaline solution is adjusted to a pH of 9.20-9.60, the plating time is 45-55 min, and the magnetic stirring rate is 250-300 r / min.

[0056] S4. After the alkaline chemical plating of AZ91D magnesium alloy in step S3 is performed, the surface is cleaned with deionized water and then placed in a constant temperature water bath for acid chemical plating. The components of the acid chemical plating solution are 20-25 g / L of nickel salt, 20-25 g / L of sodium hypophosphite, 4-6 g / L of citric acid, and 18-22 g / L of ammonium bifluoride. During the acid chemical plating process, the temperature is 80-85°C, the acidic solution is adjusted to PH 6.00-6.25, the plating time is 45-55 min, and the magnetic stirring rate is 250-300 r / min. After acid chemical plating, since the plating process is in an acidic environment, the water bath needs to be quickly taken out, stirring is stopped, and it is washed with deionized water and blown dry with hot air.

[0057] S5. Prepare a basic plating solution, the components of which are: nickel sulfate 100-160 g / L, ammonium citrate 6-15 g / L, ammonium bifluoride 30-50 g / L, saccharin sodium 1-3 g / L, and sodium dodecyl sulfate 0.1-0.2 g / L.

[0058] S6. After the agarwood particles are processed by a high-speed intelligent crusher, the particle diameter reaches 200nm~500nm.

[0059] S7. Prepare the electroplating solution, mix the crushed agarwood particles and Tween20 with deionized water to obtain a mixed solution, and apply magnetic stirring, mechanical stirring and ultrasonic waves to fully disperse the mixed solution, and add the dispersed mixed solution to the basic plating solution prepared in step S5 to obtain the electroplating solution required for preparing the nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added agarwood particles, and place the plating solution in the ultrasonic field again and add mechanical stirring to continue to disperse it.

[0060] S8. Immerse the anode nickel plate and the AZ91D magnesium alloy after acid chemical plating in step S4 as cathodes in the electroplating solution prepared in step S7, and then connect a pulse power supply and an ultrasonic generator between the cathode and the anode for electroplating. The electroplating process is: voltage 2 to 4V, current density 1.5 to 3A·cm -2 , duty cycle 35-80%, ultrasonic power 150-240W, ultrasonic frequency 45KHZ and 80KHZ alternating for 10-20s, mechanical stirring speed 150r / min-400r / min, deposition temperature 45-50℃, deposition time 20-70min.

[0061] In order to enable those skilled in the art to more clearly understand the technical solution of the present disclosure, the technical solution of the present disclosure will be described in detail below in conjunction with specific embodiments.

[0062] Example 1

[0063] A method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow is as follows:

[0064] S1. Grinding and polishing: AZ91D magnesium alloy was ground and polished with sandpaper, and then ultrasonically cleaned in ethanol solution for 2 min and cleaned with deionized water for 2 min.

[0065] S2. Alkaline washing and degreasing: alkaline washing and degreasing of the AZ91D magnesium alloy after polishing in step S1; prepare an alkaline washing solution containing 35g / L sodium hydroxide, 30g / L sodium phosphate, and 10g / L sodium carbonate, the alkaline washing temperature is 65°C, and the alkaline washing time is 20min.

[0066] S3. Pickling: pickling the AZ91D magnesium alloy after alkali washing and degreasing in step S2, preparing a solution with a mass fraction of 80% and a concentration of 600 cm 3 / L phosphoric acid pickling solution, and rinse with deionized water for 1 minute after pickling.

[0067] S4. Surface conditioning: Surface conditioning is performed on the AZ91D magnesium alloy after pickling in step S3. A surface conditioning solution containing 160 g / L potassium pyrophosphate, 20 g / L sodium carbonate, and 11 g / L potassium fluoride is prepared. The surface conditioning is performed on the pickled AZ91D magnesium alloy at 70°C for 2.5 min. After the surface conditioning, the alloy is rinsed with deionized water for 1 min.

[0068] S5. Activation: Activate the AZ91D magnesium alloy after the surface conditioning in step S4 by preparing an activation solution containing 180 mL / L phosphoric acid and 95 g / L ammonium bifluoride. Activate the AZ91D magnesium alloy after the surface conditioning at room temperature for 1.5 min. After activation, rinse with deionized water for 1 min.

[0069] S6. Alkaline chemical plating. The AZ91D magnesium alloy activated in step S5 is subjected to alkaline chemical plating. An alkaline chemical plating solution containing 20 g / L nickel sulfate, 25 g / L sodium hypophosphite, 20 g / L sodium citrate, 10 g / L ammonium bifluoride, and 20 g / L sodium carbonate is prepared. The pH value is 9.40. The prepared alkaline chemical plating solution is placed in a constant temperature water bath at 75°C. The plating is performed for 45 minutes with a magnetic stirring rate of 210 r / min.

[0070] S7. Acid chemical plating: Acid chemical plating is performed on the AZ91D magnesium alloy after the alkaline chemical plating in step S6. An acid chemical plating solution containing 20 g / L nickel sulfate, 20 g / L sodium hypophosphite, 5 g / L citric acid, and 20 g / L ammonium bifluoride is prepared. The pH value is 6.20. The prepared acid chemical plating solution is placed in a constant temperature water bath at 80°C. The plating is performed for 45 minutes with a magnetic stirring rate of 210 r / min.

[0071] S8. Prepare a basic plating solution, the components of which are: 120 g / L nickel sulfate, 10 g / L ammonium citrate, 40 g / L ammonium bifluoride, 3 g / L saccharin sodium, and 0.1 g / L sodium dodecyl sulfate.

[0072] S9. After the agarwood particles are processed by a high-speed intelligent crusher, the particle diameter reaches 200nm~500nm.

[0073] S10. Prepare the electroplating solution, mix the agarwood particles with a content of 1g / L and 10mL / L Tween20 crushed in step S9 with deionized water to obtain a mixed solution, and apply magnetic stirring, mechanical stirring and ultrasonic waves to fully disperse the mixed solution, add the dispersed mixed solution to the basic plating solution prepared in step S8, and obtain the electroplating solution required for preparing the nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added agarwood particles, and place the plating solution in the ultrasonic field again and add mechanical stirring to continue to disperse it.

[0074] S11. Immerse the anode nickel plate and the AZ91D magnesium alloy after acid chemical plating in step S7 in the electroplating solution prepared in step S10 and place them in an ultrasonic generator, with the positive and negative electrodes of the pulse power supply connected to the anode and cathode respectively. The electrodeposition process is: voltage 3V, current density 2A·cm -2 , duty cycle 80%, ultrasonic power 210W, ultrasonic frequency of 45KHz and 80KHz alternating for 10s and 20s, mechanical stirring speed 300r / min, deposition temperature 55℃, deposition time 60min, and finally prepared a nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added agarwood particles.

[0075] Figure 1 (a) is the surface metallographic structure morphology of the composite deposition layer prepared in this embodiment. The deposition layer is relatively uniform and dense; Figure 2 (a) From the perspective of cross-sectional metallographic structure, no peeling or cracking is observed, and the deposited layer is tightly bonded to the AZ91D magnesium alloy. Figure 3 (a) is the SEM microstructure of the composite deposition layer surface prepared in this embodiment. It is further observed that the deposition layer is uniform and dense. The nodules that appear are agarwood particles and metal nickel co-deposited on the surface of the deposition layer. Nodules are very common in nickel-based electrodeposition and can be caused by the incorporation of inert particles, resulting in uneven current distribution on the cathode. The hardness test results are shown in Figure 2. Figure 7 As shown in the figure, the microhardness of the composite deposition layer is 1126.8HV, which is 16 times higher than the microhardness of AZ91D magnesium alloy (69.382HV) and 1.2 times higher than the microhardness of the pure nickel layer without adding agarwood particles (933.6HV). Figure 8 As shown in the figure, the self-corrosion potential of the deposited layer is -0.446 V, which is 0.873 V more positive than that of AZ91D magnesium alloy (-1.32 V) and 0.096 V more negative than that of pure nickel layer (-0.350 V). The self-corrosion current density is 7.771×10 -7 A.cm -2 ) drops to 7.569×10 -7 A.cm -2 , compared with AZ91D magnesium alloy (1.669×10 -4 A.cm -2 ) decreased by 3 orders of magnitude, indicating that the hardness and corrosion resistance of the deposited layer increased compared with that without adding agarwood particles. It can be seen that adding agarwood particles can 2+ Co-deposition becomes a heterogeneous nucleation site for Ni 2+ It provides a large number of nucleation centers, which plays a role in fine grain strengthening. The agarwood particles are dispersed in the sedimentary layer, which can hinder the movement of dislocations, prevent the corrosive medium from penetrating into the matrix, and improve the hardness and corrosion resistance of the sedimentary layer.

[0076] Example 2

[0077] A method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow thereof is different from that of Example 1 in that:

[0078] The content of agarwood particles in the electroplating solution prepared in S10 is 3 g / L, and the rest is the same as in Example 1.

[0079] Figure 1 (b) is the metallographic structure of the composite deposition layer prepared in this embodiment. The deposition layer is more uniform and dense than that in Example 1. Figure 2 (b) From the perspective of the cross-sectional metallographic structure, no peeling or cracking is observed, and the deposited layer is tightly bonded to the AZ91D magnesium alloy. Figure 3 (b) The SEM microstructure of the composite sediment layer surface prepared in this embodiment shows that the nodules on the sediment layer surface are reduced, which is due to the increase in the content of agarwood particles, which has a certain effect on the grain refinement. Figure 7 As shown in the figure, the microhardness of the composite deposition layer is 1085.9HV, which is 15.65 times higher than the microhardness of AZ91D magnesium alloy (69.382HV) and 1.16 times higher than the microhardness of pure nickel layer (933.6HV). Figure 8 As shown in the figure, the self-corrosion potential of the deposited layer is -0.056 V, which is 1.264 V positively shifted from AZ91D magnesium alloy (-1.32 V) and 0.294 V positively shifted from pure nickel layer (-0.350 V). The self-corrosion current density is higher than that of pure nickel layer (7.771×10 -7 A.cm -2 ) decreased to 1.046×10 -7 A.cm -2 , compared with AZ91D magnesium alloy (1.669×10 -4 A.cm -2 ) decreased by 3 orders of magnitude, indicating that with the increase of the amount of agarwood particles added, the hardness and corrosion resistance of the deposited layer were further improved.

[0080] Example 3

[0081] A method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow thereof is different from that of Example 1 in that:

[0082] The content of agarwood particles in the electroplating solution prepared in S10 is 5 g / L, and the rest is the same as in Example 1.

[0083] Figure 1 (c) is the surface metallographic structure morphology of the composite deposition layer prepared in this embodiment. The deposition layer is uniform and dense, and due to the increase in the content of agarwood particles, the deposition layer becomes obviously yellow. Combined with the EDS test on the deposition layer, the results are as follows Figure 5As shown in the figure, six elements, Ni, C, Pb, Cd, Cr, and Hg, were detected on the surface of the sedimentary layer, proving that the agarwood particles were successfully co-deposited with metallic nickel. Figure 2 (c) From the perspective of the cross-sectional metallographic structure, no peeling or cracking is observed, and the deposited layer is tightly bonded to the AZ91D magnesium alloy. Figure 3 (c) is the SEM microstructure of the composite sediment layer surface prepared in this embodiment. It is observed that the nodules on the surface of the sediment layer disappear and the layer is uniform and dense, indicating that the increase in the content of agarwood particles further refines the grains to a certain extent. The hardness test results are as follows: Figure 7 As shown in the figure, the microhardness of the composite deposition layer is 1600.7HV, which is 23 times higher than the microhardness of AZ91D magnesium alloy (69.382HV) and 1.71 times higher than the microhardness of pure nickel layer (933.6HV). Figure 8 As shown in the figure, the self-corrosion potential of the deposited layer is -0.205 V, which is 1.115 V positively shifted from AZ91D magnesium alloy (-1.32 V) and 0.145 V positively shifted from pure nickel layer (-0.350 V). The self-corrosion current density is higher than that of pure nickel layer (7.771×10 -7 A.cm -2 ) decreased to 1.281×10 -7 A.cm -2 , compared with AZ91D magnesium alloy (1.669×10 -4 A.cm -2 ) decreased by 3 orders of magnitude, indicating that when the addition amount of agarwood particles was 5g / L, the hardness of the deposited layer reached the highest and the corrosion resistance was also significantly improved.

[0084] Example 4

[0085] A method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow thereof is different from that of Example 1 in that:

[0086] The content of agarwood particles in the electroplating solution prepared in S10 is 7 g / L, and the rest is the same as in Example 1.

[0087] Figure 1 (d) is the metallographic structure of the composite deposited layer prepared in this example. The deposited layer is uniform and dense and further turns yellow. Figure 2 (d) From the perspective of the cross-sectional metallographic structure, no peeling or cracking is observed, and the deposited layer is tightly bonded to the AZ91D magnesium alloy. Figure 3 (d) is the SEM microstructure of the composite deposition layer surface prepared in this embodiment. The surface of the deposition layer gradually tends to be smooth and dense, the number of surface defects is minimal, and the cellular morphology gradually disappears, indicating that the addition of agarwood particles promotes the deposition of metal nickel ions and increases the deposition rate. Figure 7As shown in the figure, the microhardness of the composite deposited layer is 1433.5HV, which is 20 times higher than the microhardness of AZ91D magnesium alloy (69.382HV) and 1.54 times higher than the microhardness of the pure nickel layer (933.6HV). The hardness of the deposited layer is relatively high. The electrochemical corrosion resistance test is shown in the figure. Figure 8 As shown in the figure, the self-corrosion potential of the deposited layer is -0.181 V, which is 1.139 V positively shifted from AZ91D magnesium alloy (-1.32 V) and 0.169 V positively shifted from pure nickel layer (-0.350 V). The self-corrosion current density is higher than that of pure nickel layer (7.771×10 -7 A.cm -2 ) dropped to 6.277×10-8A·cm -2 , compared with AZ91D magnesium alloy (1.669×10 -4 A.cm -2 ) decreased by 4 orders of magnitude, indicating that as the amount of agarwood particles added to the sedimentary layer further increased, the hardness and corrosion resistance also increased further.

[0088] Example 5

[0089] A method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow thereof is different from that of Example 1 in that:

[0090] The content of agarwood particles in the electroplating solution prepared in S10 is 9 g / L, and the rest is the same as in Example 1.

[0091] Figure 1 (e) is the metallographic structure morphology of the composite deposited layer prepared in this example. The deposited layer is uniform and dense, and the color of the deposited layer changes from yellow to yellow-brown. Figure 2 (e) From the perspective of the cross-sectional metallographic structure, no peeling or cracking is observed, and the deposited layer is tightly bonded to the AZ91D magnesium alloy. Figure 3 (e) is the SEM microstructure of the composite deposition layer surface prepared in this embodiment. It can be seen that as the amount of agarwood particles added increases, the cellular morphology becomes more and more obvious, indicating that too many agarwood particles cannot further increase the deposition rate. On the contrary, the agglomeration phenomenon hinders the movement of metal nickel ions to the cathode, resulting in a decrease in the deposition rate. The hardness test results are shown in Figure 2. Figure 7 As shown in the figure, the microhardness of the composite deposited layer is 1024.5HV, which is 15 times higher than the microhardness of AZ91D magnesium alloy (69.382HV) and 1.09 times higher than the microhardness of the pure nickel layer (933.6HV). The hardness of the deposited layer is relatively high. The electrochemical corrosion resistance test is shown in the figure. Figure 8 As shown in the figure, the self-corrosion potential of the deposited layer is -0.018 V, which is 1.302 V positively shifted from AZ91D magnesium alloy (-1.32 V) and 0.332 V positively shifted from pure nickel layer (-0.350 V). The self-corrosion current density is 7.426×10 -8 A.cm-2 Compared with AZ91D magnesium alloy (1.669×10 -4 A.cm -2 ) decreased by 4 orders of magnitude, and the self-corrosion current density of this embodiment is the lowest and the corrosion resistance is the best.

[0092] Comparative Example 1

[0093] A method for preparing a pure nickel layer by electrodeposition on the surface of AZ91D magnesium alloy. The specific process flow is as follows:

[0094] S1-S8 are the same as in Example 1.

[0095] S9: immerse the anode nickel plate and the sample after step S7 as the cathode in the basic plating solution prepared in step S8 and place them in an ultrasonic generator, and connect the positive and negative poles of the pulse power supply to the anode and cathode respectively. The electrodeposition process is: voltage 3V, current density 2A·cm -2 , duty cycle 80%, ultrasonic power 210W, ultrasonic frequency of 45KHz and 80KHz alternating for 10s and 20s, mechanical stirring speed 300r / min, deposition temperature 55℃, deposition time 60min, and finally prepared pure nickel layer electroplated on the surface of AZ91D magnesium alloy.

[0096] Comparative Example 2

[0097] A method for preparing a nickel-based nano-diamond composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow is as follows:

[0098] S1-S8 are the same as in Example 1.

[0099] S9. Prepare an electroplating solution, add 5 g / L of nanodiamonds into the basic plating solution prepared in step S8, and obtain the plating solution required for preparing a nickel-based composite electrodeposited layer on the surface of AZ91D magnesium alloy with added nanodiamonds, and place the plating solution in an ultrasonic field again and add mechanical stirring to continue dispersion.

[0100] S10. Immerse the anode nickel plate and the AZ91D magnesium alloy after acid chemical plating in step S7 in the electroplating solution prepared in step S9 and place them in an ultrasonic generator, with the positive and negative electrodes of the pulse power supply connected to the anode and cathode respectively. The electrodeposition process is: voltage 3V, current density 2A·cm -2 , duty cycle 80%, ultrasonic power 210W, ultrasonic frequency of 45KHz and 80KHz alternating for 10s and 20s, mechanical stirring speed 300r / min, deposition temperature 55℃, deposition time 60min, and finally a nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added nanodiamonds was prepared.

[0101] Comparative Example 3

[0102] A method for preparing a nickel-based nano-diamond composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow is different from that of Example 4 in that:

[0103] S10. Electrodeposition process: voltage 3V, current density 1.5A·cm -2 , duty cycle 40%, ultrasonic power 240W, ultrasonic frequency of 45KHz and 80KHz alternating for 10s and 20s, mechanical stirring speed 300r / min, deposition temperature 55℃, deposition time 80min, and finally prepared a nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added agarwood particles.

[0104] Comparative Example 4

[0105] A method for preparing a nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy. The specific process flow is different from that of Example 4 in that:

[0106] S8. Prepare a basic plating solution, the components of which are: 120 g / L nickel sulfate, 10 g / L ammonium citrate, 40 g / L ammonium bifluoride, and 3 g / L saccharin sodium.

[0107] S10 prepares the electroplating solution, mixes the agarwood particles and 3g / L sodium dodecyl sulfate with deionized water, and applies magnetic stirring, mechanical stirring and ultrasonic waves to fully disperse the mixed solution, and adds the dispersed mixed solution to the basic plating solution prepared in step S8 to obtain the plating solution required for preparing the nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added agarwood particles, and the plating solution is placed in the ultrasonic field again and mechanically stirred to continue to disperse it.

[0108] The effects of the above comparative example and the technical solution of the best embodiment of the present invention are compared:

[0109] The comparative effect evaluation of the magnesium alloy electrodeposition layers prepared in the embodiment and the comparative example is shown in Table 1.

[0110] Comparative Example 5

[0111] A method for preparing a composite electrodeposition layer of agarwood particles on the surface of AZ91D magnesium alloy with a nickel layer. The specific process flow is as follows:

[0112] S3. Pickling: pickling the AZ91D magnesium alloy after alkaline washing and degreasing in step S2, with the pickling time being 60s.

[0113] S4. Surface conditioning: Surface conditioning is performed on the AZ91D magnesium alloy after pickling in step S3. The surface conditioning time is 210 seconds.

[0114] S6. Alkaline chemical plating: alkaline chemical plating is performed on the AZ91D magnesium alloy activated in step S5, and the pH value is 9.15.

[0115] S7. Acid chemical plating: Acid chemical plating is performed on the AZ91D magnesium alloy after the alkaline chemical plating in step S6, and the pH is 6.45.

[0116] The rest is the same as in Example 1.

[0117] Table 1 Comparative effect evaluation table of magnesium alloy electrodeposition layers prepared in the embodiments and comparative examples

[0118]

[0119]

[0120] The above-described embodiments are only preferred embodiments of the present invention, but not all feasible embodiments of the present invention. For those skilled in the art, any obvious changes made thereto without departing from the principles and spirit of the present invention should be considered to be included in the scope of protection of the claims of the present invention.

Claims

1. A composite electrodeposition layer of nickel-based agarwood particles on a magnesium alloy surface, characterized in that: It consists of three layers. The first layer is an alkaline chemical plating layer, which is directly attached to the AZ91D magnesium alloy substrate as the first layer of the composite electrodeposition layer; the second layer is an acidic chemical plating layer, which is located above the first alkaline chemical plating layer and is the middle layer of the composite electrodeposition layer; the third layer is an electrodeposition layer.

2. The method for preparing the nickel-based agarwood particle composite electrodeposition layer on the surface of magnesium alloy as claimed in claim 1, characterized in that: The cathode is made of chemically plated AZ91D magnesium alloy, and the anode is made of a nickel plate with a mass fraction greater than 99%. The two are respectively connected to the negative and positive electrodes of a pulse power supply, immersed in a pre-prepared electroplating solution and placed in an ultrasonic generator for electrodeposition. Using the principle of electrochemistry, the agarwood particles and metallic nickel are co-deposited on the surface of the AZ91D magnesium alloy to prepare a nickel-based agarwood particle composite electrodeposited layer on the surface of the AZ91D magnesium alloy.

3. The method for preparing the nickel-based agarwood particle composite electrodeposition layer on the surface of magnesium alloy as claimed in claim 2, characterized in that: The electroplating solution is composed of nickel sulfate as the main salt, ammonium citrate and ammonium bifluoride as the main additional salts, sodium saccharin and sodium dodecyl sulfate are added to achieve the purpose of refining grains and reducing pores, and Tween 20 and agarwood particles are added at a weight ratio of 5-15:1-9.

4. The method for preparing the nickel-based agarwood particle composite electrodeposition layer on the surface of magnesium alloy as claimed in claim 2, characterized in that: The specific steps are as follows: S1. Grinding and polishing: Grinding and polishing the surface of AZ91D magnesium alloy, and then using anhydrous ethanol ultrasonic cleaning and deionized water cleaning; S2. Alkaline washing and degreasing: using the saponification of alkaline solution to remove the oil stains on the surface of the AZ91D magnesium alloy after polishing in step S1, the composition of the alkaline solution is 30-50 g / L of sodium hydroxide, 30-35 g / L of sodium phosphate, and 10-12 g / L of sodium carbonate, and the alkaline washing is carried out at 60-70°C for 15-20 min and then washed with deionized water; S3. Pickling: Pickle the AZ91D magnesium alloy after alkali washing and degreasing in step S2, 80-90wt%, concentration 580-620cm 3 / L phosphoric acid solution pickling for 35 to 45 seconds to remove oxides on the surface of AZ91D magnesium alloy, and then rinse with deionized water; S4. Surface conditioning: Surface conditioning the pickled AZ91D magnesium alloy at 65-70°C for 2-2.5 min using a pyrophosphate system to remove the oxides produced in step S3 and slightly etch the β phase of the AZ91D magnesium alloy to level the surface, so that the AZ91D magnesium alloy is fully exposed, the surface conditioning solution includes 150-170 g / L potassium pyrophosphate, 18-22 g / L sodium carbonate, and 8-12 g / L potassium fluoride, and the surface conditioning is followed by washing with deionized water; S5. Activation: Activate the AZ91D magnesium alloy after surface conditioning in step S4; place the AZ91D magnesium alloy after surface conditioning in a mixed solution of phosphoric acid and ammonium bifluoride and activate it at room temperature for 1 to 2 minutes, the volume ratio of phosphoric acid to ammonium bifluoride being 2 to 3:1 to 2; remove oxides and generate a magnesium fluoride protective film layer, and wash with deionized water after activation; the phosphoric acid is preferably 170 to 190 mL / L; the ammonium bifluoride is preferably 90 to 100 g / L. S6. Alkaline chemical plating: the AZ91D magnesium alloy activated in step S5 is subjected to alkaline chemical plating, the alkaline chemical plating solution comprises: nickel sulfate 20-25g / L, sodium hypophosphite 20-25g / L, sodium citrate 18-22g / L, ammonium bifluoride 10-12g / L, sodium carbonate 18-22g / L; the plating process is: the plating temperature is 70-75°C, the pH is adjusted to 9.20-9.60 with appropriate amount of ammonia water, the plating time is 40-50min, and the magnetic stirring rate is 210-280r / min; S7. Acid chemical plating: Acid chemical plating is performed on the AZ91D magnesium alloy after the alkaline chemical plating in step S6, and the acid chemical plating solution includes: 20-25 g / L nickel sulfate, 20-25 g / L sodium hypophosphite, 4-6 g / L citric acid, and 18-22 g / L ammonium bifluoride; the plating process is: the plating temperature is 80-85°C, the pH is adjusted to 6.00-6.25 with an appropriate amount of ammonia water, the plating time is 40-50 min, and the magnetic stirring rate is 210-280 r / min; S8. Prepare a basic plating solution: The basic plating solution components are: nickel sulfate 100-160g / L, ammonium citrate 6-15g / L, ammonium bifluoride 30-50g / L, saccharin sodium 1-3g / L, sodium dodecyl sulfate 0.1-0.2g / L; S9. Ultrafine grinding: The diameter of the agarwood particles reaches 200nm~500nm after being processed by a high-speed intelligent grinder; S10. Prepare the electroplating solution: mix the ultrafinely crushed agarwood particles and Tween20 in step S9 with deionized water to obtain a mixed solution, and apply magnetic stirring, mechanical stirring and ultrasonic waves to fully disperse the mixed solution, and add the dispersed mixed solution to the basic plating solution prepared in step S8; after mixing, place it in an ultrasonic field again and add mechanical stirring to continue dispersing, and obtain the electroplating solution required for preparing the nickel-based agarwood particle composite electrodeposition layer on the surface of AZ91D magnesium alloy; S11. Electrodeposition: The anode nickel plate and the AZ91D magnesium alloy after the acid chemical plating in step S7 are immersed in the electroplating solution prepared in step S10 as cathodes, and then a pulse power supply and an ultrasonic generator are connected between the cathode and the anode for electroplating; the electroplating process is: voltage 2 to 4V, current density 1.5 to 3A·cm -2 , duty cycle 35-80%, ultrasonic power 150-240W, ultrasonic frequency 45KHZ and 80KHZ alternating for 10-20s, mechanical stirring speed 150r / min-400r / min, deposition temperature 45-50℃, deposition time 20-70min, and finally prepare a nickel-based composite electrodeposition layer on the surface of AZ91D magnesium alloy with added agarwood particles.

5. The method for preparing the composite electrodeposition layer of nickel-based agarwood particles on the surface of magnesium alloy as claimed in claim 4, characterized in that: In step S10, magnetic stirring, mechanical stirring and ultrasonic stirring are applied to the agarwood particles and Tween20 mixture to fully disperse them. The process conditions are: magnetic stirring rate is 300r / min, action time is 10min; mechanical stirring speed is 300r / min, ultrasonic power is 210W, and action time is 20min.

6. The method for preparing the composite electrodeposition layer of nickel-based agarwood particles on the surface of magnesium alloy as claimed in claim 4, characterized in that: In step S10, the dispersed mixed solution is added to the basic plating solution prepared in step S8, mixed, and then placed in an ultrasonic field again with mechanical stirring to continue dispersion. The process conditions are: mechanical stirring speed of 300r / min, ultrasonic power of 210W, and action time of 10min.

7. The method for preparing the nickel-based agarwood particle composite electrodeposition layer on the surface of magnesium alloy as claimed in claim 4, characterized in that: In step S11, the anode and cathode are immersed in the electroplating solution, the anode and cathode area ratio is 1-2:2-3, and the inter-electrode distance is 25 mm.

8. The method for preparing the composite electrodeposition layer of nickel-based agarwood particles on the surface of magnesium alloy as claimed in claim 4, characterized in that: In step S11, the electrodeposition process is performed with a current density of 2A·cm -2 , duty cycle 80%, ultrasonic power 210W, ultrasonic frequency 45KHZ and 80KHZ alternating action time 10s and 20s, mechanical stirring speed 300r / min.

9. The method for preparing a composite electrodeposition layer of nickel-based agarwood particles on a magnesium alloy surface as claimed in claim 4, characterized in that: In step S4, the surface conditioning solution is 160 g / L potassium pyrophosphate, 20 g / L sodium carbonate, and 11 g / L potassium fluoride, and the surface conditioning conditions are a surface conditioning temperature of 70° C. and a time of 2.5 min.

10. The method for preparing the composite electrodeposition layer of nickel-based agarwood particles on the surface of magnesium alloy as claimed in claim 4, characterized in that: In step S8, a basic plating solution is prepared, wherein the basic plating solution is 120 g / L nickel sulfate, 10 g / L ammonium citrate, 40 g / L ammonium bifluoride, 3 g / L sodium saccharin, and 0.1 g / L sodium dodecyl sulfate.