Antimony-doped single crystal pulling process method
By optimizing the doping process, melting power, and other parameters in the antimony-doped single crystal pulling process, the problem of resistance difference caused by antimony metal doping was solved, thereby improving the production efficiency and yield of silicon wafers.
Patent Information
- Application Number
- CN202411065136.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
In the monocrystalline silicon crystal pulling process, when antimony metal is used for doping, there are large differences in the resistance of crystal rods in different furnaces, with the resistance difference between the head and tail exceeding 0.2Ω, which affects the silicon wafer production efficiency and yield.
By adjusting parameters such as doping process, melting power, crucible rotation, furnace pressure and argon flow rate, the antimony-doped single crystal pulling process is optimized to ensure that the resistance difference between the head and tail of a single crystal rod is less than 0.1Ω.
This reduces the difference in resistivity of monocrystalline silicon between different furnaces, thereby improving the production efficiency and yield of silicon wafers.
Smart Images

Figure BDA0004979130780000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of single crystal silicon manufacturing, and in particular to a crystal pulling process method for antimony-doped single crystals. Background Art
[0002] At present, in the single crystal silicon pulling process, because the segregation coefficient of antimony metal is 0.023<1 and it is extremely volatile, when antimony metal is used for single crystal pulling while the existing phosphorus-doped crystal pulling process remains unchanged, there is a large difference in the resistance of the crystal rods on different furnaces, and the resistance of a single crystal rod decreases in the early stage and increases in the later stage. The resistance difference between the head and the tail is >0.2Ω, which affects the production efficiency and yield of silicon wafers.
[0003] Patent technical document CN202110984273.4 discloses a single crystal silicon crystal pulling process method, which includes using a low furnace pressure of no more than 18Torr in the single crystal furnace during the equal diameter stage of crystal growth, and gradually reducing the furnace pressure of the single crystal furnace as the length of the crystal rod increases during the equal diameter stage of crystal growth. The flow rate of argon gas introduced into the single crystal furnace is kept within a constant range, so that the axial resistivity attenuation slope of the single crystal doped with volatile dopants, especially gallium, can be reduced, and its resistivity effective length can be increased. However, when doping with antimony metal, it is still inevitable that the head-to-tail resistance difference is large.
[0004] To this end, the present invention provides a method for pulling antimony-doped single crystals. By adjusting the doping process, melt power, crucible rotation, furnace pressure and argon gas flow during crystal pulling, the resistance difference between different furnaces is reduced and the resistance difference between the head and tail of a single crystal rod is less than 0.1Ω. Summary of the invention
[0005] In view of this, the purpose of the present invention is to propose an antimony-doped single crystal pulling process method, and to provide an antimony-doped single crystal pulling process method, so that the resistance difference between the head and tail of the final single crystal rod is less than 0.1Ω.
[0006] Based on the above purpose, the present invention provides an antimony-doped single crystal pulling process method, including melting material, doping, seeding, shouldering and equal diameter;
[0007] Furthermore, the number of barrels added is the last barrel, and the last barrel added can shorten the antimony melting time and reduce the volatilization of the antimony alloy.
[0008] Furthermore, when the last barrel is added, the melt power is adjusted from 100-110kW to 80-90kW, and the furnace pressure is adjusted from 5-7torr to 15-20torr. The purpose is to reduce the volatilization time of molten antimony, lower the temperature in the antimony melting furnace and increase the furnace pressure during the melting process to reduce the impact of different furnaces on the volatilization of antimony alloys.
[0009] Furthermore, when the equal diameter length is between 0-500 mm, the argon flow rate is 90-100 slpm, the furnace pressure is 5-8 torr, and the crucible rotation speed is 5.5-6 r / min.
[0010] Furthermore, when the equal-diameter length is between 500mm and the end of crystal pulling, the argon flow rate is adjusted from 90-100slpm to 70-80slpm, and the furnace pressure is adjusted from 5-8torr to 11-13torr. The purpose is to reduce the volatilization of the doped antimony alloy in the later stage of equal-diameter and ensure the resistance consistency of the crystal rod in the later stage of crystal pulling; the crucible rotation is adjusted from 5.5-6r / min to 4-5slpm. The purpose is to balance the increase in oxygen content caused by the increase in furnace pressure, so that the oxygen content can be controlled.
[0011] Furthermore, the power of the melt is 100-110 kW and the furnace pressure is 5-7 torr.
[0012] Furthermore, the doping is antimony metal doping.
[0013] Furthermore, the last barrel is the last barrel to which the single crystal furnace is charged.
[0014] Furthermore, when the crystal induction and shoulder release start, the argon flow rate is adjusted from 70-80slpm to 90-100slpm, and the furnace pressure is adjusted from 11-13torr to 5-8torr, in order to accelerate the volatilization of the doped antimony alloy and ensure the resistance consistency of the early crystal pulling crystal rod; the crucible rotation is adjusted from 4.5-5r / min to 5.5-6r / min, in order to ensure crystallization and controllable oxygen content.
[0015] Furthermore, the argon flow rate is adjusted from 90-100 slpm to 70-80 slpm, the furnace pressure is adjusted from 5-8 torr to 11-13 torr, and the crucible speed is adjusted from 5.5-6 r / min to 4-5 slpm, and the process is completed when the equal diameter length is between 500-1000 mm.
[0016] Beneficial effects of the present invention: The present invention achieves the reduction of resistivity differences of single crystal silicon grown between different furnaces by regulating the power of the doping process, the melting process, the crucible rotation, the furnace pressure and the argon flow rate during crystal pulling, and the various processes cooperate with each other, thereby achieving the goal of reducing the resistance difference between the head and tail of a single crystal rod <0.1Ω, thereby improving the production efficiency and yield of silicon wafers. DETAILED DESCRIPTION
[0017] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0018] Embodiment: Crystal pulling is performed in a 36-inch hot field, with a total feed of 600 kg.
[0019] (1) Material preparation: After receiving the material report from the site, loading and doping are carried out. Antimony alloy is doped in the last barrel of material added to the single crystal furnace;
[0020] (2) During normal production, adjust the main power to 110kw and the furnace pressure to 5torr for melting;
[0021] (3) When adding the last barrel of material, adjust the main power to 80 kW and the furnace pressure to 20 torr to melt the material;
[0022] (4) After the addition of materials is completed, the temperature is adjusted, and after the temperature adjustment is completed, seeding is performed;
[0023] (5) Seeding process: the crucible speed was adjusted to 5.5 r / min, the argon flow rate was adjusted to 100 slpm, and the furnace pressure was adjusted to 5 torr for seeding;
[0024] (6) Shoulder release process: the crucible speed is adjusted to 5.5 r / min, the argon flow rate is adjusted to 100 slpm, and the furnace pressure is adjusted to 5 torr for shoulder release;
[0025] (7) Equal diameter process: When the equal diameter length is 0-500 mm: the crucible speed is 5.5 r / min, the argon flow rate is 100 slpm, the furnace pressure is 5 torr, and the crystal is pulled at normal pulling speed;
[0026] (8) When the equal diameter length is 500-1000 mm: the crucible rotation speed is adjusted from 5.5 r / min to 4.5 r / min, the argon flow rate is adjusted from 100 slpm to 80 slpm, and the furnace pressure is adjusted from 5 torr to 13 torr, and crystal pulling is performed at normal pulling speed;
[0027] (9) After the equal diameter length reaches 1000 mm: the crucible rotation is maintained at 4.5 r / min, the argon flow rate is maintained at 80 slpm, the furnace pressure is maintained at 13 torr, and crystal pulling is performed at normal pulling speed;
[0028] (10) After the diameter is equalized, the finishing is carried out normally and the crystal rod is taken out for data inspection.
[0029] After testing, the final single crystal N-type silicon rod has a head resistance of 1.01Ω, a tail resistivity difference of 1.03Ω, and a final single crystal N-type silicon rod has a head resistivity difference of 0.02Ω.
[0030] Table 1 Variation table of equal diameter process parameters
[0031] Length(mm) Argon gas flow rate (slpm) Crucible speed (r / min) Furnace pressure (torr) 0 100 5.5 5 80 100 5.5 5 150 100 5.5 5 300 100 5.5 5 500 100 5.5 5 800 90 5 8 1100 80 4.5 13 1600 80 4.5 13 2200 80 4.5 13 2800 80 4.5 13 3400 80 4.5 13 4000 80 4.5 13
[0032] Table 2 Melt process parameter changes
[0033]
[0034] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0035] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for pulling an antimony-doped single crystal, characterized in that: Including melt, doping, seeding, shouldering and equal diameter; the number of barrels for doping is the last barrel; when the last barrel is doped, the melt power is adjusted from 100-110kW to 80-90kW, and the furnace pressure is adjusted from 5-7torr to 15-20torr; When the equal diameter length is between 0-500 mm, the argon flow rate is 90-100 slpm, the furnace pressure is 5-8 torr, and the crucible rotation speed is 5.5-6 r / min; When the equal diameter length is between 500 mm and the end of crystal pulling, the argon flow rate is adjusted from 90-100 slpm to 70-80 slpm, the furnace pressure is adjusted from 5-8 torr to 11-13 torr, and the crucible rotation speed is adjusted from 5.5-6 r / min to 4-5 slpm.
2. The antimony-doped single crystal pulling process according to claim 1, characterized in that: The power of the melt is 100-110 kW and the furnace pressure is 5-7 torr.
3. The antimony-doped single crystal pulling process according to claim 1, characterized in that: The doping is antimony metal doping.
4. The antimony-doped single crystal pulling process according to claim 1, characterized in that: The last barrel is the last barrel to be charged into the single crystal furnace.
5. The antimony-doped single crystal pulling process according to claim 1, characterized in that: When the seeding and shouldering process begins, the argon flow rate is adjusted from 70-80 slpm to 90-100 slpm, the furnace pressure is adjusted from 11-13 torr to 5-8 torr, and the crucible speed is adjusted from 4.5-5 r / min to 5.5-6 r / min.
6. The antimony-doped single crystal pulling process according to claim 1, characterized in that: The argon flow rate is adjusted from 90-100 slpm to 70-80 slpm, the furnace pressure is adjusted from 5-8 torr to 11-13 torr, and the crucible speed is adjusted from 5.5-6 r / min to 4-5 slpm, and the process is completed when the equal diameter length is between 500-1000 mm.