Photoelectric dual-mode stress-strain sensing fiber and preparation method thereof
The preparation of hard-core soft-shell structure photonic crystal microspheres through wet spinning and seed emulsion polymerization has solved the problem of difficulty in combining traditional hard photonic crystal microspheres with electrosensing fibers, and realized photoelectric dual-mode stress-strain sensing fibers Easy preparation and high sensitivity, suitable for human movement monitoring.
Patent Information
- Application Number
- CN202411006576.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-25
AI Technical Summary
It is difficult for traditional hard photonic crystal microspheres to directly combine with electrosensing fibers, and the addition of adhesive materials affects the tensile properties of the fibers, resulting in complex and unstable preparation of photoelectric dual-mode sensing fibers.
Thermoplastic polyurethane-based electrosensing fibers were continuously prepared by wet spinning, and hard-core soft-shell structure photonic crystal microspheres were prepared by seed emulsion polymerization, and dip them on the electrosensing fibers to form photoelectric dual-mode stress-strain sensing fibers.
It realizes the simple and rapid preparation of photoelectric dual-mode stress-strain sensing fibers, avoids the influence of adhesion materials on electrical and optical signals, improves biocompatibility and sensitivity, and is suitable for human motion monitoring.
Smart Images

Figure CN118957799A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material engineering, and in particular relates to a photoelectric dual-mode stress-strain sensing fiber and a preparation method thereof. Background Art
[0002] In sensors with optoelectronic dual-signal responses, the optical signal provides direct visual information, while the electrical signal provides accurate strain quantification. Currently, various optical materials have been developed for strain sensing, such as organic light-emitting diodes, inorganic phosphors, organic chromophores, photonic crystals, etc. Among these materials, mechanochromic photonic crystals are considered to be one of the most promising candidates, mainly because they can produce instant and intuitive dynamic optical signal responses without consuming any energy. On the other hand, the strain-related electrical signal can be used as an effective indicator for quantifying deformation. In particular, highly sensitive electronic strain sensors have been widely explored in monitoring human motion with small strains. By combining mechanochromic photonic crystals with highly sensitive electronic strain sensors, some interactive wearable devices with optical / electrical dual-signal outputs have been realized for monitoring human motion.
[0003] When traditional hard photonic crystal microspheres (such as polystyrene, polymethyl methacrylate, and silicon dioxide) are directly used as optical signal sensors, they have a deformation variable of less than 1% and poor biocompatibility, making it difficult to meet the requirements of flexibility and stretchability in the wearable field. At present, electrical sensing fibers cannot be directly combined with traditional hard photonic crystal microspheres, and there is no effective bonding or adhesion between the fibers and the microspheres; at the same time, there is no way for the microspheres to directly form a strong interaction without other media, which makes it difficult to prepare fiber-based optoelectronic dual-mode stress and strain sensors.
[0004] When further selecting the adhesion medium, not only should the photonic crystal layer be elastic, but also the adhesion between it and the electrical sensing fiber should not affect the electrical sensing effect, which further increases the difficulty of preparing fiber-type photoelectric dual-mode stress and strain sensors. Zhao et al. mixed SiO2 with polyethylene glycol phenyl ether acrylate (PEGPEA), injected the mixed solution into a capillary, used the capillary as a template to initiate polymerization under ultraviolet light to form an optical signal sensing fiber, and then sealed the ion conductive gel to prepare the photoelectric dual-mode stress and strain sensing fiber. This preparation method is not only complicated, but also the gel-type fiber is easily exposed to the air, which can easily cause unstable signal transmission, which is very unfavorable for use in an in vitro environment (Zhao RL, He Y, He Y, et al. Dual-Mode Fiber Strain Sensor Based on MechanochromicPhotonic Crystal and Transparent Conductive Elastomer for Human MotionDetection[J]. ACS Applied Materials&Interfaces, 2023, 15(12): 16063-16071.).
[0005] The preparation steps of fiber-based photoelectric dual-mode sensors are very complicated. How to simply and quickly prepare photoelectric dual-mode sensing fibers is an urgent problem to be solved. Summary of the invention
[0006] Technical issues:
[0007] Directly combining traditional hard photonic crystal microspheres with electrical sensing fibers cannot produce optoelectronic dual-mode sensing fibers, while adding adhesive materials will affect the tensile properties of the fiber's optoelectronic layers, thereby affecting the optoelectronic dual-mode sensing performance.
[0008] Technical solution:
[0009] In order to solve the above problems, the present invention first adopts wet spinning to continuously prepare TPU (thermoplastic polyurethane)-based electrical sensing fibers as electrical signal sensing modules, then synthesizes hard-core and soft-shell structured photonic crystal microspheres that can form their own elastic membranes as optical signal sensing modules, and finally dips the TPU electrical sensing fibers into hard-core and soft-shell structured photonic crystal microsphere emulsion to realize the rapid preparation of optoelectronic dual-mode sensing fibers.
[0010] The purpose of the present invention is to provide a photoelectric dual-mode stress-strain sensing fiber and a preparation method thereof. The method is simple and convenient and can realize the continuous preparation of the photoelectric dual-mode stress-strain sensing fiber.
[0011] In addition, the present invention also provides the application of the photoelectric dual-mode stress-strain sensing fiber in sensing.
[0012] In order to achieve the aforementioned invention object, the present invention adopts the following technical solutions:
[0013] The present invention provides a photoelectric dual-mode stress-strain sensing fiber, comprising a TPU electrical sensing fiber core layer and a light sensing cortex formed by hard-core and soft-shell photonic crystal microspheres, wherein the hard-core and soft-shell photonic crystal microspheres can self-assemble and form a light sensing elastic film, display structural color, and thus realize light signal sensing under stress and strain.
[0014] The present invention also provides a method for preparing the photoelectric dual-mode stress-strain sensing fiber, comprising the following steps:
[0015] S1, dispersing TPU in DMF, mixing, and obtaining TPU / DMF spinning solution;
[0016] S2, dispersing the conductive material in DMF, mixing, and obtaining a DMF dispersion of the conductive material;
[0017] S3, mixing the TPU / DMF spinning solution obtained in S1 with the conductive material DMF dispersion obtained in S2, loading the mixture into a syringe and preparing a TPU electric sensing fiber by wet spinning;
[0018] S4, preparing a photonic crystal microsphere emulsion with a hard core and soft shell structure by seed emulsion polymerization;
[0019] S5, dip-coating the TPU electric sensing fiber prepared in S3 into the hard-core soft-shell photonic crystal microsphere emulsion prepared in S4, then taking out and drying, to obtain an optoelectronic dual-mode stress-strain sensing fiber;
[0020] The method for preparing the photonic crystal microsphere emulsion with a hard core and soft shell structure in S4 comprises:
[0021] (a) emulsifying a portion of a hard core monomer, a crosslinking agent, an emulsifier, and water, and then adding an initiator to react to obtain a polymer seed emulsion;
[0022] (b) adding another portion of the hard core monomer, the crosslinking agent, and the initiator to the obtained polymer seed emulsion, and polymerizing to obtain a hard core microsphere system;
[0023] (c) adding a soft shell monomer, a crosslinking agent, and an initiator to the obtained hard core microsphere system to initiate polymerization, thereby obtaining a photonic crystal microsphere emulsion with a hard core and a soft shell structure.
[0024] The hard core monomer is one or more of styrene (St), methyl methacrylate (MMA) and acrylonitrile (AN).
[0025] The soft shell monomer is selected from:
[0026] ① Ethyl acrylate (EA), or
[0027] ② A combination of ethyl acrylate (EA) and butyl acrylate (BA), or
[0028] ③ Combination of methyl methacrylate (MMA) and butyl acrylate (BA).
[0029] In one embodiment of the present invention, the mass ratio of ethyl acrylate (EA) to butyl acrylate (BA) in the soft shell monomer is (19-20):(0-1).
[0030] In one embodiment of the present invention, the mass ratio of methyl methacrylate (MMA) to butyl acrylate (BA) in the soft shell monomer is 1:3.
[0031] In one embodiment of the present invention, step S1, adding TPU into DMF, and magnetically stirring at room temperature for 4 hours to obtain TPU / DMF spinning solution.
[0032] In one embodiment of the present invention, in step S1, TPU is thermoplastic polyurethane, DMF is N,N-dimethylformamide, and the concentration of TPU / DMF spinning solution is 15-25 wt.%, more preferably 20-22.5 wt.%.
[0033] In one embodiment of the present invention, in step S2, a conductive material is added into DMF, and a conductive material DMF dispersion is obtained by ultrasonic dispersion.
[0034] In one embodiment of the present invention, the conductive material in step S2 can be one or more of conductive carbon black (CB), graphene oxide (GO), reduced graphene oxide (rGO), carbon nanotubes (CNTs), MXene, silver nanowires (AgNWs), silver nanoparticles (AgNPs) and the like.
[0035] In one embodiment of the present invention, the concentration of the conductive material DMF dispersion in step S2 is 10-40 mg / mL, more preferably 30-40 mg / mL.
[0036] In one embodiment of the present invention, in step S3, the TPU / DMF solution in steps S1 and S2 and the conductive material DMF dispersion are mixed in a ratio of 1:1, loaded into a syringe and prepared by wet spinning to obtain TPU electrical sensing fiber, and the coagulation bath is an isopropyl alcohol, water and calcium chloride mixed solution (IPA:H2O=1:2, 5wt.% CaCl2).
[0037] In one embodiment of the present invention, step S4, preparing photonic crystal microspheres with a hard core and soft shell structure by seed emulsion polymerization:
[0038] First, the hard monomer, crosslinking agent, emulsifier and water are emulsified for a certain time, and then an initiator is added to initiate polymerization under certain temperature conditions to obtain a polymer seed emulsion, wherein the particle size of the polymer seed is about 120nm, the polymer dispersibility index (PDI) is less than 0.08, the emulsification time is 10-30min, the temperature is 70-85°C, and the polymerization time is 1-1.5h;
[0039] Secondly, hard monomer, crosslinking agent and initiator are added again to initiate polymerization to obtain hard core microspheres with a particle size of about 170-220 nm and a PDI of less than 0.08, wherein the polymerization time is 1.5-2.5 h;
[0040] One or more soft monomers or a certain proportion of soft and hard monomers, a crosslinking agent, and an initiator are added to the reaction system to initiate polymerization to obtain hard-core soft-shell photonic crystal microspheres with a particle size of about 200-300 and a PDI of less than 0.08, wherein the polymerization time is 1.5-2.5 hours.
[0041] In one embodiment of the present invention, the syringe used in step S3 is a 10 mL injection needle, the wet spinning injection rate is 50-80 mL / min, and the spinneret hole size is 15-18G.
[0042] In one embodiment of the present invention, in step S4, the mass ratio of the hard core monomer in (a) to the hard core monomer in (b) is 1:(1-2). Specifically, it can be 1:1.5.
[0043] In one embodiment of the present invention, in step S4, the emulsifier used for emulsification is one of sodium dodecyl sulfate (SDS), sodium dodecylbenzene sulfonate, and sodium dodecyl sulfonate.
[0044] In one embodiment of the present invention, in step S4, the emulsifier accounts for 0.15-0.25wt.% of the total monomer concentration; specifically, 0.2wt.% can be selected. (Total monomer refers to the total mass of the hard core monomer and the soft shell monomer)
[0045] In one embodiment of the present invention, in step S4, the cross-linking agent may be one or more of diene cross-linking agents such as divinylbenzene (DVB), allyl methacrylate (ALMA), and isoprene.
[0046] In one embodiment of the present invention, in step S4, the amount of the cross-linking agent in (a) or (b) relative to the hard core in this step is 10-14 wt.%.
[0047] In one embodiment of the present invention, in step S4, the amount of the crosslinking agent in (c) relative to the soft shell monomer in this step is 0.2-1.0 wt.%.
[0048] In one embodiment of the present invention, in step S4, the initiator may also be one or more of ammonium persulfate (APS), potassium persulfate, and sodium persulfate.
[0049] In one embodiment of the present invention, in step S4, the ratio of initiator to monomer in (a), (b) or (c) is 0.5-1 wt. %.
[0050] In one embodiment of the present invention, the dipping time in step S5 is 10-60 seconds, and the drying time is 10-60 seconds.
[0051] The present invention provides a photoelectric dual-mode stress-strain sensing fiber based on the above method.
[0052] The present invention also provides application of the photoelectric dual-mode stress-strain sensing fiber in preparing a photoelectric signal sensing component.
[0053] The present invention also provides the application of the photoelectric dual-mode stress-strain sensing fiber in the construction of a human joint motion monitoring product.
[0054] Beneficial effects of the present invention:
[0055] The preparation method of the photoelectric dual-mode stress-strain sensing fiber prepared by the present invention is simple and rapid, easy to continuously produce, and does not need to add additional adhesive materials, thereby avoiding the influence of the adhesive materials on electrical signal sensing and optical signal sensing; the thermoplastic polyurethane has good biocompatibility, and the photonic crystal layer is not only non-toxic but also can better protect the internal electrical sensing layer; the TPU electrical sensing fiber is distributed with a large number of holes, which can improve the electrical signal sensing sensitivity and can monitor small-amplitude movements; the optical signal sensing layer is affected by the soft shell layer and has good elasticity, and can change the spacing between the photonic crystal microspheres when subjected to stress and strain, thereby causing changes in the optical signal. These characteristics make the photoelectric dual-mode stress-strain sensing fiber have broad application prospects in the field of human body movement monitoring. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 It is a flow chart of the method for preparing the photoelectric dual-mode stress-strain sensing fiber of the present invention;
[0057] Figure 2 Electron micrograph of the MXene / TPU fiber and optoelectronic dual-mode stress-strain sensing fiber provided in Example 2. DETAILED DESCRIPTION
[0058] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with some embodiments, but the following examples are not used to limit the present invention.
[0059] Test method:
[0060] Electrical signal sensing test: The photoelectric dual-mode stress-strain sensing fiber is clamped in an electronic universal material testing machine with a spacing of 10 mm. Copper wires are connected from both ends and connected to a desktop digital multimeter via a wire to test the resistance change caused by the fiber being stretched:
[0061]
[0062] Where GF is the sensor sensitivity, R is the stretch resistance, R0 is the initial resistance, and ε is the strain
[0063] Optical signal sensing test: Fix the optoelectronic dual-mode stress-strain sensing fiber and use a fiber optic spectrometer to test the spectral changes caused by fiber stretching.
[0064] Embodiment 1:
[0065] Step S1, TPU / DMF spinning solution preparation: 2.25 g of TPU particles were weighed, added into 7.75 g of DMF solution, and magnetically stirred for 4 h to obtain 22.5 wt.% TPU / DMF spinning solution.
[0066] Step S2, preparation of Ti3C2Tx MXene DMF dispersion: 400 mg of MXene was added to 10 mL of DMF solution for ultrasonic dispersion to obtain a MXene / DMF dispersion with a concentration of 40 mg / mL.
[0067] Step S3, preparation of MXene / TPU fiber: The prepared 22.5wt.% TPU / DMF spinning solution and 40mg / mLMXene / DMF dispersion were mixed in a volume ratio of 1:1, mixed by a vortex mixer for 10min, and then ultrasonically mixed for 10min to obtain a uniform MXene / TPU / DMF spinning solution, and the spinning solution was loaded into a 10mL syringe with a spinneret of 16G, and the spinning solution was injected into a coagulation bath (IPA:H2O=1:2, 5wt.%CaCl2) by a syringe pump (injection rate of 80mL) to coagulate to obtain porous MXene / TPU fiber.
[0068] Step S4, preparation of PS@P(MMA-BA) core-shell structure photonic crystal microspheres:
[0069] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0070] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.
[0071] (3) 5 g MMA, 15 g BA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (MMA-BA) photonic crystal microsphere emulsion with a particle size of about 300 nm.
[0072] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PS@P (MMA-BA) emulsion was added to a culture dish, and the porous MXene / TPU fiber was immersed therein. After 10 seconds, the fiber was taken out and placed in an oven at 60°C for 30 seconds to be dried. The red photoelectric dual-mode stress-strain sensing fiber was taken out.
[0073] Embodiment 2:
[0074] Steps S1, S2 and S3 are the same as those in Example 1.
[0075] Step S4, preparation of PS@P(MMA-BA) core-shell structure photonic crystal microspheres:
[0076] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.066 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0077] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 200 nm.
[0078] (3) 5 g MMA, 15 g BA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (MMA-BA) photonic crystal microsphere emulsion with a particle size of about 280 nm.
[0079] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PS@P (MMA-BA) emulsion was added to a culture dish, and the porous MXene / TPU fiber was immersed therein. After 10 seconds, the fiber was taken out and placed in an oven at 60°C for 30 seconds to be dried. The green photoelectric dual-mode stress-strain sensing fiber was taken out.
[0080] Embodiment 3:
[0081] Step S1 is the same as in Example 1
[0082] Step S2, preparation of rGO DMF dispersion: 400 mg rGO was added into 10 mL DMF solution for ultrasonic dispersion to obtain rGO / DMF dispersion with a concentration of 40 mg / mL.
[0083] Step S3, preparation of rGO / TPU fiber: the experimental method is the same as that of Example 1.
[0084] Step S4, preparation of PS@P(EA-BA) core-shell structure photonic crystal microspheres:
[0085] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.066 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0086] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 200 nm.
[0087] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion with a particle size of about 280 nm.
[0088] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PS@P(EA-BA) emulsion was added to a culture dish, and the porous rGO / TPU fiber was immersed therein. After 10 seconds, the fiber was taken out and placed in an oven at 60°C to dry for 30 seconds, and the green photoelectric dual-mode stress-strain sensing fiber was taken out.
[0089] Embodiment 4:
[0090] Step S1 is the same as in Example 1
[0091] Step S2, preparation of CB / MXene DMF dispersion: 200 mg CB and 200 mg MXene were added to 10 mL of DMF solution for ultrasonic dispersion to obtain a CB / MXene / DMF dispersion with a conductive material concentration of 40 mg / mL.
[0092] Step S3, preparation of CB / MXene / TPU fiber: the experimental method is the same as that in Example 1.
[0093] Step S4, preparation of PAN@P(EA-BA) core-shell structure photonic crystal microspheres:
[0094] (1) 5 g of AN and 0.5 g of DVB were added to 100 mL of deionized water containing 0.066 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PAN seeds with a particle size of more than 120 nm.
[0095] (2) 7.5 g AN and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PAN core with a particle size of about 200 nm.
[0096] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PAN@P (EA-BA) photonic crystal microsphere emulsion with a particle size of about 280 nm.
[0097] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PAN@P(EA-BA) emulsion was added to a culture dish, and the porous CB / MXene / TPU fiber was immersed therein. After 10 seconds, the fiber was taken out and placed in an oven at 60°C for 30 seconds to be dried. The green photoelectric dual-mode stress-strain sensing fiber was taken out.
[0098] Embodiment 5:
[0099] Step S1 is the same as in Example 1
[0100] Step S2, preparation of AgNWs / MXene DMF dispersion: 200 mg of AgNWs and 200 mg of MXene were added into 10 mL of DMF solution for ultrasonic dispersion to obtain an AgNWs / MXene / DMF dispersion with a conductive material concentration of 40 mg / mL.
[0101] Step S3, preparation of AgNWs / MXene / TPU fibers: the experimental method is the same as that in Example 1.
[0102] Step S4, preparation of PS@PEA core-shell structure photonic crystal microspheres:
[0103] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0104] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.
[0105] (3) 20 g EA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@PEA photonic crystal microsphere emulsion with a particle size of about 300 nm.
[0106] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PS@PEA emulsion was added to a culture dish, and the porous AgNWs / MXene / TPU fiber was immersed therein. After 10 seconds, the fiber was taken out and placed in an oven at 60°C to dry for 30 seconds. The red photoelectric dual-mode stress-strain sensing fiber was taken out.
[0107] Embodiment 6:
[0108] Step S1 is the same as in Example 1
[0109] Step S2, preparation of AgNPs / MXene DMF dispersion: 200 mg of AgNPs and 200 mg of MXene were added to 10 mL of DMF solution for ultrasonic dispersion to obtain an AgNPs / MXene / DMF dispersion with a conductive material concentration of 40 mg / mL.
[0110] Step S3, preparation of AgNPs / MXene / TPU fibers: the experimental method is the same as that in Example 1.
[0111] Step S4, preparation of PMMA@P(EA-BA) core-shell structure photonic crystal microspheres:
[0112] (1) 5 g of MMA and 0.5 g of DVB were added to 100 mL of deionized water containing 0.066 g of SDS, and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PMMA seeds with a particle size of more than 120 nm.
[0113] (2) 7.5 g MMA and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PMMA core with a particle size of about 200 nm.
[0114] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PMMA@P(EA-BA) photonic crystal microsphere emulsion with a particle size of about 280 nm.
[0115] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PMMA@P(EA-BA) emulsion was added to a culture dish, and the porous AgNPs / MXene / TPU fiber was immersed therein. After 10 seconds, the fiber was taken out and placed in an oven at 60°C for 30 seconds to be dried. The green photoelectric dual-mode stress-strain sensing fiber was taken out.
[0116] Comparative Example 1:
[0117] Step S1 is the same as in Example 1
[0118] Step S2, prepare 10 mg / mL MXene / DMF dispersion, the method is the same as Example 1
[0119] Step S3, preparation of MXene / TPU fiber, the method is the same as Example 1
[0120] Step S4,
[0121] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0122] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.
[0123] Step S5, preparation of photoelectric dual-mode stress and strain sensing fiber: 10 mL of PS emulsion was added to a centrifuge tube, and the porous MXene / TPU fiber was immersed in the centrifuge tube. After 10 seconds, it was lifted up and placed in an oven at 60°C for 30 seconds to dry. The hard-shell photoelectric dual-mode stress and strain sensing fiber was taken out.
[0124] Comparative Example 2:
[0125] Step S1, TPU / DMF spinning solution preparation: 1.5 g TPU particles were weighed, added into 8.5 g DMF solution, and magnetically stirred for 4 h to obtain 15 wt.% TPU / DMF spinning solution.
[0126] Step S2 is the same as in Example 1
[0127] Step S3, preparation of porous MXene / TPU fiber: the prepared 15wt.% TPU / DMF spinning solution and 40mg / mL MXene / DMF dispersion were mixed in a ratio of 1:1, mixed by a vortex mixer for 10min, and then ultrasonically mixed for 10min to obtain a uniform MXene / TPU / DMF spinning solution, and the spinning solution was loaded into a 10mL syringe with a spinneret of 16G, and the spinning solution was injected into a coagulation bath (IPA:H2O=1:2, 5wt.%CaCl2) by a syringe pump (injection rate of 80mL) to coagulate to obtain porous MXene / TPU fiber.
[0128] Step S4, preparation of PS@P(MMA-BA) core-shell structure photonic crystal microspheres:
[0129] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.070 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0130] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 170 nm.
[0131] (3) 5 g MMA, 15 g BA and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (MMA-BA) photonic crystal microsphere emulsion with a particle size of about 210 nm.
[0132] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PS@P (MMA-BA) emulsion was added to a culture dish, and the porous MXene / TPU fiber was immersed therein. After 10 seconds, it was taken out and placed in an oven at 60°C to dry for 30 seconds, and the purple photoelectric dual-mode stress-strain sensing fiber was taken out.
[0133] Comparative Example 3:
[0134] Step S1, TPU / DMF spinning solution preparation: weigh 2.5 g of TPU particles, add them into 7.5 g of DMF solution, and stir them magnetically for 4 hours to obtain 25 wt.% TPU / DMF spinning solution.
[0135] Step S2 is the same as in Example 1
[0136] Step S3, preparation of porous MXene / TPU fiber: The prepared 25wt.% TPU / DMF spinning solution and 40mg / mL MXene / DMF dispersion were mixed in a ratio of 1:1, mixed by a vortex mixer for 10min, and then ultrasonically mixed for 10min to obtain a uniform MXene / TPU / DMF spinning solution, and the spinning solution was loaded into a 10mL syringe with a spinneret of 16G, and the spinning solution was injected into a coagulation bath (IPA:H2O=1:2, 5wt.%CaCl2) by a syringe pump (injection rate of 80mL) to coagulate to obtain porous MXene / TPU fiber.
[0137] Step S4, preparation of PS@PBA core-shell structure photonic crystal microspheres:
[0138] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0139] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.
[0140] (3) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@PBA photonic crystal microsphere emulsion with a particle size of about 320 nm.
[0141] Step S5, preparation of photoelectric dual-mode stress-strain sensing fiber: 10 mL of PS@PBA emulsion was added to a culture dish, and the porous MXene / TPU fiber was immersed therein. After 10 seconds, the fiber was taken out and placed in an oven at 60°C to dry for 30 seconds. The white photoelectric dual-mode stress-strain sensing fiber was obtained.
[0142] Comparative Example 4:
[0143] Step S1 is the same as in Example 1
[0144] Step S2, prepare 10 mg / mL MXene / DMF dispersion, the method is the same as Example 1
[0145] Step S3, preparation of MXene / TPU fiber, the method is the same as Example 1
[0146] Step S4,
[0147] (1) 12.5 g of St and 1.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.1 g of APS was then added to initiate polymerization for 2.5 h to obtain a PS core.
[0148] (2) 19 g EA, 1 g BA and 0.04 g ALMA were added into the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion.
[0149] Step S5, preparation of photoelectric dual-mode stress and strain sensing fiber: 10 mL of PS emulsion was added to a centrifuge tube, and the porous MXene / TPU fiber was immersed in the centrifuge tube. After 10 seconds, it was lifted up and placed in an oven at 60°C for 30 seconds to dry. The hard-shell photoelectric dual-mode stress and strain sensing fiber was taken out.
[0150] Table 1. Comparison of results of Examples 1-6 and Comparative Examples 1-4
[0151]
[0152]
[0153]
[0154] Example 7: Optimization of TPU concentration in S1
[0155] S1, TPU / DMF spinning solution preparation: Weigh a certain amount of TPU particles and add them into a certain amount of DMF solution, and keep the total amount at 10 g, and stir magnetically for 4 h to obtain TPU / DMF spinning solutions of different concentrations (as shown in Table 2).
[0156] S2-S5 are the same as in Example 1.
[0157] The results are shown in Table 2.
[0158] Table 2
[0159]
[0160]
[0161] Example 8: Optimization of the concentration of conductive material in S3
[0162] S1 is the same as Example 1.
[0163] S2, preparation of Ti3C2Tx MXene DMF dispersion: A certain amount of MXene (as shown in Table 3) was added into 10 mL of DMF solution and ultrasonically dispersed to obtain a MXene / DMF dispersion of a certain concentration.
[0164] S3-S5 are the same as in Example 1.
[0165] The results are shown in Table 3.
[0166] Table 3
[0167]
[0168]
[0169] Example 9: Optimization of the combination ratio of monomers for soft shell in step S4 (3)
[0170] S1-S3 refer to Example 1, only S4 is adjusted:
[0171] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of about 120 nm.
[0172] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.05 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 220 nm.
[0173] (3) A certain amount of EA, BA (as shown in Table 4) and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (EA-BA) photonic crystal microsphere emulsion.
[0174] S5 refers to Example 1.
[0175] The results are shown in Table 4.
[0176] Table 4
[0177]
[0178]
[0179] Example 10: Optimization of the combination ratio of monomers for soft shell in step (3) of S4
[0180] S1-S3 refer to Example 1, only S4 is adjusted:
[0181] (1) 5 g of St and 0.5 g of DVB were added to 100 mL of deionized water containing 0.065 g of SDS and emulsified at 300 rpm for 30 min. The reaction temperature was then raised to 85 °C and maintained for 10 min. 0.05 g of APS was then added to initiate polymerization for 1 h to obtain PS seeds with a particle size of more than 120 nm.
[0182] (2) 7.5 g St and 1 g DVB were added to the reaction system, and then 0.08 g APS was added to initiate polymerization for 1.5 h to obtain a PS core with a particle size of about 230 nm.
[0183] (3) A certain amount of MMA, BA (as shown in Table 5) and 0.04 g ALMA were added to the reaction system, and then 0.1 g APS was added to initiate polymerization for 1.5 h to obtain a core-shell structured PS@P (MMA-BA) photonic crystal microsphere emulsion.
[0184] S5 refers to Example 1.
[0185] The results are shown in Table 5.
[0186] Table 5
[0187]
[0188] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a photoelectric dual-mode stress-strain sensing fiber. It is characterized in that The following steps are involved: S1, dispersing TPU in DMF, mixing, and obtaining TPU / DMF spinning solution; S2, dispersing the conductive material in DMF, mixing, and obtaining a DMF dispersion of the conductive material; S3, mixing the TPU / DMF spinning solution obtained in S1 with the conductive material DMF dispersion obtained in S2, loading the mixture into a syringe and preparing a TPU electric sensing fiber by wet spinning; S4, preparing a photonic crystal microsphere emulsion with a hard core and soft shell structure by seed emulsion polymerization; S5, dip-coating the TPU electric sensing fiber prepared in S3 into the hard-core soft-shell photonic crystal microsphere emulsion prepared in S4, then taking out and drying, to obtain an optoelectronic dual-mode stress-strain sensing fiber; The method for preparing the photonic crystal microsphere emulsion with a hard core and soft shell structure in S4 comprises: (a) emulsifying a portion of a hard core monomer, a crosslinking agent, an emulsifier, and water, and then adding an initiator to react to obtain a polymer seed emulsion; (b) adding another portion of the hard core monomer, the crosslinking agent, and the initiator to the obtained polymer seed emulsion, and polymerizing to obtain a hard core microsphere system; (c) adding a soft shell monomer, a crosslinking agent, and an initiator to the obtained hard core microsphere system to initiate polymerization to obtain a photonic crystal microsphere emulsion with a hard core and a soft shell structure; The hard core monomer is one or more of styrene, methyl methacrylate, and acrylonitrile; The soft shell monomer is selected from: ① Ethyl acrylate, or ② A combination of ethyl acrylate and butyl acrylate, or ③Combination of methyl methacrylate and butyl acrylate.
2. The method according to claim 1, It is characterized in that The mass ratio of ethyl acrylate to butyl acrylate in the monomer for soft shell is (19-20):(0-1).
3. The method according to claim 1, It is characterized in that The mass ratio of methyl methacrylate to butyl acrylate in the monomer for the soft shell is 1:
3.
4. The method according to claim 1, It is characterized in that The TPU / DMF spinning solution concentration is 15-25wt.%.
5. The method according to claim 1, It is characterized in that The TPU / DMF spinning solution concentration is 20-22.5wt.%.
6. The method according to claim 1, It is characterized in that The concentration of TPU / DMF spinning solution is: the conductive material in step S2 is one or more of conductive carbon black, graphene oxide, reduced graphene oxide, carbon nanotubes, MXene, silver nanowires, and silver nanoparticles.
7. The method according to claim 1, It is characterized in that The concentration of the conductive material DMF dispersion in S2 is 10-40 mg / mL.
8. The method according to claim 1, It is characterized in that The concentration of the conductive material DMF dispersion in S2 is 30-40 mg / mL.
9. The method according to claim 1, It is characterized in that In S3, the TPU / DMF solution in steps S1 and S2 and the conductive material DMF dispersion are mixed in a ratio of 1:1, loaded into a syringe and wet-spinned to prepare TPU electrical sensing fibers, and the coagulation bath is a mixed solution of isopropanol, water and calcium chloride.
10. The method according to claim 1, It is characterized in that In S4, the particle size of the polymer seed is about 120nm, and the PDI is less than 0.08; the particle size of the hard core microsphere is about 170-220nm, and the PDI is less than 0.08; the particle size of the hard core soft shell structured photonic crystal microsphere is about 200-300, and the PDI is less than 0.
08.
11. The method according to claim 1, It is characterized in that In step S4, the mass ratio of the monomer for hard core in (a) to the monomer for hard core in (b) is 1:(1-2).
12. The method according to claim 1, It is characterized in that In step S4, the emulsifier used for emulsification is one of sodium dodecyl sulfate (SDS), sodium dodecylbenzene sulfonate, and sodium dodecyl sulfonate.
13. The method according to claim 1, It is characterized in that In step S4, the crosslinking agent is one or more of diene crosslinking agents such as divinylbenzene, allyl methacrylate, isoprene, etc.; the amount of the crosslinking agent in (a) or (b) relative to the hard core in this step is 10-14wt.%; the amount of the crosslinking agent in (c) relative to the soft shell monomer in this step is 0.2-1.0wt.%.
14. The method according to claim 1, It is characterized in that In step S4, the initiator is one or more of ammonium persulfate, potassium persulfate, and sodium persulfate; the ratio of the initiator to the monomer in (a), (b) or (c) is 0.5-1 wt. %.
15. The method according to claim 1, It is characterized in that The dipping time in S5 is 10-60 s, and the drying time is 10-60 s.
16. An optoelectronic dual-mode stress-strain sensing fiber prepared by the method according to any one of claims 1 to 15.
17. Use of the optoelectronic dual-mode stress-strain sensing fiber according to claim 16 in preparing optoelectronic signal sensing components.
18. Application of the optoelectronic dual-mode stress-strain sensing fiber according to claim 16 in the construction of human joint motion monitoring products.
Citation Information
Patent Citations
Core-shell polymer microsphere and application thereof
CN115975131A
Application of photoelectric dual-mode flexible fiber in pressure-temperature sensor
CN116026411A
Elastic multifunctional wave-absorbing fabric based on metamaterial structure and preparation method of elastic multifunctional wave-absorbing fabric
CN117863677A
Method for preparing super-soft aqueous shell / core copolymer of polyacrylate and polyurethane by means of solvent-free process