Preparation method of less-metal friction plate for electromagnetic three-phase asynchronous brake motor

By using materials such as polyvinyl alcohol modified phenolic resin and nano-nitrile rubber powder in the friction pads of the electromagnetic three-phase asynchronous brake motor, the impact strength of the friction pads is improved and the hardness is reduced, solving the problem of adhesion between the friction pads and the cast iron brake disc and reducing damage to the brake disc.

CN118959480APending Publication Date: 2024-11-15CHINA RAILWAY LONGCHANG MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410874863.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The friction pads used in existing electromagnetic three-phase asynchronous brake motors have low impact strength, high compression modulus and hardness, which makes the friction pads easy to stick to the cast iron brake disc, causing damage to the brake disc.

Method used

Friction pads are prepared by using polyvinyl alcohol modified phenolic resin, nano-nitrile rubber powder and polyacrylonitrile-based carbon fiber to replace metal fibers, combined with mineral fibers, potassium hexatitanate whiskers and other materials, through mixing, hot pressing and sintering curing, to reduce hardness and improve impact strength.

Benefits of technology

It improves the impact strength of the friction pads, reduces the compression modulus and hardness, reduces the adhesion between the friction pads and the cast iron brake disc, and reduces damage to the brake disc.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a low-metal friction plate for an electromagnetic three-phase asynchronous brake motor, which comprises the following steps of: weighing the following raw materials for preparing a friction material: 5-10% of polyvinyl alcohol modified phenolic resin; 4-10% of nano nitrile rubber powder; 8-16% of mineral fiber; 10 to 15% of potassium hexatitanate whisker; 0-5% of polyacrylonitrile-based carbon fiber; 13-28% of magnesium oxide; 6-8% of artificial graphite; 12 to 28% of diatomite; 4-6% of antimony sulfide; 1-3% of iron oxide red; 1-3% of cryolite; 10-15 kg of raw materials are added into a vertical shaft type high-speed mixer to be stirred and mixed, and a mixture is obtained; 700-750 g of the mixture is weighed and subjected to hot press molding, and a rough friction plate blank is obtained; and the friction plate rough blank is put into a sintering furnace to be subjected to curing treatment. The friction plate prepared by the method does not adhere to a cast iron brake disc in the using process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a metal-less friction plate for an electromagnetic three-phase asynchronous brake motor. Background Art

[0002] The metal-free friction plate for electromagnetic three-phase asynchronous brake motor is composed of metal matrix and friction material. It is an important braking component in the motor and is directly related to the performance and operation safety of the motor.

[0003] The DC disc brake of the electromagnetic three-phase asynchronous brake motor is installed on the end cover of the motor's non-shaft extension end. When the power is connected, the brake starts to work. Under the action of electromagnetic suction, the electromagnet attracts the armature and compresses the spring, the brake disc is disengaged from the armature and the end cover, and the motor runs; when the power is cut off, the electromagnet loses the electromagnetic force, the spring pushes the armature to press the brake disc and friction plate, generating friction, and the motor stops rotating.

[0004] The existing motor friction plate made of cashew nut shell oil modified phenolic resin, ordinary nitrile rubber powder and carbon fiber has low impact strength, high compression modulus and hardness, which is not conducive to reducing the adhesion between the friction plate and the cast iron brake disc. The product has a high density and is easy to cause damage to the brake disc. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings of the prior art, the present invention proposes a method for preparing a low-metal friction plate for an electromagnetic three-phase asynchronous brake motor, wherein polyvinyl alcohol-modified phenolic resin, nano-nitrile rubber powder and polyacrylonitrile-based carbon fiber are added to the friction plate formula to enhance the product impact strength and reduce the elastic modulus, thereby replacing the reinforcing effect of metal fiber, thereby reducing the adhesion between the friction plate and the cast iron brake disc, reducing the product density and reducing the damage to the brake disc.

[0006] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor, comprising the following steps:

[0007] Step 1, weigh the raw materials for preparing the friction material according to the mass percentage of the following components: polyvinyl alcohol modified phenolic resin, 5-10%; nano-nitrile rubber powder, 4-10%; mineral fiber, 8-16%; potassium hexatitanate whisker, 10-15%; polyacrylonitrile-based carbon fiber, 0-5%; magnesium oxide 13-28%; artificial graphite, 6-8%; diatomaceous earth, 12-28%; antimony sulfide, 4-6%; red iron oxide, 1-3%; cryolite, 1-3%;

[0008] Step 2: Add 10-15 kg of raw materials into a vertical high-speed mixer and stir to obtain a mixture;

[0009] Step 3, weighing 700-750g of the mixed material and hot pressing it to obtain a friction plate rough blank;

[0010] Step 4: placing the friction plate blank into a sintering furnace for curing;

[0011] Step 5: Mechanically process the cured friction plate to obtain a finished product.

[0012] Compared with the prior art, the present invention has the following positive effects:

[0013] The friction plate obtained by the present invention using polyvinyl alcohol modified phenolic resin, nano nitrile rubber powder and polyacrylonitrile-based carbon fiber has high impact strength, low compression modulus and hardness, and will not cause adhesion between the friction plate and the cast iron brake disc during use, thereby reducing damage to the brake disc. DETAILED DESCRIPTION

[0014] The invention discloses a low-metal friction plate suitable for an electromagnetic three-phase asynchronous brake motor. The motor friction plate consists of a metal matrix and a friction material, wherein the friction material comprises the following components: polyvinyl alcohol-modified phenolic resin, 5-10%; nano-nitrile rubber powder, 4-10%; mineral fiber, 8-16%; potassium hexatitanate whisker, 10-15%; polyacrylonitrile-based carbon fiber, 0-5%; magnesium oxide, 13-28%; artificial graphite, 6-8%; diatomaceous earth, 12-28%; antimony sulfide, 4-6%; red iron oxide, 1-3%; and cryolite, 1-3%.

[0015] The preparation method of the friction plate includes weighing, mixing, hot pressing, heat treatment and mechanical processing, and the specific preparation process includes the following steps:

[0016] 1. Weigh the raw materials according to the mass percentage of each component;

[0017] 2. Add 10-15kg of raw materials into the vertical high-speed mixer, mix for 8-16min, and stir at a speed of 800-1500r / min;

[0018] 3. Weigh 700-750g of the mixture, add the mixture into a hot pressing mold at 145-155℃ and press it into shape. The pressing pressure is 25-30MPa. In the early stage of pressing, the upper pressing head needs to return to deflate 3-5 times. After deflation, keep the temperature and pressure for 14-18 minutes;

[0019] 4. Put the rough blank into a sintering furnace for curing treatment, wherein the curing temperature is 80-90°C, and the temperature is kept for 1 hour; the curing temperature is 90-100°C, and the temperature is kept for 1 hour; the curing temperature is 100-120°C, and the temperature is kept for 5 hours; the curing temperature is 120-140°C, and the temperature is kept for 2 hours; the curing temperature is 140-160°C, and the temperature is kept for 2 hours; the curing temperature is 160-180°C, and the temperature is kept for 2 hours; the curing temperature is 180-190°C, and the temperature is kept for 2 hours;

[0020] 5. The cured friction plate is subjected to mechanical processing to obtain a finished product.

[0021] Embodiment 1

[0022] Raw material preparation:

[0023] Polyvinyl alcohol modified phenolic resin, 5%; nano-nitrile rubber powder, 5%; mineral fiber, 14%; potassium hexatitanate whisker, 14%; polyacrylonitrile-based carbon fiber, 3%; magnesium oxide 21%; artificial graphite, 7%; diatomaceous earth, 22%; antimony sulfide, 5%; red iron oxide, 2%; cryolite, 2%. Weigh 10 kg of the above raw materials according to mass percentage, put them into a vertical shaft high-speed mixer and mix for 10 minutes at a stirring speed of 1000 r / min.

[0024] Compression molding: Weigh 720g of the mixture and put it into a 148℃ mold with a pressing pressure of 25MPa. After keeping the temperature and pressure for 10s, the upper pressure head returns to relieve pressure and release air. Repeat this operation 3 times and continue to keep the temperature and pressure for 15min to obtain the rough friction plate.

[0025] Sintering and curing: put the rough blank into a sintering furnace for curing treatment, the curing temperature is 85℃, keep warm for 1h; curing temperature is 95℃, keep warm for 1h; curing temperature is 110℃, keep warm for 5h; curing temperature is 130℃, keep warm for 2h; curing temperature is 150℃, keep warm for 2h; curing temperature is 170℃, keep warm for 2h; curing temperature is 180, keep warm for 2h. The cured friction plate is mechanically processed to obtain the finished product.

[0026] Embodiment 2

[0027] Raw material preparation:

[0028] Polyvinyl alcohol modified phenolic resin, 7%; nano-nitrile rubber powder, 6%; mineral fiber, 8%; potassium hexatitanate whisker, 10%; polyacrylonitrile-based carbon fiber, 5%; magnesium oxide 25%; artificial graphite, 8%; diatomaceous earth, 21%; antimony sulfide, 4%; red iron oxide, 3%; cryolite, 3%. Weigh 15 kg of the above raw materials according to mass percentage, put them into a vertical shaft high-speed mixer and mix for 14 minutes at a stirring speed of 1200 r / min.

[0029] Compression molding: Weigh 750g of the mixture and put it into a 155℃ mold with a pressing pressure of 30MPa. After keeping the temperature and pressure for 8s, the upper pressure head returns to relieve the pressure and release the air. Repeat this operation 4 times and continue to keep the temperature and pressure for 18min to obtain the rough friction plate.

[0030] Sintering and curing: put the rough blank into a sintering furnace for curing treatment, the curing temperature is 90℃, keep warm for 1h; curing temperature is 100℃, keep warm for 1h; curing temperature is 120℃, keep warm for 5h; curing temperature is 140℃, keep warm for 2h; curing temperature is 160℃, keep warm for 2h; curing temperature is 175℃, keep warm for 2h; curing temperature is 190℃, keep warm for 2h. The cured friction plate is mechanically processed to obtain the finished product.

[0031] Comparative Example 1

[0032] Raw material preparation:

[0033] Cashew nut shell oil modified phenolic resin, 5%; ordinary nitrile rubber powder (particle size 0.45mm), 5%; mineral fiber, 14%; potassium hexatitanate whisker, 14%; ordinary carbon fiber, 3%; magnesium oxide 21%; artificial graphite, 7%; diatomaceous earth, 22%; antimony sulfide, 5%; red iron oxide, 2%; cryolite, 2%. Weigh 15kg of the above raw materials according to mass percentage, put them into a vertical shaft high-speed mixer and mix for 10 minutes at a stirring speed of 1000r / min.

[0034] Compression molding: Weigh 750g of the mixture and put it into a 148℃ mold with a pressing pressure of 30MPa. After keeping the temperature and pressure for 10s, the upper pressure head returns to relieve pressure and release air. Repeat this operation 3 times and continue to keep the temperature and pressure for 18min to obtain the rough friction plate.

[0035] Sintering and curing: put the rough blank into a sintering furnace for curing treatment, the curing temperature is 85℃, keep warm for 1h; curing temperature is 95℃, keep warm for 1h; curing temperature is 110℃, keep warm for 5h; curing temperature is 130℃, keep warm for 2h; curing temperature is 150℃, keep warm for 2h; curing temperature is 170℃, keep warm for 2h; curing temperature is 180, keep warm for 2h. The cured friction plate is mechanically processed to obtain the finished product.

[0036] The physical and mechanical properties of the motor friction plate samples of the above-mentioned embodiment and comparative example are compared as shown in Table 1 below.

[0037] Table 1 Comparison of physical and mechanical properties of motor friction plate samples

[0038] Test No. <![CDATA[Density / (g / cm 3 )]]> Impact strength / (MPa) Compression modulus / MPa Hardness / HRR Example 1 1.831 4.41 429 62.2 Example 2 1.842 4.53 442 61.9 Comparative Example 1 1.838 2.89 532 86.5

[0039] From the experimental data in Table 1, it can be seen that the friction plate obtained by using polyvinyl alcohol modified phenolic resin, nano-nitrile rubber powder and polyacrylonitrile-based carbon fiber has high impact strength, low compression modulus and hardness, and no adhesion between the friction plate and the cast iron brake disc occurs during use. The motor friction plate made of cashew nut shell oil modified phenolic resin, ordinary nitrile rubber powder and carbon fiber has low impact strength, high compression modulus and hardness.

Claims

1. A method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor, characterized in that: The steps include: Step 1, weigh the raw materials for preparing the friction material according to the mass percentage of the following components: polyvinyl alcohol modified phenolic resin, 5-10%; nano-nitrile rubber powder, 4-10%; mineral fiber, 8-16%; potassium hexatitanate whisker, 10-15%; polyacrylonitrile-based carbon fiber, 0-5%; magnesium oxide 13-28%; artificial graphite, 6-8%; diatomaceous earth, 12-28%; antimony sulfide, 4-6%; red iron oxide, 1-3%; cryolite, 1-3%; Step 2: Add 10-15 kg of raw materials into a vertical high-speed mixer and stir to obtain a mixture; Step 3, weighing 700-750g of the mixed material and hot pressing to obtain a friction plate blank; Step 4: placing the friction plate blank into a sintering furnace for curing; Step 5: Mechanically process the cured friction plate to obtain a finished product.

2. The method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor according to claim 1, characterized in that: When performing the stirring and mixing in step 2, the stirring speed is 800-1500 r / min and the mixing time is 8-16 min.

3. The method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor according to claim 1, characterized in that: During the hot pressing process of step three, the temperature of the hot pressing mold is 145-155° C. and the pressing pressure is 25-30 MPa.

4. The method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor according to claim 1, characterized in that: During the hot pressing process in step three, the upper pressing head needs to be released 3-5 times during the initial pressing process.

5. The method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor according to claim 4, characterized in that: During the hot pressing process in step 3, the upper pressing head is released on the return stroke after keeping the temperature and pressure for 8-10 seconds.

6. The method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor according to claim 4, characterized in that: During the hot pressing process of step 3, the upper pressing head is kept warm and pressurized for 14-18 minutes after the upper pressing head returns and vents.

7. The method for preparing a metal-free friction plate for an electromagnetic three-phase asynchronous brake motor according to claim 1, characterized in that: The curing treatment method of step four is: curing temperature 80-90°C, keep warm for 1 hour; curing temperature 90-100°C, keep warm for 1 hour; curing temperature 100-120°C, keep warm for 5 hours; curing temperature 120-140°C, keep warm for 2 hours; curing temperature 140-160°C, keep warm for 2 hours; curing temperature 160-180°C, keep warm for 2 hours; curing temperature 180-190°C, keep warm for 2 hours.