Different asphalt film thickness sample preparation device suitable for adhesive force drawing instrument
By designing a device including a thermal oil tank and a heating tank, using heating and pressure to control the thickness of the bitumen film, the problem of inaccurate control of bitumen film thickness in the prior art is solved, and the accuracy of bitumen-aggregate adhesion test is achieved and Easy to operate.
Patent Information
- Application Number
- CN202411049050.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-15
AI Technical Summary
The prior art is difficult to accurately control the thickness of the bitumen film, resulting in large test errors in the asphalt-aggregate adhesion test, and the preparation process is complicated and inconvenient to operate.
A device including a thermal oil tank, a heating tank, an electric pressurization pump and a lifting shaft is designed to control the uniform heating and distribution of asphalt through heating and pressure, accurately control the thickness of the asphalt film, and simplify operation.
It realizes accurate control of the thickness of the asphalt film, reduces test errors, is simple to operate, safe and reliable, and can effectively simulate the adhesion interface between asphalt and aggregate.
Smart Images

Figure CN118961335A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sample preparation, in particular to a device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller. Background Art
[0002] In recent years, in the development and research of roads, asphalt roads have become the main structural form of modern traffic roads due to their own characteristics. The rapid growth of road traffic volume and the continuous increase in the number of heavy-loaded vehicles cause shear deformation of the asphalt pavement under the repeated action of wheel dynamic loads, eventually forming rutting, bumps, and other defects that affect the normal use of the road and bring serious hidden dangers to driving safety. The asphalt-aggregate interface phase structure is very complex, and asphalt road diseases often originate and develop from the interface phase. The asphalt in the asphalt-aggregate interface exists in the form of an asphalt film, and the thickness of different asphalt films has a great influence on the performance of the interface phase. Therefore, how to accurately control the thickness of the asphalt film is the key to studying the performance of the asphalt-aggregate interface phase.
[0003] At present, asphalt-aggregate adhesion can be tested by pull-out test. Different asphalt film thickness has a great influence on asphalt-aggregate adhesion test. Most of the methods to control the thickness of asphalt film are calculated by calculation, and the thickness of asphalt film is calculated under the premise of assuming that the thickness of asphalt film in asphalt mixture is uniform. Therefore, the uniformity of asphalt film prepared by mass method varies greatly.
[0004] Therefore, it is urgent to design a sample preparation device for different asphalt film thicknesses suitable for adhesion puller. Summary of the invention
[0005] The purpose of the present invention is to provide a device for preparing samples of different asphalt film thicknesses suitable for an adhesion pull-off instrument, so as to solve the problems existing in the above-mentioned prior art, and can accurately control the thickness of the asphalt film used for the asphalt pull-off test and reduce the test error; and the device is lightweight and convenient, simple to operate, and has good practicality.
[0006] To achieve the above object, the present invention provides the following solution: The present invention provides a device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller, comprising:
[0007] A box body, in which a heat transfer oil tank is fixedly installed; the heat transfer oil tank is a hollow cylindrical structure, with a hollow groove in the center, and the hollow groove runs through the top and bottom surfaces of the box body; a baffle is installed in the hollow groove; the baffle is connected to the film making assembly at the bottom, and a heating groove is formed at the top;
[0008] The thermal oil tank is connected to the heating tank via a pressurizing component;
[0009] The film-making assembly comprises a movable part and a collection stone plate arranged at the bottom of the box body.
[0010] A sealing cover is sealed on the top of the heating tank.
[0011] A heating resistance wire is installed in the thermal oil tank, and the heating resistance wire is used to heat the heat-conducting medium of the thermal oil tank.
[0012] A temperature sensor is also installed in the thermal oil tank.
[0013] The pressurizing assembly includes an electric pressurizing pump, and the baffle is configured to connect the heating tank with the movable part when the electric pressurizing pump is started.
[0014] The movable part includes a pipeline, and a lifting shaft is movably installed on the outer wall of the pipeline in the vertical direction; an upper bottom plate is fixedly installed at the bottom end of the lifting shaft; the upper bottom plate is fixedly connected to the lower bottom plate through a connecting ring, and an asphalt storage space connected to the pipeline is reserved in the upper bottom plate and the lower bottom plate;
[0015] The lower base plate is arranged directly above the aggregate stone plate;
[0016] The pipeline is configured to communicate with the heating tank.
[0017] The lower bottom plate is provided with a plurality of asphalt holes at equal intervals; the bottom surface of the connecting ring is provided with an overflow hole; the asphalt holes are used to drip the asphalt in the asphalt storage space onto the surface of the aggregate slab.
[0018] A displacement sensor is also installed at the top end of the lifting shaft.
[0019] The aggregate stone slab is placed on the two fixing plates, and the two ends of the fixing plates are mounted on the bottom surface of the box body through fixing rods. The bottom surface of the box body is also provided with a slideway; the fixing rod is fixedly installed in the slideway.
[0020] The side wall of the box is also equipped with an electronic panel.
[0021] The present invention discloses the following technical effects: the present invention can accurately control the covering thickness of asphalt on the aggregate surface and effectively simulate the adhesion interface between asphalt and aggregate; compared with traditional quality control methods, the present invention is easy to make, simple to operate, safe and reliable. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0023] Figure 1 It is a front view of the structure of the present invention;
[0024] Figure 2 It is a side view of the structure of the present invention;
[0025] Figure 3 It is a top view of the structure of the present invention;
[0026] Figure 4 Schematic diagram of the lower base plate structure;
[0027] Figure 5 A comparative bar graph of a comparative embodiment of the present invention;
[0028] Among them, 1. Heating tank; 2. Electric pressure pump; 3. Heating resistor wire; 4. Thermal oil tank; 5. Lifting shaft; 6. Fixed rod; 7. Fixed plate; 8. Sealing cover; 9. Temperature sensor; 10. Electronic panel; 11. Displacement sensor; 12. Pipeline; 13. Connecting ring; 14. Overflow hole; 15. Lower base plate; 16. Upper base plate; 17. Baffle; 18. Slide. DETAILED DESCRIPTION
[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0031] The present invention provides a device for preparing samples of different asphalt film thicknesses suitable for an adhesion pull-off instrument, comprising:
[0032] The box body has a heat transfer oil tank 4 fixedly installed in it; the heat transfer oil tank is a hollow cylindrical structure, with a hollow groove in the center, which runs through the top and bottom surfaces of the box body; a baffle 17 is installed in the hollow groove; the baffle 17 is connected to the film making assembly below, and a heating tank 1 is formed above;
[0033] The heat transfer oil tank 4 is connected to the heating tank 1 through a pressurizing component;
[0034] The film-making assembly comprises a movable part and a collection stone plate arranged at the bottom of the box body.
[0035] A sealing cover 8 is installed on the top of the heating tank 1 in a sealed manner.
[0036] A heating resistor 3 is installed in the thermal oil tank 4 , and the heating resistor 3 is used to heat the heat-conducting medium in the thermal oil tank 4 .
[0037] A temperature sensor 9 is also installed in the thermal oil tank 4 .
[0038] The pressurizing assembly includes an electric pressurizing pump 2 , and the baffle 17 is configured to connect the heating tank 1 with the movable part when the electric pressurizing pump 2 is started.
[0039] In one embodiment of the present invention, the heating resistor wire 3 heats the thermal oil in the thermal oil tank 4, and a temperature sensor 9 is provided inside the thermal oil tank; after the thermal oil in the thermal oil tank 4 is heated up, the asphalt in the heating tank 1 is evenly heated to a set temperature, and the heating tank 1 is equipped with a sealing cover 8 for sealing. A baffle 17 is provided at the connection between the heating tank 1 and the pipeline 12 to prevent the hot asphalt from flowing freely, and the baffle 17 is automatically opened when the electric booster pump 2 is started.
[0040] The movable part includes a pipeline 12, and a lifting shaft 5 is movably installed on the outer wall of the pipeline 12 in the vertical direction; an upper bottom plate 16 is fixedly installed at the bottom end of the lifting shaft 5; the upper bottom plate 16 is fixedly connected to the lower bottom plate 15 through a connecting ring 13, and an asphalt storage space connected to the pipeline 12 is reserved in the upper bottom plate 16 and the lower bottom plate 15;
[0041] The lower base plate 15 is arranged directly above the aggregate stone plate;
[0042] The pipe 12 is arranged to communicate with the heating tank 1 .
[0043] In one embodiment of the present invention, the lifting shaft 5 drives the upper bottom plate 16 and the lower bottom plate 15 to move up and down to control the thickness of the asphalt film; a pipeline 12 is arranged between the lifting shaft 5 and the upper bottom plate 16; a displacement sensor 11 is arranged at the upper end of the lifting shaft 5; the upper bottom plate 16 and the lower bottom plate 15 are an assembly with an asphalt storage space connected to the pipeline 12 in the middle; the upper bottom plate 16 and the lower bottom plate 15 are connected by a circular ring 13, and the lower bottom plate 15 has many asphalt holes.
[0044] A plurality of asphalt holes are formed at equal intervals on the lower bottom plate 15; an overflow hole 14 is formed on the bottom surface of the connecting ring 13; and the asphalt holes are used to drip the asphalt in the asphalt storage space onto the surface of the aggregate slab.
[0045] A displacement sensor 11 is also installed at the top of the lifting shaft 5 .
[0046] The aggregate stone slab is placed on two fixed plates 7 , and both ends of the fixed plates 7 are installed on the bottom surface of the box body through fixed rods 6 . The bottom surface of the box body is also provided with a slideway 18 ; the fixed rods 6 are fixedly installed in the slideway 18 .
[0047] An electronic panel 10 is also installed on the side wall of the box.
[0048] In one embodiment of the present invention, the signal output end of the electronic panel 10 is connected to the displacement sensor 11 and the temperature sensor 9 , and the signal output end is connected to the heating resistor 3 , the electric pressure pump 2 and the lifting shaft 5 .
[0049] In one embodiment of the present invention, the method for preparing an asphalt film comprises the following steps:
[0050] Turn on the switch of the electronic panel 10, adjust the temperature required for the asphalt to flow fully, heat the heat transfer oil tank 4 to the set temperature through the heating resistor 3, pour the asphalt into the heating tank 1, and keep it warm for 30 minutes; place the aggregate stone plate on the fixing plate 7, adjust the position of the fixing rod 6 on the slide 18, tighten the fixing rod 6, and ensure that the aggregate stone plate is in full contact with the connecting ring 13;
[0051] The lifting shaft 5 is controlled by the electronic panel 10 to drive the lower bottom plate 15 to contact the surface of the aggregate stone slab. After the displacement is reset, the required film thickness is set through the electronic panel 10, and the start button is pressed. The lifting shaft 5 drives the upper bottom plate 16 and the lower bottom plate 15 to rise to the set height; the heating tank 1 is sealed, and the electric pressure pump 2 is turned on to pressurize the air in the heating tank 1. At the same time, the baffle 17 is opened. As the pressure rises, asphalt is filled into the space inside the upper bottom plate 16 and the lower bottom plate 15 through the pipeline 12. The air continues to pressurize the hot asphalt through the asphalt holes of the lower bottom plate 15 to flow to the surface of the aggregate stone slab until the asphalt flows out of the overflow hole 14 of the connecting ring 13. The electric pressure pump 2 is turned off and the sealing cover 8 is opened to prevent the asphalt from continuously overflowing; the connecting ring 13 and the aggregate stone slab are removed at the same time, and the asphalt temperature is cooled to room temperature. The connecting ring 13 is removed. After the asphalt is cooled, the overflow part of the asphalt film connection is cleaned with a hot scraper, and the pulling head with ab glue is pressed on the surface of the asphalt film. The sample preparation is completed, and the test can be carried out after the AB glue is solidified. The device is equipped with a plurality of connecting rings 13 of different sizes, and samples can be prepared continuously.
[0052] Furthermore, the temperature sensor has a range of 15°C to 230°C and a heating tank capacity of 0.2L.
[0053] The connecting ring 13 is tightly fitted with the combination of the upper bottom plate 16 and the lower bottom plate 15, and the connecting ring 13 can be disassembled and installed; the upper bottom plate 16 is fixedly connected to the lower end of the lifting shaft 5, and the upper bottom plate 16 and the lower bottom plate 15 assembly are also disassembled. The upper bottom plate 16, the lower bottom plate 15 and the connecting ring 13 are all made of steel materials with a non-stick asphalt layer on the surface.
[0054] Press the reset button on the electronic panel 10 to control the lower base plate 15 to move close to the surface of the aggregate slab, press the calibration button on the electronic panel to set the required asphalt film thickness, press the start button, and the lifting shaft 5 moves up to the set height. The sizes of the upper base plate 16 and the lower base plate 15 are 10mm, 14mm, 20mm, and 50mm respectively, and are equipped with connecting rings 13 with inner diameters of 10mm, 14mm, 20mm, and 50mm, and there are multiple of each size. The moving range of the lifting shaft 5 is 0μm-1000μm, accurate to 0.1μm, and the lifting shaft 5 can be a JL182 precision industrial lifter.
[0055] When the heat transfer oil reaches the set temperature, heat the asphalt and pour it into the heating tank 1, keep it warm for 15 minutes, cover it with the sealing cover 8, press the air inlet button on the electronic panel 10 to turn on the electric booster pump 2, and open the baffle 17 to force the asphalt in the heating tank 1 to be injected into the surface of the aggregate slab through the pipe 12.
[0056] When the asphalt flows out from the overflow hole 14 of the connecting ring 13 on the surface of the aggregate slab, press the exhaust key, open the sealing cover 8, remove the connecting ring 13 to fix the asphalt shape, and after cooling, the required asphalt film thickness sample can be prepared.
[0057] Further, in a comparative embodiment of the present invention, in order to measure the actual thickness h of the asphalt film, the height of the spindle is first measured using a film thickness meter and the height is measured as H1. After the asphalt film prepared by the present invention is cooled, the spindle is gently pressed on the surface of the asphalt film, and the height of the asphalt film and the spindle is measured as H2, then h = H2-H1. The actual measurement of the film thickness of the sample to be tested is 10μm, 100μm, 200μm, 500μm, and 900μm, and the results are shown in Table 1.
[0058] Table 1
[0059]
[0060] Comparative Example:
[0061] Through existing research, it is found that when the asphalt film is a circle with a diameter of 20 mm, the corresponding relationship of different film thickness is shown in Table 2. The mass method is used to control the asphalt film thickness: the spindle is reversed on the balance, the required mass of asphalt is weighed on the bottom of the spindle, and the asphalt and the spindle are placed in an oven at the required temperature for 5 minutes. After the insulation time is over, the spindle is quickly covered on the aggregate surface and gently pressed. After the asphalt and the aggregate are cooled, the test can be carried out.
[0062] Table 2
[0063]
[0064] In order to measure the actual thickness h of the asphalt film, the height of the spindle is first measured using a film thickness meter and the height is measured as H1. After the asphalt film and aggregates are cooled using the mass method to control the asphalt film, the height of the asphalt film and the spindle is measured as H2, then h = H2-H1. The test results are shown in Table 3.
[0065] Table 3
[0066]
[0067] The comparison of the measurement errors of different asphalt film thicknesses prepared in the comparative examples and the embodiments is as follows: Figure 5As shown, the thickness error of the asphalt film prepared by the device is smaller than that of the asphalt film prepared by the mass method, which can achieve the effect of accurately controlling the thickness of the asphalt film and accurately simulate the adhesion interface between asphalt and aggregate.
[0068] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "upper", "lower", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solution of the present invention by ordinary technicians in this field should all fall within the scope of protection determined by the claims of the present invention.
Claims
1. A device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller, characterized in that: include: A box body, wherein a heat transfer oil tank (4) is fixedly installed in the box body; the heat transfer oil tank is a hollow cylindrical structure, a hollow groove is opened in the center, and the hollow groove runs through the top surface and the bottom surface of the box body; a baffle (17) is installed in the hollow groove; the baffle (17) is connected to the film making component at the bottom, and a heating groove (1) is formed at the top; The heat transfer oil tank (4) is connected to the heating tank (1) via a pressurizing component; The film-making assembly comprises a movable part and a collection stone plate arranged at the bottom of the box body.
2. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 1, characterized in that: A sealing cover (8) is sealed and installed on the top end of the heating tank (1).
3. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 1, characterized in that: A heating resistance wire (3) is installed in the heat-conducting oil tank (4), and the heating resistance wire (3) is used to heat the heat-conducting medium in the heat-conducting oil tank (4).
4. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion pull-off instrument according to claim 1, characterized in that: A temperature sensor (9) is also installed in the thermal oil tank (4).
5. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 1, characterized in that: The pressurizing component comprises an electric pressurizing pump (2), and the baffle (17) is configured to connect the heating tank (1) with the movable part when the electric pressurizing pump (2) is started.
6. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 5, characterized in that: The movable part comprises a pipeline (12), and a lifting shaft (5) is movably mounted on the outer wall of the pipeline (12) in a vertical direction; an upper base plate (16) is fixedly mounted on the bottom end of the lifting shaft (5); the upper base plate (16) is fixedly connected to the lower base plate (15) via a connecting ring (13), and an asphalt storage space connected to the pipeline (12) is reserved in the upper base plate (16) and the lower base plate (15); The lower base plate (15) is arranged directly above the aggregate stone plate; The pipeline (12) is configured to communicate with the heating tank (1).
7. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 6, characterized in that: The lower bottom plate (15) is provided with a plurality of asphalt holes at equal intervals; the bottom surface of the connecting ring (13) is provided with an overflow hole (14); the asphalt holes are used to drip the asphalt in the asphalt storage space onto the surface of the aggregate slab.
8. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 6, characterized in that: A displacement sensor (11) is also installed at the top end of the lifting shaft (5).
9. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 6, characterized in that: The aggregate stone slab is placed on the two fixing plates (7), and the two ends of the fixing plates (7) are mounted on the bottom surface of the box body through fixing rods (6). The bottom surface of the box body is also provided with a slideway (18); the fixing rods (6) are fixedly mounted in the slideway (18).
10. The device for preparing samples of different asphalt film thicknesses suitable for an adhesion puller according to claim 6, characterized in that: An electronic panel (10) is also installed on the side wall of the box.