Method for detecting metal impurities in positive electrode active material
By preparing a positive electrode slurry with a fineness sufficient to pierce the separator and then disassembling the battery, EDS analysis of black spots in the separator was used to detect non-magnetic metal impurities. This solved the problem that existing technologies could not effectively identify non-magnetic metal impurities in lithium-ion battery positive electrode materials, and improved the efficiency and accuracy of battery performance testing.
Patent Information
- Application Number
- CN202410842470.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-15
AI Technical Summary
Existing technologies cannot effectively identify the content of non-magnetic metallic impurities in the cathode material of lithium-ion batteries, which affects the battery's self-discharge and cycle performance.
By preparing a positive electrode slurry with a fineness sufficient to puncture the separator, the battery is assembled and then fully charged and disassembled. EDS analysis is used to identify non-magnetic metal impurities by detecting black spots on the separator, and physical principles are used to fabricate micro-short-circuit characteristics of the cell for detection.
It enables rapid and convenient detection of non-magnetic metallic impurities in positive electrode active materials, ensuring battery performance stability.
Smart Images

Figure CN118961772A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of battery testing, and in particular relates to a method for detecting metal impurities in positive electrode active materials. Background Art
[0002] During the preparation of positive electrode materials for lithium-ion batteries, metal impurities are often introduced due to the introduction of raw materials, the introduction of metal equipment, or in-situ generation during the sintering process. Metal impurities include magnetic metal impurities, such as iron, nickel, etc.; they also include non-magnetic metal impurities, such as copper, zinc, aluminum or their alloys; there is no effective separation method for non-magnetic metal foreign matter in the later stage, which will affect the application characteristics of the battery such as self-discharge and cycle performance. Therefore, it is very necessary to study a method that can accurately determine the content of metal impurities (including non-magnetic metals) in positive electrode materials for lithium-ion batteries. The current conventional detection methods for non-magnetic metal elements in positive electrode powder cannot effectively identify them. Summary of the invention
[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for detecting metal impurities in positive electrode active materials.
[0004] To achieve the above object, the technical solution adopted by the present invention is:
[0005] A method for detecting metal impurities in positive electrode active materials comprises the following steps: 1) homogenizing the positive electrode active material to be tested to obtain positive electrode slurry; the fineness of the positive electrode slurry meets the requirement of puncturing a diaphragm; 2) coating a current collector with the positive electrode slurry obtained in step 1) to obtain a positive electrode sheet, and assembling the battery; 3) disassembling the battery after it is fully charged, and performing EDS analysis on the black spots of the diaphragm to determine the metal impurities in the positive electrode active material.
[0006] A test method for judging whether the fineness meets the requirement of puncturing the diaphragm comprises the following steps: 1.1) coating the current collector with positive electrode slurries of different finenesses to obtain a series of positive electrode sheets, and forming a series of batteries; 1.2) disassembling the battery after fully charging, and the appearance of black spots on the diaphragm indicates that the fineness of the positive electrode slurry in step 1) meets the requirement of puncturing the diaphragm.
[0007] The impurities are non-magnetic metal elements; preferably, the non-magnetic metal elements are one of Cu, Zn, and Al, or a mixture thereof.
[0008] The fineness of step 1) is > the conventional fineness standard value; the conventional fineness standard value is the fineness value without puncturing the diaphragm; preferably, the fineness of step 1) is ≥ 2 times the conventional fineness standard value; preferably, the conventional fineness standard value is 15μm; the fineness of the positive electrode slurry is ≥ 30μm.
[0009] The positive electrode active material is one or more of lithium iron phosphate positive electrode material, nickel cobalt manganese lithium ternary positive electrode material, nickel cobalt aluminum lithium ternary positive electrode material or lithium iron manganese phosphate positive electrode material.
[0010] In step 1), the positive electrode slurry is subjected to a homogenization process adjustment so that the positive electrode slurry is agglomerated, thereby obtaining a fineness that meets the requirement of puncturing the separator.
[0011] The positive electrode slurry includes a positive electrode active material, a conductive agent, a binder and a solvent; preferably, the conductive agent is Super P; the binder is PVDF; the solvent is NMP; preferably, the mass ratio of the positive electrode active material, the conductive agent and the binder is (90-98): (1-5): (1-5).
[0012] The homogenization process adopts the following steps: a) adding a solvent to a stirring tank, rotating at a speed of 300-500 rpm, and stirring for 3-10 minutes; b) adding a binder, adjusting the speed to 1200-1800 rpm, and stirring for 20-40 minutes; c) adding a conductive agent, adjusting the speed to 3000-5000 rpm, and stirring for 20-40 minutes; d) adding a positive electrode active material three times while maintaining the speed, and stirring for 10-20 minutes each time the positive electrode active material is added; e) reducing the speed to 300-500 rpm; and the stirring time is 15-30 minutes.
[0013] The current collector is aluminum foil; the diaphragm is PE diaphragm.
[0014] The battery described in step 2) is prepared in the following manner: the positive electrode sheet, the negative electrode sheet and the separator are stacked by hot pressing, and then assembled, injected and formed.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] The method for detecting metal impurities in positive electrode active materials of the present application understands the physical properties of the positive electrode slurry to make its fineness meet the requirement of puncturing the diaphragm, and uses physical principles to create a micro-short circuit feature of the battery cell, thereby polarizing and precipitating non-magnetic metal impurities in the positive electrode active material to detect whether metal elements are contained. This method is fast and simple and can detect non-magnetic metal impurities in the positive electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1-3 The disassembly interface diagrams of different embodiments are shown;
[0018] Figure 4 Schematic diagram of the polarization process of the positive electrode;
[0019] Figure 5 This is the element analysis result diagram. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.
[0021] Example
[0022] A method for detecting metal impurities in a positive electrode active material comprises the following steps:
[0023] 1) homogenizing the positive electrode active material to be tested to obtain a positive electrode slurry; the fineness of the positive electrode slurry meets the requirement of puncturing the diaphragm;
[0024] First, a specific test is conducted on whether the fineness meets the requirement of puncturing the diaphragm, including the following steps: 1.1) The positive electrode slurry of different fineness is coated on the current collector to obtain a series of positive electrode sheets, and a series of batteries are formed; the battery is prepared by the following method: the positive electrode sheet, the negative electrode sheet and the diaphragm are stacked by hot pressing, and then assembled, injected and formed; the current collector is aluminum foil; the diaphragm is a PE diaphragm; the negative electrode sheet is a conventional negative electrode sheet, and its negative electrode active material is graphite; 1.2) The battery is fully charged and then disassembled. The appearance of black spots on the diaphragm can determine that the fineness of the positive electrode slurry in step 1) meets the requirement of puncturing the diaphragm.
[0025] Table 1 shows the results of whether positive electrode slurries of different fineness can pierce the separator. Figure 1-3 The disassembly interfaces of Examples 1 (35 μm), 2 (12 μm), and 3 (13 μm) are shown respectively.
[0026] Table 1
[0027] Example Fineness standard Cathode slurry fineness Disassembly results 1 15μm 35μm There are black spots on the negative electrode, and the corresponding diaphragm also has black spots 2 15μm 12μm No black spots found 3 15μm 13μm No black spots found
[0028] The results show that the fineness is ≥2 times of the conventional fineness standard value; for example, in this embodiment, the conventional fineness standard value is 15μm; the fineness of the positive electrode slurry satisfies ≥30μm, which can puncture the diaphragm.
[0029] Further, the study shows that when the positive electrode slurry agglomerates, its fineness is larger and can meet the requirement of puncturing the diaphragm; generally, the positive electrode slurry includes a positive electrode active material, a conductive agent, a binder and a solvent; the positive electrode active material is one or more of a lithium iron phosphate positive electrode material, a nickel cobalt manganese lithium ternary positive electrode material, a nickel cobalt aluminum lithium ternary positive electrode material or a lithium manganese iron phosphate positive electrode material; preferably, the conductive agent is Super P; the binder is PVDF; the solvent is NMP; preferably, the mass ratio of the positive electrode active material, the conductive agent and the binder is (90-98): (1-5): (1-5);
[0030] Generally, the homogenization process for agglomeration includes the following steps: a) adding a solvent to a stirring tank, rotating at a speed of 300-500 rpm, and stirring for 3-10 minutes; b) adding a binder, adjusting the speed to 1200-1800 rpm, and stirring for 20-40 minutes; c) adding a conductive agent, adjusting the speed to 3000-5000 rpm, and stirring for 20-40 minutes; d) adding the positive electrode active material three times while maintaining the speed, and stirring for 10-20 minutes each time the positive electrode active material is added; e) reducing the speed to 300-500 rpm; stirring for 15-30 minutes;
[0031] In this embodiment, the positive electrode active material is LFP, the conductive agent is super P, and the binder is PVDF slurry as an example for explanation, and the ratio is 97:0.8:2.2; NMP is used as a solvent, and the homogenization process for agglomeration includes the following steps: adding solvent to a stirring tank, rotating speed 500rpm, stirring for 5min; b) adding a binder, adjusting the speed to 1500rpm, stirring for 300min; c) adding a conductive agent, adjusting the speed to 3000rpm; stirring for 30min; d) maintaining the speed and adding the positive electrode active material three times, stirring for 15min each time the positive electrode active material is added; e) reducing the speed to 300rpm; stirring time is 15min; reducing the speed to make the homogenization uneven, that is, the positive electrode slurry can be agglomerated, and the fineness of the positive electrode slurry obtained by this method is usually >50μm.
[0032] A simulated copper-containing positive electrode active material was used as a test sample for testing. Specifically, 2.5 g of Cu was added to 100 g of LPF of the positive electrode active material, and the above-mentioned homogenization process was used for homogenization to obtain a positive electrode slurry with a fineness greater than 50 μm. 2) The positive electrode slurry containing Cu with a fineness greater than 50 μm obtained in step 1) is coated on the current collector to obtain a positive electrode sheet, and the same materials as in step 1) are used to assemble a battery; 3) The battery is disassembled after being fully charged, and the black spots of the diaphragm are analyzed by EDS to determine the metal impurities in the positive electrode active material. Figure 4 A schematic diagram of the process is shown; Figure 5 The EDS analysis results are shown. The determination method of the present application is also applicable to other non-magnetic metal elements; for example, Zn, Al, etc.
[0034] The results of the study indicate that the method for detecting metal impurities in positive electrode active materials of the present application understands the physical properties of the positive electrode slurry so that its fineness meets the requirement of puncturing the diaphragm, and utilizes physical principles to create a micro-short circuit feature of the battery cell, thereby polarizing and precipitating the non-magnetic metal impurities in the positive electrode active material to detect whether metal elements are contained. This method is fast and simple and can detect non-magnetic metal impurities in the positive electrode active material.
[0035] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for detecting metal impurities in positive electrode active materials, characterized in that: The method comprises the following steps: 1) homogenizing the positive electrode active material to be tested to obtain positive electrode slurry; the fineness of the positive electrode slurry meets the requirement of puncturing the diaphragm; 2) coating the positive electrode slurry obtained in step 1) on the current collector to obtain a positive electrode sheet, and assembling the battery; 3) disassembling the battery after it is fully charged, and performing EDS analysis on the black spots of the diaphragm to judge the metal impurities in the positive electrode active material.
2. The method for detecting metal impurities in positive electrode active materials according to claim 1, characterized in that: A test method for judging whether the fineness meets the requirement of puncturing the diaphragm comprises the following steps: 1.1) coating the current collector with positive electrode slurries of different finenesses to obtain a series of positive electrode sheets, and forming a series of batteries; 1.2) disassembling the battery after fully charging, and the appearance of black spots on the diaphragm indicates that the fineness of the positive electrode slurry in step 1) meets the requirement of puncturing the diaphragm.
3. The method for detecting metal impurities in positive electrode active materials according to claim 1, characterized in that: The impurities are non-magnetic metal elements; preferably, the non-magnetic metal elements are one of Cu, Zn, and Al, or a mixture thereof.
4. The method for detecting metal impurities in positive electrode active materials according to claim 1, characterized in that: The fineness of step 1) is > the conventional fineness standard value; the conventional fineness standard value is the fineness value without puncturing the diaphragm; preferably, the fineness of step 1) is ≥ 2 times the conventional fineness standard value; preferably, the conventional fineness standard value is 15μm; the fineness of the positive electrode slurry is ≥ 30μm.
5. The method for detecting metal impurities in positive electrode active materials according to claim 1, characterized in that: The positive electrode active material is one or more of lithium iron phosphate positive electrode material, nickel cobalt manganese lithium ternary positive electrode material, nickel cobalt aluminum lithium ternary positive electrode material or lithium iron manganese phosphate positive electrode material.
6. The method for detecting metal impurities in positive electrode active materials according to claim 1, characterized in that: In step 1), the positive electrode slurry is subjected to a homogenization process adjustment so that the positive electrode slurry is agglomerated, thereby obtaining a fineness that meets the requirement of puncturing the separator.
7. The method for detecting metal impurities in positive electrode active materials according to claim 6, characterized in that: The positive electrode slurry includes a positive electrode active material, a conductive agent, a binder and a solvent; preferably, the conductive agent is Super P; the binder is PVDF; the solvent is NMP; preferably, the mass ratio of the positive electrode active material, the conductive agent and the binder is (90-98): (1-5): (1-5).
8. The method for detecting metal impurities in positive electrode active materials according to claim 7, characterized in that: The homogenization process adopts the following steps: a) adding a solvent to a stirring tank, rotating at a speed of 300-500 rpm, and stirring for 3-10 minutes; b) adding a binder, adjusting the speed to 1200-1800 rpm, and stirring for 20-40 minutes; c) adding a conductive agent, adjusting the speed to 3000-5000 rpm, and stirring for 20-40 minutes; d) adding a positive electrode active material three times while maintaining the speed, and stirring for 10-20 minutes each time the positive electrode active material is added; e) reducing the speed to 300-500 rpm; and the stirring time is 15-30 minutes.
9. The method for detecting metal impurities in positive electrode active materials according to claim 1, characterized in that: The current collector is aluminum foil; the diaphragm is PE diaphragm.
10. The method for detecting metal impurities in positive electrode active materials according to claim 1, characterized in that: The battery described in step 2) is prepared in the following manner: the positive electrode sheet, the negative electrode sheet and the separator are stacked by hot pressing, and then assembled, injected and formed.