Light guide plate for image display

By improving the surface planarity of the resin substrate and introducing a barrier layer of high refractive index inorganic material, the problem of deterioration of the holographic layer and unclear image in high temperature and humidity environments is solved, and high-quality image display and Durability.

CN118962990APending Publication Date: 2024-11-15MITSUBISHI CHEM CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411359722.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-02-05
Filing Date
2020-02-05
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the light guide plate for image display supported by resin substrate is prone to deterioration of holographic layer and unclear images in high temperature and humidity environments, especially in wearable displays of AR or MR, with higher requirements. Quality and durability.

Method used

By improving the surface planarity of the resin substrate and introducing a barrier layer, reducing the thickness fluctuation of the holographic layer and moisture penetration, a high refractive index inorganic material and a water vapor barrier layer are used to ensure image clarity and durability of the holographic layer.

Benefits of technology

When using a resin substrate, the clarity of image display and durability of the holographic layer are realized, and are suitable for applications in high temperature and humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118962990A_ABST
    Figure CN118962990A_ABST
Patent Text Reader

Abstract

Provided is a light guide plate for image display, which is capable of displaying a clear image even when using a resin base material. A light guide plate (1004) for image display, which has a first resin base material (1001) and a holographic layer (1002), and wherein the first resin base material (1001) has an MC value of 0.120 or less as determined by evaluation on the basis of darkness contrast.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The Chinese national application number of the application to which it is directed is 202080012156.5, the international application number is PCT / JP2020 / 004237, the application date is February 5, 2020, the date of entry into China is August 2, 2021, and the name of the invention is “Light guide plate for image display”. Technical Field

[0002] The present invention relates to a light guide plate for image display.

[0003] This application claims priority based on Japanese Patent Application Nos. 2019-018943, 2019-018944, 2019-018945, and 2019-018946 filed in Japan on February 5, 2019, the contents of which are incorporated herein by reference. Background Art

[0004] There are cases where a light guide plate for image display is used in a display device. For example, in a display device using VR (virtual reality) technology, AR (augmented reality) technology, or MR (mixed reality), a light guide plate for image display in which a holographic layer is supported by a transparent substrate is used. A hologram having various optical functions (such as waveguide, reflection, and diffraction functions) is formed in the holographic layer.

[0005] As the transparent substrate, a glass substrate is often used, but from the viewpoints of processability, lightness, durability, and transportability, a resin substrate is more preferably used as the transparent substrate.

[0006] Patent Document 1 discloses a holographic laminate used in a vehicle-mounted head-up display. The holographic laminate is formed by laminating an acrylic resin substrate, an acrylic adhesive layer, a holographic layer formed of an acrylic photopolymer, an acrylic adhesive layer, and an acrylic resin substrate in this order.

[0007] Patent Document 1 states that the surface smoothness of an acrylic resin substrate can cause a change in the appearance of a hologram. According to Patent Document 1, when the maximum height Rmax indicating the surface smoothness of a holographic laminate is greater than 50 μm, the appearance of the hologram changes significantly. When the maximum height Rmax is less than 25 μm, the appearance change of the hologram is within an acceptable range. However, Patent Document 1 does not specifically state the necessity of a nanoscale surface smoothness with a maximum height Rmax of less than 1 μm. Patent Document 1 also does not state any specific example of a nanoscale surface smoothness.

[0008] In addition, the holographic material forming the holographic layer may corrode the resin substrate due to temperature changes. It is known that the holographic material will also deteriorate due to moisture absorption. Therefore, the display device using the resin substrate to support the holographic layer is prone to deterioration in a high temperature and high humidity environment.

[0009] Patent Document 2 describes that a photosensitive material layer for forming a hologram is formed on a substrate made of an optically transparent resin, and the photosensitive material layer is covered with a water-based polymer protective barrier. Patent Document 2 suggests that the water-based polymer protective barrier is provided to resist corrosion due to moisture.

[0010] Patent Document 3 describes a holographic laminate having a hologram sandwiched between resin substrates via an optical adhesive, wherein the entire periphery is covered with a protective coating layer. Patent Document 3 describes that the protective coating layer may be a coating for improving airtightness and gas barrier properties.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Application Publication No. 2000-296583

[0014] Patent Document 2: Japanese Patent Application Laid-Open No. 5-181400

[0015] Patent Document 3: Japanese Patent Application Laid-Open No. 11-184363 Summary of the invention

[0016] Problems to be solved by the invention

[0017] However, the above-mentioned related art has the following problems.

[0018] The holographic laminate described in Patent Document 1 is mainly used in a head-up display for a vehicle to be viewed by a driver. Therefore, the image quality of the displayed image may not be particularly high. However, in the case of a wearable display or a head-mounted display for AR or MR, for example, a realistic image is often displayed in the user's full field of view, or fine text is displayed. Such applications require further high image quality.

[0019] According to the research of the present inventors, when the holographic layer in the light guide plate for image display is sandwiched by the resin substrate, even if the maximum height Rmax is less than 25 μm, the image quality may be reduced. For example, when the surface of the extruded resin substrate has undulations (tooth patterns) of a pitch corresponding to the meshing pitch of the drive gear of the extrusion roller, it is easy to produce unclear image areas.

[0020] In the technique described in Patent Document 2, a resin substrate is closely attached to the surface of the photosensitive material layer on the opposite side to the aqueous polymer protective barrier.

[0021] Therefore, in a high temperature environment, the photosensitive material may corrode the resin substrate.

[0022] In addition, since the resin-made substrate contains moisture inside, the moisture diffuses into the photosensitive material layer through the close contact surface with the photosensitive material layer. In addition, since the substrate is exposed to the outside, moisture continues to penetrate into the substrate from the outside. As a result, since moisture penetrates into the photosensitive material layer through the resin-made substrate, even if the water-based polymer protective barrier is used to block the moisture, the photosensitive material layer cannot be prevented from deteriorating over time due to moisture from the substrate side.

[0023] In the technology described in Patent Document 3, the entire periphery of the laminate including the hologram is sealed with a protective coating layer. Therefore, it is possible to suppress the situation where moisture penetrates from the outside of the holographic laminate to the inside and deteriorates the hologram. However, when the protective coating layer is formed, the moisture contained in the resin matrix is ​​sealed inside the protective coating layer. As a result, the moisture contained in the resin matrix also penetrates into the hologram, which may cause the hologram to deteriorate over time. In particular, in a high temperature environment, the influence of moisture release from the resin substrate becomes significant.

[0024] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a light guide plate for image display that can display a clear image even when a resin substrate is used.

[0025] Another object of the present invention is to provide a light guide plate for image display capable of suppressing degradation of a hologram layer even when a resin substrate is used.

[0026] Means for solving problems

[0027] The inventors of the present invention have conducted intensive research and have found that by improving the flatness of a resin substrate used in a light guide plate for image display corresponding to the size of surface undulations (which change at a pitch significantly larger than the pitch measured by the surface roughness), a clear image can be displayed, thereby achieving the present invention.

[0028] When the flatness of the surface of the resin substrate is reduced due to the undulation, the thickness of the hologram layer stacked on the resin substrate fluctuates. When the thickness of the hologram layer fluctuates, the guided light fluctuates, resulting in minute distortion and deformation of the image, making the image unclear. In the case of a color image, the fluctuation of the guided light causes color shift and bleeding, resulting in unclear images.

[0029] On the other hand, when the smoothness of the surface of the resin substrate is reduced due to fine irregularities, scattering of the guided light occurs, resulting in unclear images.

[0030] The present inventors have conducted intensive studies and have found that by introducing a barrier layer into a resin substrate having a hologram layer used in a light guide plate for image display, degradation of the hologram layer can be suppressed and a clear image can be displayed, thereby completing the present invention.

[0031] In order to solve the above-mentioned problems, the present invention has the following aspects, for example.

[0032] [1] A light guide plate for image display, comprising a first resin substrate and a holographic layer, wherein:

[0033] The MC value of the first resin substrate obtained by dark tone contrast evaluation is 0.120 or less.

[0034] [2] A light guide plate for image display, comprising a first resin substrate, a first barrier layer, and a hologram layer.

[0035] [3] The image display light guide plate according to [2], wherein the first resin substrate, the first barrier layer, and the holographic layer are arranged in this order in the thickness direction.

[0036] [4] The light guide plate for image display according to [3], wherein

[0037] The light guide plate further comprises a second resin substrate and a second barrier layer.

[0038] The first resin substrate, the first barrier layer, the holographic layer, the second barrier layer, and the second resin substrate are arranged in this order in the thickness direction.

[0039] [5] The image display light guide plate according to any one of [2] to [4], wherein the refractive index of the first barrier layer is higher than the refractive index of the first resin substrate.

[0040] [6] The image display light guide plate according to any one of [2] to [5], wherein the refractive index of the first barrier layer is 1.48 or more.

[0041] [7] The image display light guide plate according to any one of [2] to [6], wherein the first barrier layer comprises an inorganic material.

[0042] [8] The light guide plate for image display according to [7], wherein the first barrier layer comprises at least one inorganic material selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon, aluminum oxide and glass.

[0043] [9] The image display light guide plate according to any one of [2] to [8], wherein the first barrier layer is disposed on a resin film.

[0044]

[10] The image display light guide plate according to any one of [2] to [9], wherein a water vapor barrier material is used as the material of the first barrier layer.

[0045]

[11] The image display light guide plate according to any one of [2] to

[10] , wherein the first barrier layer is arranged on the holographic layer.

[0046]

[12] The image display light guide plate according to any one of [1] to

[11] , wherein the refractive index of the first resin substrate is 1.48 to 1.70.

[0047]

[13] The light guide plate for image display as described in any one of [1] to

[12] , wherein the first resin substrate comprises at least one resin selected from the group consisting of poly(meth)acrylic resins, epoxy resins, cyclic polyolefins and polycarbonates.

[0048]

[14] The image display light guide plate according to any one of [1] to

[13] , wherein the first resin substrate has a heat shrinkage rate of less than 3% as measured in accordance with Appendix A of JIS K 6718-1:2015.

[0049]

[15] The image display light guide plate according to any one of [1] to

[14] , wherein the arithmetic mean roughness Ra of the surface of the first resin substrate is 10 nm or less.

[0050] Effects of the Invention

[0051] According to the present invention, it is possible to provide a light guide plate for image display that can display a clear image even when a resin substrate is used.

[0052] Furthermore, according to the present invention, it is possible to provide a light guide plate for image display that can suppress degradation of a hologram layer even when a resin substrate is used. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 This is a schematic cross-sectional view showing an example of the image display light guide plate according to the first embodiment of the present invention.

[0054] Figure 2 This is a schematic front view for explaining the evaluation method of the MC value.

[0055] Figure 3 This is a schematic plan view for explaining the evaluation method of the MC value.

[0056] Figure 4This is a schematic diagram showing an example of an image for evaluating the MC value.

[0057] Figure 5 This is a schematic diagram showing an example of a digital evaluation image of the MC value.

[0058] Figure 6 It is a schematic graph showing a method of calculating the MC value.

[0059] Figure 7 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a first modified example of the first embodiment of the present invention.

[0060] Figure 8 This is a schematic longitudinal sectional view showing an example of a manufacturing apparatus for a resin substrate according to Example 1.

[0061] Fig. 9 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a second embodiment of the present invention.

[0062] Fig.10 It is a schematic front view illustrating the method of measuring the brightness value and FOV.

[0063] Fig.11 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a first modified example of the second embodiment of the present invention.

[0064] Fig.12 1 is a schematic cross-sectional view showing a light guide plate for image display according to Example 5.

[0065] Fig.13 This is a schematic cross-sectional view showing a light guide plate for image display according to Example 6.

[0066] Fig.14 It is a schematic diagram showing the layer structure of the light guide plate for image display according to the third embodiment of the present invention.

[0067] Fig.15 It is a schematic diagram showing the layer structure of the light guide plate for image display according to the first modified example of the third embodiment of the present invention.

[0068] Fig.16 This is a diagram showing a state where two hard coating films according to the third embodiment are overlapped.

[0069] Fig.17 This is a diagram showing a state where two hard coating films are overlapped in a first modification of the third embodiment.

[0070] Fig.18 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a fourth embodiment of the present invention.

[0071] Fig.19 This is a schematic cross-sectional view showing an example of a display device including a light guide plate for image display according to a fourth embodiment of the present invention.

[0072] Fig. 20 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a first modified example of the fourth embodiment of the present invention.

[0073] Fig.21 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a second modified example of the fourth embodiment of the present invention.

[0074] Fig. 22 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a third modified example of the fourth embodiment of the present invention. DETAILED DESCRIPTION

[0075] Embodiments of the present invention will be described below with reference to the accompanying drawings. In all the drawings, even when the embodiments are different, the same or corresponding components are given the same reference numerals, and the common description is omitted.

[0076] The numerical range expressed using “~” includes the values ​​on both ends of the “~”.

[0077] "UV" means ultraviolet light.

[0078] “(Meth)acrylic acid” means one or both of acrylic acid and methacrylic acid.

[0079] “(Meth)acrylate” refers to one or both of acrylate and methacrylate.

[0080] [First embodiment]

[0081] <Basic example>

[0082] A light guide plate for image display according to a first embodiment of the present invention will be described.

[0083] The image display light guide plate of the first embodiment of the present invention has a first resin substrate and a holographic layer. The image display light guide plate of this embodiment may further have a second resin substrate. In this embodiment, the first resin substrate and the second resin substrate are sometimes referred to as "resin substrates" below. The above-mentioned resin substrate is transparent.

[0084] The hologram layer is sandwiched between the first resin substrate and the second resin substrate, or between the first resin substrate and the glass substrate.

[0085] The above-mentioned light guide plate for image display has an incident portion for incident image light, and a display image emission portion for displaying an image based on the image light. The above-mentioned holographic layer is arranged between the above-mentioned incident portion and the above-mentioned display image emission portion. The above-mentioned holographic layer has a diffraction grating pattern formed therein, which is used to guide at least the image light incident from the above-mentioned incident portion to the above-mentioned display image emission portion and emit it from the above-mentioned display image emission portion. The diffraction grating pattern of the above-mentioned display image emission portion transmits at least a part of the external light incident from the outside of the above-mentioned light guide plate for image display. It should be noted that the above-mentioned external light incident portion refers to the surface opposite to the above-mentioned display image emission portion.

[0086] The image light incident on the incident portion is guided into the holographic layer and emitted to the outside from the display image emitting portion. On the other hand, the external light also passes through the resin substrate and the display image emitting portion, and as a result, an observer of the display image emitting portion can observe both the image light and the external light in the field of view.

[0087] The image display light guide plate of this embodiment can be suitably used in a display device using AR technology or MR technology. For example, the image display light guide plate of this embodiment can be used in devices such as AR glasses such as head-mounted displays or head-up displays for vehicles.

[0088] In the resin substrate used in the light guide plate for image display of the present embodiment, the MC value obtained by the evaluation based on the dark tone contrast is less than 0.120. The definition of the MC value and the specific evaluation method are described below. The above MC value is effective in the evaluation of the surface characteristics of the above resin substrate, especially the planarity. That is, for the concavities and convexities having a lower spatial frequency than the spatial frequency of the concavities and convexities of the surface roughness, the lower the above MC value, the smaller the degree of the concavities and convexities. Therefore, the lower the above MC value of the resin substrate, the better the planarity.

[0089] The material of the resin substrate is not particularly limited as long as it is a transparent material.

[0090] The material used for the resin substrate preferably contains at least one resin selected from the group consisting of acrylic resins, cyclic polyolefin resins, and polycarbonate resins, and is more preferably an acrylic resin.

[0091] The refractive index of the material used for the resin substrate is preferably 1.48 to 1.70.

[0092] The heat shrinkage of the material used for the resin substrate is preferably less than 3%. Here, the heat shrinkage is a dimensional change rate upon heating based on Appendix A "Measurement of dimensional change (shrinkage) upon heating" of JISK 6718-1:2015.

[0093] It should be noted that the "measurement of dimensional change (shrinkage) during heating" is a standard for cast plates, but even when the resin substrate using the above-mentioned material is an extruded plate, a continuously cast plate, etc., the heat shrinkage rate in the present invention can also adopt a value based on this standard.

[0094] The smoothness of the resin substrate (expressed by surface roughness such as arithmetic mean roughness Ra or maximum height Rmax, for example) is preferably 10 nm or less in terms of arithmetic mean roughness Ra of the surface of the resin substrate.

[0095] In addition, a barrier layer described later may be introduced into the light guide plate for image display of the present embodiment. By introducing the barrier layer, degradation of the hologram layer can be suppressed and a clear image can be maintained.

[0096] The resin substrate having excellent flatness such as the above MC value can be produced by, for example, using a production method such as a casting method or an extrusion method, or by subjecting the resin substrate to post-processing such as cutting, grinding, or hot pressing.

[0097] As the above-mentioned casting method, a glass casting method can be used. In the above-mentioned glass casting method, the raw material of the above-mentioned resin substrate is flowed into between glass plates with good flatness and smoothness, and then a polymerization process is performed to solidify the raw material of the above-mentioned resin. In the case of manufacturing the above-mentioned resin substrate by the above-mentioned glass casting method, the surface shape of the glass used in the glass casting method (hereinafter sometimes referred to as "casting glass") is transferred to the above-mentioned resin substrate. Therefore, as long as the surface flatness and smoothness of the above-mentioned casting glass are good, the surface flatness and smoothness of the above-mentioned resin substrate are also good.

[0098] The smaller the internal strain (distortion) of the above-mentioned casting glass, the better the flatness of the surface of the above-mentioned casting glass, and thus the flatness of the above-mentioned resin substrate can be improved. For example, as the above-mentioned casting glass, non-strengthened glass is more preferable than tempered glass. However, even if it is tempered glass, as long as it is chemically strengthened glass with less strain than air-cooled tempered glass, the flatness of the above-mentioned resin substrate can be improved.

[0099] The thicker the cast glass is, the more the rigidity of the cast glass can be improved, and deformation of the glass during production can be suppressed, so that the planarity of the resin substrate can be improved.

[0100] When the resin base material is molded, if the casting glass is pressed by applying a surface pressure, the smoothness and planarity of the resin base material can be improved.

[0101] The above-mentioned pouring method is not limited to the above-mentioned glass pouring method.

[0102] For example, as a casting, an endless belt made of metals facing each other can be used. In this case, by rotating the endless belt while performing a polymerization step, the resin substrate can be continuously manufactured. The surface shape of the endless belt is transferred to the resin substrate. Therefore, by applying mirror finish to the surface of the endless belt, the smoothness of the resin substrate can be improved. In addition, by controlling the tension of the endless belt, the planarity of the resin substrate can be improved.

[0103] As another pouring method, there is a method of using a metal plate instead of the above-mentioned pouring glass.

[0104] In the polymerization step of the casting method, the lower the curing speed, the easier it is for the surface shape of the casting to be transferred to the resin substrate, so that the planarity and smoothness of the resin substrate can be improved.

[0105] As a means for reducing the curing speed, for example, a means such as reducing the amount of the polymerization initiator or lowering the polymerization temperature can be used.

[0106] The less the amount of the crosslinking agent added to crosslink the material of the resin substrate, the lower the curing speed can be, and the surface shape of the cast can be easily transferred to the resin substrate, thereby improving the planarity of the resin substrate. The amount of the crosslinking agent added is preferably a trace amount of 0.5 parts by mass or less relative to 100 parts by mass of the total polymerizable monomer component and polymerizable oligomer component other than the crosslinking agent as the raw material of the resin substrate.

[0107] A release agent may be used in the casting, and the smaller the amount used, the better. This makes it easier to transfer the surface shape of the casting using the resin substrate, and can improve the planarity and smoothness of the resin substrate.

[0108] In the polymerization step in the casting method, by pre-polymerizing the monomer for forming the substrate, the planarity and smoothness of the resin substrate can be improved.

[0109] In the polymerization step in the above-mentioned casting method, casting polymerization is carried out by using a raw material formed by dissolving a substrate-forming polymer in a substrate-forming monomer, which can reduce curing shrinkage and facilitate transfer of the above-mentioned cast surface shape to the above-mentioned resin substrate, thereby improving the flatness and smoothness of the above-mentioned resin substrate.

[0110] In the above-mentioned casting method, two or more of the above-mentioned techniques may be used in combination. In this case, the planarity and smoothness of the above-mentioned resin substrate can be further improved by the synergistic effect of each technique.

[0111] When the resin substrate is produced by extrusion, for example, a polishing roll method or an air knife method can be used.

[0112] Depending on the processing accuracy of the parting line of the extrusion die, the fine concavo-convex of the parting line may be transferred, thereby reducing the smoothness of the surface of the resin substrate. Therefore, the extrusion die is finished with high precision so that the parting line is smooth.

[0113] For example, in the polishing roller method, the molten resin is usually cooled by clamping and pressing with a set of three polishing rollers. When the polishing rollers are clamped, the pressure applied to the molten resin is a linear pressure. This linear pressure is easily affected by the uneven rotation of the polishing rollers and the deviation of the processing accuracy of the roller shaft or the machine. Therefore, the linear pressure becomes uneven, and the flatness reduction such as uneven thickness and tooth pattern is easily generated in the resin substrate. The tooth pattern is generated in a linear shape extending in a direction orthogonal to the feeding direction of the resin substrate.

[0114] If the surface temperature of the polishing roller is too high, the resin substrate is likely to be deformed, and therefore the surface temperature is preferably low.

[0115] As the feed mechanism of the polishing roller, it is more preferable to use a structure with reduced drive unevenness. For example, regarding the transmission mechanism such as the reducer of the feed mechanism, in order to suppress the transmission of the meshing vibration of the gear, a planetary roller can be used instead of the gear transmission mechanism. However, as long as it is a gear transmission mechanism such as a worm gear or a spiral bevel gear that is less likely to cause meshing vibration than a flat gear, it can be used as the transmission mechanism of the feed mechanism.

[0116] Instead of the polishing roller, a pair of seamless metal belts for cooling the molten resin may be disposed opposite to each other at a predetermined interval at the molten resin outlet of the extruder. In this case, the molten resin is clamped by the pair of seamless metal belts and conveyed while being cooled. As a result, the pressure applied to the molten resin becomes a surface pressure, thereby suppressing the reduction in flatness due to linear pressure in the polishing roller method.

[0117] The hologram layer uses a known resin material for forming a hologram. For example, as the resin material for forming a hologram, a known material can be appropriately selected and used. The photosensitive material can be appropriately determined in consideration of the wavelength of the light to be guided, and an acrylic hologram-forming photosensitive resin material having excellent optical properties can also be used.

[0118] The holographic layer may be formed on the surface of the resin substrate or laminated on the resin substrate with a suitable transparent layer interposed therebetween. When the image display light guide plate includes a glass substrate, the holographic layer may be formed on the surface of the glass substrate or laminated on the glass substrate with a suitable transparent layer interposed therebetween.

[0119] The resin substrate may be disposed at the outermost portion in the thickness direction of the image display light guide plate, or may be disposed inside. When the image display light guide plate includes the glass substrate, the glass substrate may be disposed at the outermost portion in the thickness direction of the image display light guide plate, or may be disposed inside.

[0120] In the image display light guide plate, one or more appropriate transparent layers may be disposed between the resin substrate and the hologram layer in the thickness direction, or between the glass substrate and the hologram layer when the glass substrate is included.

[0121] In the light guide plate for image display, a resin substrate and one or more appropriate transparent layers different from the glass substrate may be arranged on the outermost side in the thickness direction.

[0122] For example, when a transparent layer is disposed on at least one surface of a resin substrate, the transparent layer may be a hard coat layer that protects the surface of the resin substrate.

[0123] Examples of other transparent layers include an absorption layer having an absorption peak in UV or a specific wavelength range and an adhesive layer.

[0124] The following is based on Figure 1 The illustrated example explains the detailed configuration of an example of the image display light guide plate according to the present embodiment. Figure 1 This is a schematic cross-sectional view showing an example of the image display light guide plate according to the first embodiment of the present invention.

[0125] Figure 1 In the illustrated image display light guide plate 1004 , a first resin substrate 1001 , a hologram layer 1002 , and a second resin substrate 1003 are arranged in this order in the thickness direction.

[0126] The planar shape of the image display light guide plate 1004 is not particularly limited. For example, the image display light guide plate 1004 may be shaped into a shape that can be mounted in a display device to be used.

[0127] For example, the image display light guide plate 1004 may be a rectangular plate larger than the shape to be mounted on the display device. In this case, the image display light guide plate 1004 is cut into a shape that can be mounted on the display device before being mounted on the display device.

[0128] The image display light guide plate 1004 may be in the form of a flat plate, or may be in the form of a curved plate as required.

[0129] The following description will take as an example a case where the image display light guide plate 1004 is composed of a flat plate that is rectangular in plan view.

[0130] The first resin substrate 1001 is disposed on the outermost portion in the thickness direction of the image display light guide plate 1004. The first resin substrate 1001 is disposed on the surface of the image display side of the image display light guide plate 1004.

[0131] The first resin substrate 1001 has the same outer shape as that of the image display light guide plate 1004 .

[0132] Image light emitted from the hologram layer 1002 and external light transmitted through a second resin substrate 1003 and the hologram layer 1002 described later are transmitted through the first resin substrate 1001 .

[0133] The thickness of the first resin substrate 1001 is not particularly limited. For example, the thickness of the first resin substrate 1001 can be 0.05 to 2 mm. When the thickness of the first resin substrate 1001 is 0.05 mm or more, it is easy to maintain a stable shape, and the measurement error of the MC value described later can be suppressed to a small value, which is preferred. When the thickness of the first resin substrate 1001 is 2 mm or less, the mass of the light guide plate 1004 for image display can be reduced and lightweight can be achieved, so it is preferred. The thickness of the first resin substrate 1001 is preferably 0.05 mm or more, more preferably 0.1 mm or more, and further preferably 0.5 mm or more. On the other hand, from the perspective of deformation or residual strain of the substrate caused by the water absorption of the substrate, the thickness of the first resin substrate 1001 is preferably 2 mm or less, more preferably 1.5 mm or less, and further preferably 1 mm or less.

[0134] As materials that can be used in the first resin substrate 1001, for example, there can be cited organic materials such as polyethylene terephthalate, polyethylene naphthalate, polyether sulfone, polyimide, nylon, polystyrene, polyvinyl alcohol, ethylene vinyl alcohol copolymer, fluororesin film, polyvinyl chloride, polyethylene, polypropylene, cyclic polyolefin, cellulose, acetyl cellulose, polyvinylidene chloride, aromatic polyamide, polyphenylene sulfide, polyurethane, polycarbonate, poly(meth)acrylic resin, phenol resin, epoxy resin, polyarylate, polynorbornene, styrene-isobutylene-styrene block copolymer (SIBS), and allyl diglycol carbonate, preferably containing at least one resin selected from the group consisting of poly(meth)acrylic resin, epoxy resin, cyclic polyolefin and polycarbonate.

[0135] From the perspective of the transparency of the first resin substrate 1001, polycarbonate or poly (meth) acrylic resin is preferably used. From the perspective of the process resistance such as chemical resistance and processability of the first resin substrate 1001, poly (meth) acrylic resin, epoxy resin or cyclic polyolefin is preferably used. Among them, poly (meth) acrylic resin is more preferred because it can take into account both transparency and process resistance.

[0136] As the first resin base material 1001 , a plate having an MC value of 0.120 or less obtained by evaluation based on dark tone contrast was used.

[0137] Here, the specific evaluation method and calculation method of the MC value are described.

[0138] Figure 2 This is a schematic front view for explaining the evaluation method of the MC value. Figure 3 This is a schematic plan view for explaining the evaluation method of the MC value. Figure 4 This is a schematic diagram showing an example of an image for evaluating the MC value. Figure 5 This is a schematic diagram showing an example of a digital evaluation image of the MC value. Figure 6 It is a schematic graph showing a method of calculating the MC value.

[0139] (Dark tone contrast evaluation)

[0140] Dark contrast evaluation can be used Figure 2 and Figure 3 The evaluation device 1200 shown is used for this purpose.

[0141] The evaluation device 1200 includes a light source 1201, a screen 1202, and a camera 1203 (see Figure 3 ) and the operation processing unit 1204 (refer to Figure 3 ).

[0142] In the evaluation device 1200 , the measurement sample S is irradiated with measurement light emitted from the light source 1201 , thereby forming a transmission projection image of the measurement sample S on the screen 1202 , and the MC value of the measurement sample S is calculated based on the brightness distribution of the transmission projection image.

[0143] The shape of the measurement sample S is the same as the outer shape of the first resin substrate 1001. The following description will take as an example a case where the measurement sample S is a flat plate having a rectangular shape in plan view.

[0144] The type of light source 1201 is not particularly limited as long as it can form a transmission projection image of the measurement sample S. For example, as the light source 1201, it is more preferable to use a point light source from the perspective of a clear transmission projection image projected onto the screen 1202. Examples of point light sources include metal halide lamps, halogen lamps, and high-pressure mercury lamps. The wavelength of light is preferably in the range of 280 to 780 nm. When the measurement sample S is a resin substrate, it is preferably in the range of 400 nm to 780 nm.

[0145] As the screen 1202, for example, a matte screen, a micro-bead screen, and a beaded screen can be cited. The color of the screen 1202 is not particularly limited as long as it does not hinder the brightness measurement of the projection image on the screen 1202. The color of the screen 1202 can be, for example, white or gray. The size of the screen 1202 is not particularly limited as long as it is a size that includes the transmission projection image of the measurement sample S in the required measurement range. The screen 1202 is more preferably a size that includes the transmission projection image of the entire measurement sample S or larger.

[0146] The type of camera 1203 is not particularly limited as long as it can accurately capture the brightness of the transmission projection image on the screen 1202. For example, the camera 1203 may be an analog camera or a digital camera. From the perspective of easy digital analysis, the camera 1203 is more preferably a digital camera. It should be noted that, in the case of capturing with an analog camera, the image analysis described below is performed after the obtained image is converted into a digital image.

[0147] As the size of the digital image, if it is expressed as the number of horizontal and vertical pixels, for example, 800×600, 1024×768, 1600×1200, 2048×1536, or 5472×3648 is used. However, the size of the digital image is not limited to these as long as it has a resolution that can obtain a curve of brightness change corresponding to the unevenness of the measurement sample S caused by undulations, etc.

[0148] The brightness value is the shade after the data of each pixel is converted to a single color. The resolution of the brightness value is determined by the grayscale number of each pixel. The grayscale number of each pixel is not particularly limited as long as the MC value below 0.120 can be calculated. The grayscale number of each pixel can be, for example, 128 grayscales, 256 grayscales, 512 grayscales, or 1024 grayscales.

[0149] However, when the contrast of the transmission projection image is reduced due to constraints such as the transmittance of the measurement sample S and the brightness of the light source 1201, it is more preferable to use as high a grayscale number as possible in order to improve measurement accuracy.

[0150] The shooting using the camera 1203 is preferably performed under light shielding. When the shooting using the camera 1203 is performed under light shielding, a higher-precision brightness distribution can be obtained compared to the case where it is not performed under light shielding. The method of shooting under light shielding is not particularly limited. For example, when the shooting environment in which the evaluation device 1200 is configured is a room with a window, the window slits can be pasted to make the entire room light-shielded. For example, the evaluation device 1200 can have a light-shielding housing that surrounds at least the optical path from the light source 1201 to the screen 1202 and the optical path from the screen 1202 to the camera 1203.

[0151] The shooting mode of the camera 1203 may be a color image mode or a monochrome image mode. When shooting in the color image mode, it is more preferable to convert the image into a monochrome image using image processing software.

[0152] For example, due to the influence of the optical characteristics of the lens of the camera 1203, the brightness of the end of the captured image may be lower than the brightness of the center. In the case where the noise caused by such uneven brightness is too large, it is more preferable to perform shading correction on the captured image in advance according to the optical characteristics of the lens and then obtain the brightness distribution of the measurement sample S. Shading correction can be performed using appropriate image processing software before analyzing the captured image. Regarding the correction amount of shading correction, for example, a correction glass plate with good flatness and smoothness can be used instead of the measurement sample S for shooting, and the correction amount can be determined in such a way that the brightness distribution is uniform. In this case, the brightness unevenness based on the optical characteristics of the light source 1201 is also corrected.

[0153] In the following, for simplicity of description, the camera 1203 is described as a digital camera that captures the transmission projection image of the screen 1202 in the monochrome image mode. In this case, the output value of the pixel of the digital image is proportional to the brightness of the transmission projection image.

[0154] When the camera 1203 is an analog camera, the digital image described below may be replaced with a digital image generated from an image captured by the camera 1203 .

[0155] The calculation processing unit 1204 obtains the brightness distribution based on the digital image captured by the camera 1203, and calculates the MC value based on the brightness distribution. The calculation processing unit 1204 includes a computer capable of executing appropriate image processing software.

[0156] The arrangement of each unit in the evaluation device 1200 and the arrangement of the measurement sample S during measurement will be described.

[0157] Hereinafter, the positional relationship is sometimes described based on the XYZ orthogonal coordinate system. The X-axis extends along the horizontal plane. The Y-axis is orthogonal to the X-axis on the horizontal plane. The Z-axis is a vertical axis, which is orthogonal to the X-axis and the Y-axis. The direction along the X-axis, the direction along the Y-axis, and the direction along the Z-axis are referred to as the X-direction, the Y-direction, and the Z-direction, respectively.

[0158] like Figure 2 As shown, in the evaluation device 1200, the screen 1202 is arranged parallel to the YZ plane. The light source 1201 is arranged at a distance (d1+d2) from the screen 1202 in the X direction. The optical axis O of the light source 1201 is parallel to the X axis.

[0159] like Figure 3As shown in FIG. 1 , the measurement sample S is arranged in the middle of the light source 1201 and the screen 1202 on the optical axis O. When the vertices of the rectangular shape in the cross section passing through the center in the thickness direction of the measurement sample S are represented by A, B, C, and D, the side AD and the side BC are parallel to the Y axis. The side AD represents the side close to the light source 1201, and the side BC represents the side close to the screen 1202.

[0160] like Figure 2 As shown, the center SO of the rectangle ABCD in the measurement sample S is arranged on the optical axis O and is away from the light source 1201 by a distance d1 in the X direction. In addition, the measurement sample S is arranged in the following posture: it is rotated by an elevation angle θ in a clockwise manner as shown in the figure, with an axis passing through the center SO in a horizontal plane and parallel to the Y axis as the center. A However, when the thickness of the measurement sample S is thin, the center of one surface in the thickness direction of the measurement sample S may be arranged at the same position as described above instead of the center SO of the measurement sample S.

[0161] Here, the distances d1 and d2 are appropriately set according to, for example, the radiation angle and light quantity of the light source 1201, the size of the measurement sample S, and the size of the screen 1202. For example, the distances d1 and d2 may be 30 to 1000 cm.

[0162] For example, the distance d1 is more preferably as short as possible within the range where the light source 1201 can be installed. The distance d2 is more preferably as short as possible within the range where the screen 1202 can be installed. The shorter the distances d1 and d2 are, the more efficiently the measurement light emitted by the light source 1201 can be used.

[0163] Elevation angle θ A It is preferably 5 to 90 degrees. A The measurement was performed at 20°.

[0164] The arrangement position of the camera 1203 is not particularly limited as long as it is a position where its own shadow and reflected light are not reflected in the imaging range and the entire transmission projection image on the screen 1202 can be imaged. Figure 3 In the example shown, the camera 1203 is arranged at a position adjacent to the camera 1203 in the Y direction when viewed from above. Although not particularly shown, by arranging the camera 1203 at a different height from the measurement sample S in the Z direction, it can be arranged at a position where its own shadow and reflected light are not projected into the imaging range.

[0165] With such an arrangement, the measurement light emitted from the light source 1201 is projected onto the screen 1202 after passing through the measurement sample S. When the light source 1201 is a point light source, the measurement light is radially diffused, so a transmission projection image is formed on the screen 1202 based on the light intensity of the light transmitted through the measurement sample S. The transmission projection image is captured by the camera 1203 and sent to the calculation processing unit 1204 in the form of a digital image.

[0166] For example, Figure 4 The digital image schematically shown in FIG. 1 is sent to the operation processing unit 1204 . Figure 4 The outermost frame in represents the end of the screen 1202. The trapezoid PaPbPcPd in ​​the center represents the transmission projection image I of the measurement sample S. Points Pa, Pb, Pc, and Pd correspond to points A, B, C, and D of the measurement sample S, respectively.

[0167] The transmission projection image I has a brightness distribution. Figure 4 In the example shown, there are a high brightness portion Ib and a low brightness portion Is. The high brightness portion Ib is formed by projecting measurement light transmitted according to the transmittance of the measurement sample S onto the screen 1202 .

[0168] The brightness distribution on the transmission projection image I includes brightness unevenness caused by the optical path length and the intensity distribution of the radiated light from the light source 1201. Even if the measurement sample S does not have a concave-convex defect, this brightness unevenness will occur to a certain extent.

[0169] Since the measurement light is radiated light, the light intensity of the measurement light traveling along the optical axis O is the largest, and decreases toward the periphery of the measurement sample S. The radiated light intensity distribution of the light source 1201 is also the same.

[0170] When the brightness unevenness is greater than the brightness unevenness caused by the concavo-convex defect, correction is performed in advance. For example, when the difference between the brightness value on the optical axis O and the brightness value at the outer edge of the measurement sample S is 5 or more, it is more preferable to correct the brightness unevenness.

[0171] The brightness unevenness caused by the light intensity distribution of the measurement light can be corrected based on, for example, the law of light attenuation (the intensity of the attenuated light is inversely proportional to the square of the distance from the light source). For example, the brightness unevenness caused by the intensity distribution of the radiated light of the light source 1201 can be corrected based on the intensity distribution of the radiated light of the light source 1201.

[0172] For example, by performing imaging using a calibration glass plate as described above, calibration data can be obtained.

[0173] However, when there is only brightness unevenness smaller than that caused by the unevenness due to the concavo-convex defect depending on the measurement conditions, correction of the light intensity distribution of the measurement light and the light source 1201 may be omitted.

[0174] Next, the removal of brightness unevenness which is measurement noise will be described.

[0175] It is considered that the low brightness portion Is is formed by a concavo-convex defect corresponding to an error in the planarity of the surface of the measurement sample S.

[0176] For example, when the curvature radius of the concavoconvex formed in the measurement sample S is relatively small, it is considered that the measurement light is diffused by the lens effect of the concavoconvex part before reaching the screen 1202. This depends on the smoothness.

[0177] For example, when the measurement sample S is deformed in a wave shape, the thickness may not change even if there are surface irregularities. This depends on the flatness. It is believed that in this case, the irregularities do not have a lens effect, but will produce the same refraction and diffraction of the measurement light, thus playing a role in brightness unevenness.

[0178] Furthermore, it is also considered that, for example, by measuring the unevenness formed in the sample S, a strain distribution is generated near the unevenness, the emission direction of the measurement light is disturbed, and the light intensity on the screen 1202 changes.

[0179] For example, if the incident angle to the measurement sample S increases, the change in the transmittance characteristics depending on the incident angle increases. Therefore, it is also believed that the transmittance of the concave and convex parts formed in the measurement sample S changes and plays a role in the uneven brightness. It is also believed that the transmittance that changes due to the uneven refractive index caused by the strain inside the measurement sample S also plays a role in the uneven brightness.

[0180] It is believed that the uneven brightness will be caused by any one or more combinations of these factors. It is further believed that the magnitude of the uneven brightness is highly correlated with the depth of the uneven brightness. Therefore, the planarity of the sample S can be evaluated by measuring the difference in brightness between the low brightness portion Is and the high brightness portion Ib.

[0181] Figure 4 In the example shown, the low brightness portion Is is elliptical. Such a low brightness portion Is corresponds to an elliptical concave portion or convex portion in the surface of the measurement sample S. For example, in the case where tooth patterns are formed in the measurement sample S, the low brightness portion Is is formed in a stripe shape. In this case, the low brightness portion Is is formed at equal pitches in a direction orthogonal to the extrusion direction of the first resin substrate 1001 and in substantially parallel.

[0182] The calculation processing unit 1204 analyzes the digital image and calculates the MC value in the following manner.

[0183] The digital image used for measuring the MC value may be the entire trapezoid PaPbPcPd. However, when a portion of the measurement sample S is cut off and used in a display device, for example, the measurement may be performed over the entire range of the size used in the display device.

[0184] Depending on the situation, a part of the area inside the trapezoid PaPbPcPd can be extracted in a trapezoidal shape in the digital image used for the measurement of the measurement sample S. For example, regarding a defect to be detected by the MC value, when the directionality, pitch, etc. are known in advance, such as tooth pattern, a part of the area of ​​the trapezoid PaPbPcPd can be used as long as the measurement error is considered to include the size and range of two or more tooth patterns. This is also the case when the shape of the measurement sample S is designed to have a gentle curve.

[0185] For example, when the measurement sample S is a rectangular shape of 200 mm×200 mm in a plane, the measurement range preferably includes a rectangular range of at least 180 mm×80 mm on the measurement sample S. Here, the longitudinal direction of the measurement range coincides with the direction in which the brightness changes most.

[0186] For example, when the measurement sample S is not a flat plate but a curved plate, it is more preferable that the width of the measurement range in the direction having the curve is 50 mm or more. For example, when the measurement sample S has a spherical curve as a whole, it is more preferable that a rectangular range of 50 mm×50 mm is included with the top of the curve as the center.

[0187] Hereinafter, as an example, a case where the entire trapezoidal PaPbPcPd is used will be described.

[0188] The calculation processing unit 1204 obtains the brightness distribution on the predetermined measurement line. For example, the measurement line is a (N-1) line segment qiQi formed by connecting points qi (where i=1,...,N-1) obtained by dividing the side AD on the measurement sample S into N equal parts and points Qi (where i=1,...,N-1) obtained by dividing the side BC on the measurement sample S into N equal parts.

[0189] In this case, on the measurement sample S, point qi and point Qi are points on a plane parallel to the ZX plane.

[0190] Figure 4 Points qi, Qi on the transmission projection image I are shown.

[0191] For example, N can be appropriately selected according to the size of the concavo-convex defect between 2 and 10000. For example, in the case of a defect with a width of 100 mm, N can be selected so that the pitch of the measurement lines is about 1 to 20 mm.

[0192] For example, when the low brightness portion Is is in the form of stripes, the arrangement of the measurement sample S can be changed so that the measurement line intersects the low brightness portion Is to obtain a digital image. In this case, the measurement line N can be selected so that the interval between the measurement lines along the length direction of the low brightness portion Is is about 1 to 20 mm.

[0193] Figure 4 In the example shown, N=8. Figure 5 The measurement line L3 in FIG. Figure 4 Since the measurement line on the measurement sample S is projected as an oblique line, the measurement line L3 on the transmission projection image I becomes a digitized oblique line.

[0194] The calculation processing unit 1204 converts the coordinates of points qi and Qi on the measurement sample S into pixel coordinates on the transmission projection image I based on the positional relationship among the light source 1201 , the screen 1202 , and the measurement sample S, thereby extracting the brightness value of each measurement line.

[0195] Figure 6 An example of the brightness distribution along the measurement line L3 is schematically shown in FIG. Figure 6 The horizontal axis represents the position of the pixel in the Z direction, and the vertical axis represents the brightness value.

[0196] As shown in the curve 1210, the brightness on the measurement line L3 decreases from the point q3 to the point Q3 from a substantially constant high brightness value, reaches the minimum brightness value, and then becomes a substantially flat high brightness value again. In the Z direction, the interval from q3 to p1 and the interval from p2 to Q3 are both included in the high brightness portion Ib. The interval from p1 to p2 is included in the low brightness portion Is.

[0197] The calculation processing unit 1204 obtains the minimum value Lmin and the maximum value Lmax of the brightness based on such brightness distribution.

[0198] The MC value is defined by the following equation (1). The calculation processing unit 1204 calculates the MC value based on the following equation (1) using Lmin and Lmax.

[0199] [Number 1]

[0200]

[0201] The MC value is an index that objectively indicates the magnitude of the drop in the low brightness portion Is in the brightness distribution.

[0202] As described above, the worse the planarity of the measurement sample S, the lower the brightness of the low brightness portion Is. Therefore, the larger the MC value, the worse the planarity of the surface of the measurement sample S, and the smaller the MC value, the better the planarity of the surface of the measurement sample S.

[0203] Similarly, the calculation processing unit 1204 calculates the MC value for each measurement line.

[0204] The MC value of the measurement sample S is regarded as the maximum value among the MC values ​​of each measurement line.

[0205] As described above, in the image display light guide plate of the present invention, the MC value of the resin substrate needs to be 0.120 or less. Thus, the display image using a hologram such as AR or MR formed using the light guide plate has good clarity. The MC value of the resin substrate is 0.120 or less, preferably 0.110 or less, more preferably 0.100 or less, further preferably 0.080 or less, and particularly preferably 0.070 or less.

[0206] On the other hand, by making the MC value 0.001 or more, the substrates can be prevented from sticking to each other when the substrates are stacked, and the handling properties during substrate processing tend to be good. The MC value of the resin substrate is preferably 0.001 or more, more preferably 0.005 or more, further preferably 0.010 or more, and particularly preferably 0.020 or more.

[0207] As described above, in the image display light guide plate of the present invention, the refractive index of the resin substrate is preferably 1.48 to 1.70. This can increase the viewing angle when used as the image display light guide plate.

[0208] In addition, as described above, in the image display light guide plate of the present invention, the heat shrinkage of the resin substrate measured in accordance with Appendix A of JIS K 6718-1:2015 is preferably less than 3%. As a result, the clarity of a display image using a hologram such as AR or MR formed using the light guide plate tends to be good. The heat shrinkage is preferably less than 3.0%, more preferably 2.5% or less, and even more preferably 2.0% or less.

[0209] In addition, as described above, in the light guide plate for image display of the present invention, the arithmetic mean roughness Ra of the surface of the resin substrate is preferably 10 nm or less. As a result, the clarity of the display image using a hologram such as AR or MR formed using the light guide plate tends to be good. The arithmetic mean roughness Ra of the surface of the resin substrate is preferably 10 nm or less, more preferably 8 nm or less, and further preferably 5 nm or less.

[0210] Here, back to Figure 1 1004 is a diagram showing an image display light guide plate 1004.

[0211] The hologram layer 1002 in the image display light guide plate 1004 is laminated on the surface of the first resin substrate 1001. The structure of the hologram layer 1002 is not particularly limited. The hologram layer 1002 has a suitable diffraction grating corresponding to the function required of the image display light guide plate 1004 formed therein.

[0212] The second resin substrate 1003 is laminated on the surface of the hologram layer 1002 on the opposite side to the first resin substrate 1001. As the second resin substrate 1003, the same structure as the first resin substrate 1001 is used. However, the thickness and material of the second resin substrate 1003 may be different from those of the first resin substrate 1001. In particular, since the second resin substrate 1003 is arranged on the surface of the external light incident side opposite to the side where the displayed image is emitted in the image display light guide plate 1004, a material having a higher surface hardness than the first resin substrate 1001 can be used.

[0213] Such an image display light guide plate 1004 can be manufactured, for example, as follows.

[0214] Using the above-mentioned manufacturing method, the first resin substrate 1001 and the second resin substrate 1003 having an MC value of 0.120 or less are prepared. For example, a photopolymer material for forming a hologram is coated on the first resin substrate 1001. At this time, a transparent sealing layer having the same thickness as the hologram layer 1002 can be provided on the outer periphery of the first resin substrate 1001. In this case, the photopolymer material is coated on the concave portion formed by being surrounded by the sealing layer. After the hologram layer 1002 is formed, the sealing layer seals the outer periphery of the hologram layer 1002. As the sealing layer, a material having excellent gas barrier properties can be used. In this case, the durability of the hologram layer 1002 can be improved.

[0215] Thereafter, the second resin substrate 1003 is placed on the photopolymer material.

[0216] However, the above manufacturing sequence is an example. For example, a photopolymer material may be applied on the second resin substrate 1003, and then the first resin substrate 1001 may be placed on the photopolymer material.

[0217] Thereafter, the laminate of the first resin substrate 1001 , the photopolymer material, and the second resin substrate 1003 is bonded together by reduced pressure pressing.

[0218] Thereafter, interference fringes corresponding to the diffraction pattern are formed in the photopolymer material of the laminate, and a diffraction grating is formed in the photopolymer material.

[0219] In this way, the image display light guide plate 1004 is manufactured.

[0220] According to the image display light guide plate 1004, since the MC value of the first resin substrate 1001 and the second resin substrate 1003 is 0.120 or less, the concavo-convex defects on the respective surfaces are reduced. As a result, it is possible to suppress the disturbance of the optical paths of the image light that transmits the first resin substrate 1001 to display an image and the external light that transmits the second resin substrate 1003 and the first resin substrate 1001 and overlaps with the image light due to the influence of the concavo-convex defects. As a result, a clear image is displayed on the image display light guide plate 1004.

[0221] As described above, according to the present embodiment, it is possible to provide a light guide plate for image display that can display a clear image even when a resin substrate is used.

[0222] <First Modification>

[0223] A first modified example of the first embodiment of the present invention will be described.

[0224] Figure 7 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a first modified example of the first embodiment of the present invention.

[0225] like Figure 7 As shown, a light guide plate 1014 for image display according to a first modification of the first embodiment of the present invention is obtained by adding a first hard coating layer 1011A and a second hard coating layer 1011B to the light guide plate 1004 for image display according to the basic example of the first embodiment of the present invention.

[0226] The following description will focus on differences from the basic example of the first embodiment of the present invention.

[0227] The first hard coating layer 1011A and the second hard coating layer 1011B are provided mainly for the purpose of protecting the surface of the first resin substrate 1001. The materials of the first hard coating layer 1011A and the second hard coating layer 1011B are made of a high-hardness transparent material, at least one of which has a surface hardness higher than that of the surface of the first resin substrate 1001. As long as at least one of the first hard coating layer 1011A and the second hard coating layer 1011B has a high hardness higher than that of the first resin substrate 1001, it may have a multilayer structure made of two or more transparent materials having different hardnesses.

[0228] Figure 7 In the example shown, the first hard coating layer 1011A is disposed on the first surface 1001a of the first resin substrate 1001 on the opposite side to the hologram layer 1002. The first hard coating layer 1011A forms the outermost surface of the light guide plate 1014 for image display.

[0229] The second hard coating layer 1011B is disposed on the second surface 1001 b of the first resin substrate 1001 which faces the hologram layer 1002 .

[0230] The thickness of the first hard coating layer 1011A is more preferably 1 to 50 μm.

[0231] The thickness of the second hard coating layer 1011B is more preferably 1 to 50 μm.

[0232] Regarding the planarity of the surface of the first hard coating layer 1011A and the second hard coating layer 1011B, when the MC value is measured in the form of a laminate of the first hard coating layer 1011A and the second hard coating layer 1011B and the first resin substrate 1001 (hereinafter referred to as the coated substrate), it is more preferably 0.120 or less.

[0233] The arithmetic mean roughness Ra of the surfaces of the first hard coating layer 1011A and the second hard coating layer 1011B is more preferably 10 nm or less.

[0234] The refractive index of the material of the first hard coating layer 1011A and the second hard coating layer 1011B is not particularly limited.

[0235] For example, from the perspective of visibility of the real image, the refractive index of the material of the first hard coating layer 1011A and the second hard coating layer 1011B should be preferably equal to or lower than that of the first resin substrate 1001. However, when selecting a material for the purpose of increasing the hardness of the hard coating layer, the refractive index may be higher than that of the first resin substrate 1001.

[0236] For example, when the refractive index of the material of the first hard coating layer 1011A and the second hard coating layer 1011B is equal to the refractive index of the material of the first resin substrate 1001, the interface between the surface of the first resin substrate 1001 and the first hard coating layer 1011A and the second hard coating layer 1011B disappears optically. In this case, the MC value of the substrate after coating substantially represents the degree of concavo-convex defects on the surface of the first hard coating layer 1011A and the second hard coating layer 1011B. For example, when the concavo-convex defects are reduced compared to the surface of the first resin substrate 1001 by forming the first hard coating layer 1011A and the second hard coating layer 1011B, the refractive index of the material of the first hard coating layer 1011A and the second hard coating layer 1011B is preferably close to the refractive index of the material of the first resin substrate 1001.

[0237] Generally, the refractive index of the material of the first hard coating layer 1011A and the second hard coating layer 1011B is different from the refractive index of the material of the first resin substrate 1001, so the following evaluation is obtained: the MC value of the substrate after coating includes both the uneven defects on the surfaces of the first hard coating layer 1011A and the second hard coating layer 1011B and the uneven defects on the surface of the first resin substrate 1001. However, by forming the layer thickness of the first hard coating layer 1011A and the second hard coating layer 1011B to a certain layer thickness, in the case where the uneven defects on the surfaces of the first hard coating layer 1011A and the second hard coating layer 1011B follow the uneven defects on the surface of the first resin substrate 1001, it can be considered that the MC value of the first resin substrate 1001 itself is equal to the MC value of the first resin substrate 1001 formed with the first hard coating layer 1011A and the second hard coating layer 1011B.

[0238] For example, from the perspective of wide viewing angle, the refractive index of the material of the first hard coat layer 1011A and the second hard coat layer 1011B is preferably equal to or higher than the refractive index of the material of the hologram layer 1002. As the refractive index increases, the critical angle of light guided tends to increase.

[0239] The surface hardness of the first hard coating layer 1011A and the second hard coating layer 1011B is not particularly limited as long as it is higher than the surface hardness of the first resin substrate 1001. For example, the pencil hardness (JIS K 5600-5-4: 1999) of the first hard coating layer 1011A and the second hard coating layer 1011B is preferably H or higher, and further preferably 2H or higher.

[0240] As materials suitable for the first hard coating layer 1011A and the second hard coating layer 1011B, for example, hard coating agents including polymerizable monomers or polymerizable oligomers that form a cured product by irradiation with active energy rays can be cited. As the above-mentioned polymerizable monomers, for example, (meth)acrylate monomers having a free radical polymerizable unsaturated group in the molecule can be cited. As the above-mentioned polymerizable oligomers, (meth)acrylate oligomers having a free radical polymerizable unsaturated group in the molecule can be cited.

[0241] As the above-mentioned (meth) acrylate monomer having a free radical polymerizable unsaturated group in the molecule, for example, at least one monomer selected from the group consisting of carbamate (meth) acrylate, polyester (meth) acrylate, epoxy (meth) acrylate, melamine (meth) acrylate, polyfluorinated (meth) alkyl acrylate and silicone (meth) acrylate can be cited. As the above-mentioned (meth) acrylate oligomer having a free radical polymerizable unsaturated group in the molecule, for example, an oligomer comprising a structural unit of at least one monomer selected from the group consisting of carbamate (meth) acrylate, polyester (meth) acrylate, epoxy (meth) acrylate, melamine (meth) acrylate, polyfluorinated (meth) alkyl acrylate and silicone (meth) acrylate can be cited. The above-mentioned polymerizable monomer or the above-mentioned polymerizable oligomer can also be used in combination of more than two kinds. Among these, for reasons such as high surface hardness, a monomer or oligomer of carbamate (meth) acrylate is preferred.

[0242] Examples of the urethane (meth)acrylate include urethane (meth)acrylates obtained by reacting a polyisocyanate compound with a (meth)acrylate compound having one hydroxyl group in its molecular structure, and urethane (meth)acrylates obtained by reacting a polyisocyanate compound with a (meth)acrylate compound having one hydroxyl group in its molecular structure and a polyol compound.

[0243] The first hard coating layer 1011A and the second hard coating layer 1011B may include a cured product of a polyfunctional (meth)acrylate.

[0244] Examples of the polyfunctional (meth)acrylate include trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol tetra(meth)acrylate, and dipentaerythritol tetra(meth)acrylate. alcohol octa(meth)acrylate, pentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerol tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate or di(trimethylolpropane) tetra(meth)acrylate, or those modified with PO, EO or caprolactone or the like.

[0245] When forming the first hard coating layer 1011A and the second hard coating layer 1011B, additives such as cross-linking agents, polymerization initiators, lubricants, plasticizers, organic particles, inorganic particles, antifouling agents, antioxidants or catalysts, or additives such as silicone or fluorine for preventing dirt and adhesion can be added to the hard coating agent within a range that does not hinder the physical properties.

[0246] The first hard coating layer 1011A and the second hard coating layer 1011B may use a material having a refractive index different from that of the first resin substrate 1001. In this case, the first hard coating layer 1011A and the second hard coating layer 1011B can change the refractive index of the outermost surface of the image display light guide plate 1014 and the refractive index based on the interface with the hologram layer 1002 according to the refractive index of the first resin substrate 1001.

[0247] Such a first variant of the first embodiment of the present invention, the image display light guide plate 1014 can be manufactured in the same manner as the basic example of the first embodiment of the present invention, for example, after the first resin substrate 1001 is formed in the same manner as the basic example of the first embodiment of the present invention, and before lamination with the photopolymer material for forming the holographic layer 1002, the first hard coating layer 1011A and the second hard coating layer 1011B are respectively formed on the first surface 1001a and the second surface 1001b of the first resin substrate 1001, and other aspects are the same as the basic example of the first embodiment of the present invention.

[0248] The first hard coating layer 1011A and the second hard coating layer 1011B can be formed by applying hard coating liquid as respective raw materials to the first surface 1001a and the second surface 1001b, respectively, and then curing the hard coating liquid. The coating method of the hard coating liquid is not particularly limited. For example, as the coating method of the hard coating liquid, there is the following method: directly coating a photocurable resin composition on the surface of a substrate by a coating method such as a casting method, a roller coating method, a rod coating method, a spray coating method, an air knife coating method, and a dipping method, and curing the coated film by light irradiation, thereby forming a cured film on the substrate.

[0249] In addition, for example, the following method can be cited: a photocurable resin composition is coated on the surface of at least one casting material used to constitute a mold for injection molding polymerization by the above-mentioned coating method, the coated film is irradiated with light to cure it, thereby forming a cured film on the mold material, a mold for injection molding polymerization is assembled using the mold material in a manner such that the cured film is on the inner side, a raw material of a base material is injected into the mold to carry out injection molding polymerization, and after the polymerization is completed, the laminate with the cured film integrated on the surface of the base material is taken out.

[0250] Among them, the first hard coating layer 1011A and the second hard coating layer 1011B can be formed in the same manner as the first resin substrate 1001 in the manufacturing process of the first resin substrate 1001 .

[0251] The materials and the coating methods of the materials used in the first hard coating layer 1011A and the second hard coating layer 1011B are preferably materials and the coating methods of the materials that are not likely to increase the unevenness of the uneven defects on the surface of the first resin substrate 1001. The materials and the coating methods of the materials used in the first hard coating layer 1011A and the second hard coating layer 1011B are more preferably materials and the coating methods of the materials that can alleviate the unevenness of the uneven defects on the surface of the first resin substrate 1001.

[0252] For example, the above-mentioned hard coating agent, alkoxysilane polycondensation curing resin, melamine resin, etc. can be used as the material.

[0253] For example, as the coating method, conventionally known coating methods such as bar coating, dip coating, reverse gravure coating, direct gravure coating, roll coating, die coating or curtain coating can be used, and dip coating, die coating or gravure coating is particularly preferred.

[0254] According to the first variant example of the first embodiment of the present invention, similarly to the basic example of the first embodiment of the present invention, the MC values ​​of the first resin substrate 1001 and the second resin substrate 1003 are less than 0.120. Therefore, similarly to the basic example of the first embodiment of the present invention, a light guide plate for image display that can display a clear image even when using a resin substrate can be provided.

[0255] Furthermore, according to the first modification of the first embodiment of the present invention, since the first hard coating layer 1011A and the second hard coating layer 1011B are stacked on the first resin substrate 1001, the surface of the first resin substrate 1001 can be prevented from being scratched.

[0256] For example, in the manufacturing process of the image display light guide plate 1014 and the display device, it is possible to prevent the deterioration of the planarity due to scratches on the surface of the first resin substrate 1001. Therefore, it is possible to reduce the defective rate of the image display light guide plate 1014 and the display device caused by handling in the manufacturing process such as conveyance.

[0257] For example, since the first hard coating layer 1011A constitutes the outermost surface of the image display light guide plate 1014 , it is possible to suppress degradation of image quality due to scratches on the outermost surface of the image display light guide plate 1014 during use.

[0258] In the description of the first modification, a case where a hard coating layer is formed on each surface in the thickness direction of the first resin substrate 1001 is described as an example. However, one of the first hard coating layer 1011A and the second hard coating layer 1011B may be omitted.

[0259] In the description of the first modification, the case where the hard coating layer is formed only on the first resin substrate 1001 is described as an example. However, at least one of the first hard coating layer 1011A and the second hard coating layer 1011B may be formed on the second resin substrate 1003 .

[0260] [Second embodiment]

[0261] <Basic example>

[0262] Next, a light guide plate for image display according to a second embodiment of the present invention will be described.

[0263] The image display light guide plate according to the second embodiment of the present invention comprises a first resin substrate, a first barrier layer and a holographic layer. The first barrier layer is preferably disposed on the surface of at least one of the first resin substrate and the holographic layer, and the first barrier layer is more preferably disposed on the holographic layer. The first resin substrate, the first barrier layer and the holographic layer are preferably disposed in order in the thickness direction.

[0264] The image display light guide plate of the second embodiment of the present invention may further include a second barrier layer and a second resin substrate. Preferably, the first barrier layer is disposed on at least one of the surface of the first resin substrate facing the holographic layer and the surface of the holographic layer facing the first resin substrate, and the second barrier layer is disposed on the surface of the second resin substrate facing the holographic layer and the surface of the holographic layer facing the second resin layer substrate. More preferably, the first barrier layer and the second barrier layer are disposed on the surface of the holographic layer facing the first resin substrate and the surface of the holographic layer facing the second resin layer substrate, respectively. The first resin substrate, the first barrier layer, the holographic layer, the second barrier layer and the second resin substrate are preferably stacked in order in the thickness direction.

[0265] In the present embodiment, the first resin substrate and the second resin substrate may be collectively referred to as “resin substrate”. Also, the first barrier layer and the second barrier layer may be collectively referred to as “barrier layer”.

[0266] One or more transparent layers may be disposed between the barrier layer and the resin substrate. One or more transparent layers may be disposed between the barrier layer and the holographic layer.

[0267] Examples of the transparent layer include a hard coat layer, an adhesive layer, and an anchor coat layer.

[0268] In the light guide plate for image display according to the second embodiment of the present invention, a glass substrate may be provided to sandwich the barrier layer and the holographic layer between the resin substrate. In this case, since the glass substrate itself has barrier properties, the glass substrate may be disposed on the surface of the holographic layer opposite to the surface facing the barrier layer.

[0269] As the resin substrate, the resin substrate in the first embodiment described above can be used appropriately.

[0270] The material used for the resin substrate is not particularly limited as long as it is a transparent material, but it preferably contains at least one resin selected from the group consisting of acrylic resins, cyclic polyolefin resins, and polycarbonate resins.

[0271] The refractive index of the barrier layer is preferably higher than the refractive index of the resin substrate, and more preferably 1.48 or more.

[0272] As the material of the barrier layer, a water vapor barrier material is preferably used.

[0273] The material of the barrier layer preferably includes an inorganic material, and more preferably includes at least one inorganic material selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon (DLC), aluminum oxide, and glass.

[0274] Furthermore, by using an auxiliary layer containing a fluorine-based material, a cycloolefin-based polymer, vinylidene chloride, or the like as a part of the barrier layer in combination with the inorganic material, the barrier layer can be made into a multilayer structure, and the water vapor barrier property can be further improved.

[0275] Furthermore, the barrier layer may be disposed on the resin film, and in this case, the resin film is more preferably disposed between the barrier layer and the resin substrate.

[0276] The hologram layer is sandwiched between the first resin substrate and the second resin substrate, or between the first resin substrate and the glass substrate.

[0277] The image display light guide plate has an incident portion into which image light is incident, and a display portion that displays an image based on the image light. The holographic layer is disposed between the incident portion and the display portion. A diffraction grating pattern is formed in the holographic layer, which is used to guide at least the image light incident from the incident portion to the display portion and emit it from the display portion. The diffraction grating pattern in the display portion transmits at least a portion of external light incident from outside the image display light guide plate.

[0278] The image light incident on the incident part is guided into the holographic layer and emitted from the display part to the outside. On the other hand, the external light also passes through the resin substrate and the display part, so that the observer of the display part can observe both the image light and the external light in the field of view.

[0279] The image display light guide plate of the second embodiment of the present invention is suitable for use in a display device using VR technology or AR technology. For example, in addition to being used for display purposes, the image display light guide plate of the second embodiment of the present invention can also be used in a combiner for a head-up display (HUD) for automobiles or a holographic optical element (HOE) represented by a reflective plate for a reflective liquid crystal display device.

[0280] A known resin material for forming a hologram is used in the hologram layer. Examples of the resin material for forming a hologram include a solvent-soluble thermosetting resin having at least one cationically polymerizable ethylene oxide ring in a structural unit, and a hologram recording material composed of an ethylenic monomer capable of free radical polymerization (Japanese Patent Application Laid-Open Nos. 8-1676, 8-1677, 8-1678, and 8-1679).

[0281] The following is based on Fig. 9 The example shown will explain the detailed structure of an example of the image display light guide plate according to the second embodiment of the present invention. Fig. 9 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to the second embodiment of the present invention.

[0282] Fig. 9 In the illustrated image display light guide plate 2006 , a first resin base material 2001 , a first barrier layer 2002 , a hologram layer 2003 , a second barrier layer 2004 , and a second resin base material 2005 are arranged in this order in the thickness direction.

[0283] The planar shape of the image display light guide plate 2006 is not particularly limited. For example, the image display light guide plate 2006 may be shaped into a shape that can be mounted in a display device to be used.

[0284] For example, the image display light guide plate 2006 may be a rectangular plate larger than the shape to be mounted on the display device. In this case, the image display light guide plate 2006 is cut into a shape that can be mounted on the display device before being mounted on the display device.

[0285] The image display light guide plate 2006 may be in the form of a flat plate, or may be in the form of a curved plate as required.

[0286] The following description will take as an example a case where the image display light guide plate 2006 is composed of a flat plate that is rectangular in plan view.

[0287] The first resin substrate 2001 is disposed at the outermost portion in the thickness direction of the image display light guide plate 2006. The first resin substrate 2001 is disposed on the surface of the image display light guide plate 2006 on the side where the display image is emitted.

[0288] The first resin substrate 2001 has the same outer shape as that of the image display light guide plate 2006 .

[0289] Image light emitted from the hologram layer 2003 and external light transmitted through a second resin substrate 2005 and the hologram layer 2003 described later are transmitted through the first resin substrate 2001 .

[0290] The thickness of the first resin substrate 2001 is not particularly limited. For example, the thickness of the first resin substrate 2001 may be 0.1 to 10 mm.

[0291] The material forming the first resin substrate 2001 is not particularly limited as long as it is a transparent resin material. As the material forming the first resin substrate 2001, in consideration of optical properties such as transparency and refractive index of light, as well as physical properties such as impact resistance, heat resistance and durability, for example, polyolefin resins such as homopolymers or copolymers of olefins such as ethylene, propylene or butene; amorphous polyolefin resins such as cyclic polyolefins; polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN); cellulose resins such as triacetyl cellulose, diacetyl cellulose and cellophane; polyamide resins such as nylon 6, nylon 66, nylon 12 and copolymer nylon; partial hydrolyzate of ethylene-vinyl acetate copolymer (EVA); VOH), polyimide resins, polyetherimide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, polycarbonate resins, polyvinyl butyral resins, polyarylate resins, fluororesins, poly(methyl)acrylic resins, polystyrene resins, polyvinyl alcohol, ethylene vinyl alcohol copolymers, polyvinyl chloride, cellulose, acetyl cellulose, polyvinylidene chloride, polyphenylene sulfide, polyurethane, phenol resins, epoxy resins, polyarylate resins, polynorbornene, styrene-isobutylene-styrene block copolymers (SIBS), allyl diglycol carbonate, and organic materials such as biodegradable resins. Among these, it is preferred to include at least one resin selected from the group consisting of poly(methyl)acrylic resins, epoxy resins, cyclic polyolefins, and polycarbonates. It should be noted that the first resin substrate 2001 can be formed by two or more materials, or it can be a laminated structure formed by laminating two or more materials.

[0292] From the perspective of transparency of the first resin substrate 2001, polycarbonate or poly(meth)acrylic resin is preferred. From the perspective of chemical resistance and process resistance such as processability of the first resin substrate 2001, poly(meth)acrylic resin, epoxy resin or cyclic polyolefin is preferred. Poly(meth)acrylic resin is more preferred because it can achieve both transparency and process resistance.

[0293] The first barrier layer 2002 is disposed between the first resin substrate 2001 and the holographic layer 2003 described later. Fig. 9 In the illustrated structure, the first barrier layer 2002 is in close contact with the surfaces of the first resin substrate 2001 and the hologram layer 2003. However, the first barrier layer 2002 does not need to be in close contact with the surfaces of both the first resin substrate 2001 and the hologram layer 2003, but is preferably disposed at least on the hologram layer 2003. The first barrier layer 2002 prevents the gas that penetrates from the outside of the image display light guide plate 2006 and the first resin substrate 2001 from penetrating into the hologram layer 2003.

[0294] The first barrier layer 2002 preferably has a lower oxygen permeability and a lower water vapor permeability, for example. In particular, the first barrier layer 2002 is more preferably made of a material having excellent water vapor barrier properties (low water vapor permeability) because degradation of the hologram layer can be suppressed.

[0295] For example, the oxygen permeability of the first barrier layer 2002 may be 1 cm 3 / m 2 · Below the day.

[0296] For example, the water vapor permeability of the first barrier layer 2002 may be 1 g / m 2 The water vapor permeability of the first barrier layer 2002 is more preferably 0.5 g / m 2 · Below the day.

[0297] The material of the first barrier layer 2002 is not particularly limited as long as it has the property of blocking the gas that causes the degradation of the hologram layer 2003, but it is preferably made of an inorganic material because it has excellent gas barrier properties and tends to have excellent clarity of displayed images.

[0298] In this case, the inorganic material used in the first barrier layer 2002 may have a higher refractive index than the first resin substrate 2001. For example, the refractive index of the first barrier layer 2002 may be 1.48 to 3.00. When the first barrier layer 2002 has a high refractive index, light that passes through the first resin substrate 2001 via the first barrier layer 2002 enters the optically sparse first resin substrate 2001 from the optically dense first barrier layer 2002, so the emission angle of light from the first barrier layer 2002 toward the first resin substrate 2001 increases according to the refractive index difference between the first barrier layer 2002 and the first resin substrate 2001. As a result, the FOV (Field Of View) in the image display light guide plate 2006 can be expanded.

[0299] Examples of the material of the first barrier layer 2002 include silicon oxide, silicon oxynitride, DLC, aluminum oxide, and glass.

[0300] Regarding the material of the first blocking layer 2002, as described above, it can be an oxide such as zinc oxide, antimony oxide, indium oxide, cerium oxide, calcium oxide, cadmium oxide, silver oxide, gold oxide, chromium oxide, silicon oxide, cobalt oxide, zirconium oxide, tin oxide, titanium oxide, iron oxide, copper oxide, nickel oxide, platinum oxide, palladium oxide, bismuth oxide, magnesium oxide, manganese oxide, molybdenum oxide, vanadium oxide or barium oxide.

[0301] When the first barrier layer 2002 is formed of silicon oxide, the thickness thereof may be 10 to 300 nm. If the thickness is less than 10 nm, the moisture resistance may be insufficient. If the thickness is greater than 300 nm, the silicon oxide film may be prone to cracking and may be easily peeled off from the film-forming surface.

[0302] A particularly preferred layer thickness is 20 to 200 nm.

[0303] The method for forming the first barrier layer 2002 from the silicon oxide is not particularly limited. For example, the first barrier layer 2002 can be formed by any conventionally known method such as vacuum evaporation, sputtering, ion plating, or plasma CVD. When the first barrier layer 2002 is formed from the silicon oxide, in order to improve the adhesion between the film-forming surface and the silicon oxide, a surface treatment such as applying a corona discharge treatment or a low-temperature plasma treatment to the film-forming surface, coating a silane coupling agent on the film-forming surface, or coating a mixture of a saturated polyester and an isocyanate on the film-forming surface can be performed.

[0304] For example, when a silicon oxide thin film is formed by vacuum evaporation, silicon, silicon monoxide, silicon dioxide, or a mixture thereof is used as an evaporation substance, and the vacuum evaporation temperature is 1.0×10 -3 ~1.0×10 -5It is heated and evaporated by electron beam, resistance heating or high frequency heating under a vacuum of Torr.

[0305] Alternatively, a reactive vapor deposition method may be employed while supplying oxygen gas.

[0306] The silicon oxide forming the first barrier layer 2002 may contain calcium, magnesium, or oxides thereof as impurities in an amount of 10 mass % or less.

[0307] When the first barrier layer 2002 is formed of silicon oxynitride, the same structure as the first barrier layer 2002 having silicon oxide as a main component is used except that the silicon oxide is replaced with the silicon oxynitride.

[0308] DLC is generally an amorphous carbon material formed of a ternary structure of a diamond-like structure, a graphite-like structure, and a polyethylene-like polymer structure containing hydrogen atoms in the structure. In the production of the above-mentioned DLC, when hydrocarbons such as ethylene, acetylene or benzene are used as a carbon source, a substantially ternary structure containing hydrogen is generally formed.

[0309] The DLC is excellent in hardness, lubricity, wear resistance, chemical stability, heat resistance and surface smoothness. Since the DLC forms the dense polymer structure, it is also excellent in gas barrier properties and water vapor barrier properties.

[0310] The method for forming the first barrier layer 2002 using the DLC is not particularly limited. As the DLC coating method, for example, a known appropriate coating method such as a plasma CVD method or a physical vapor deposition method such as an ion plating method or an ion beam sputtering method can be used.

[0311] When the first barrier layer 2002 is formed of aluminum oxide, the first barrier layer 2002 may be formed of, for example, only Al2O3, or may be formed by mixing two or more selected from the group consisting of Al, AlO, and Al2O3. The atomic ratio of Al:O in the aluminum oxide layer varies depending on the conditions for producing the aluminum oxide layer. The aluminum oxide layer that can be used as the first barrier layer 2002 may contain a trace amount (up to 3% relative to the total components) of other components within a range that does not impair the barrier performance.

[0312] The thickness of the aluminum oxide layer can be set according to the requirements of the barrier performance. For example, the thickness of the aluminum oxide layer can be 5 to 800 nm.

[0313] The method for forming the first barrier layer 2002 from aluminum oxide is not particularly limited. For example, the first barrier layer 2002 may be formed by PVD (physical vapor deposition) such as vacuum deposition, sputtering, or ion plating, or CVD (chemical vapor deposition).

[0314] For example, in the vacuum evaporation method, Al, Al2O3, etc. can be used as the evaporation source material, and resistance heating, high-frequency induction heating, electron beam heating, etc. can be used as the heating method of the evaporation source. In the vacuum evaporation method, oxygen, nitrogen, or water vapor can be introduced as a reactive gas, or reactive evaporation using means such as ozone addition or ion assistance can be used. In addition, a bias voltage can be applied to the film-forming surface, the temperature of the film-forming surface can be increased, or it can be cooled. The same is true for other film-forming methods such as PVD and CVD other than vacuum evaporation methods such as sputtering.

[0315] When the first barrier layer 2002 is formed of glass, examples of the material of the first barrier layer 2002 include borosilicate glass, alkali-free glass, low-alkali glass, soda-lime glass, sol-gel glass, or glass obtained by subjecting these glasses to heat treatment or surface treatment. As the material of the first barrier layer 2002, alkali-free glass is particularly preferred from the viewpoint of avoiding coloration due to impurities.

[0316] When the first barrier layer 2002 is formed of glass, the thickness thereof may be 10 to 200 μm. When the thickness is 10 μm or more, the mechanical strength and gas barrier properties tend to be excellent. The thickness is preferably 10 μm or more, and more preferably 30 μm or more. In addition, when the thickness is 200 μm or less, the optical properties of the light guide plate such as light transmittance tend to be excellent. The thickness is preferably 200 μm or less, more preferably 100 μm or less, further preferably 75 μm or less, and particularly preferably 50 μm or less.

[0317] The method for forming the first barrier layer 2002 from glass is not particularly limited. As a method for forming the first barrier layer 2002 from glass, for example, a slit-down method, a fusion method, or a float method can be used. In addition, the glass used can be commercially available glass as it is, or commercially available glass can be ground into a desired thickness for use. Examples of the commercially available glass include "EAGLE2000" manufactured by Corning, "AN100" manufactured by Asahi Glass, "OA10G" manufactured by Nippon Electric Glass, and "D263" manufactured by Schott.

[0318] In addition, as a part of the first barrier layer 2002, an auxiliary layer containing a fluorine-based material, a cycloolefin-based polymer or vinylidene chloride can be introduced. By making the first barrier layer 2002 into a multilayer structure with the above-mentioned inorganic material layer, the water vapor barrier property can be further improved.

[0319] As the fluorine-based material, for example, PCTFE (polychlorotrifluoroethylene) can be used. In addition, as the cycloolefin-based polymer, a cycloolefin polymer or a cycloolefin copolymer can be used.

[0320] The thickness of the auxiliary layer may be set according to the requirements of water vapor barrier performance. For example, when a fluorine-based material is used, the thickness may be 0.1 to 100 μm.

[0321] The hologram layer 2003 is laminated on the surface of the first barrier layer 2002. The structure of the hologram layer 2003 is not particularly limited. The hologram layer 2003 has a suitable diffraction grating corresponding to the function required of the image display light guide plate 2006 formed therein.

[0322] The second barrier layer 2004 is formed on the surface of the hologram layer 2003 opposite to the surface of the hologram layer 2003 on which the first barrier layer 2002 is formed.

[0323] The second barrier layer 2004 has the same structure as that exemplified in the description of the first barrier layer 2002. However, the second barrier layer 2004 may be different from the first barrier layer 2002 in terms of material, thickness, etc.

[0324] The second resin substrate 2005 is laminated on the surface of the second barrier layer 2004 on the opposite side to the hologram layer 2003. As the second resin substrate 2005, the same structure as that exemplified in the description of the first resin substrate 2001 is used. However, the thickness, material, etc. of the second resin substrate 2005 may be different from those of the first resin substrate 2001. In particular, since the second resin substrate 2005 is arranged on the surface of the external light incident side located opposite to the side from which the displayed image is emitted in the image display light guide plate 2006, a material having a higher surface hardness than that of the first resin substrate 2001 can be used.

[0325] Such an image display light guide plate 2006 can be manufactured, for example, as follows.

[0326] A first resin substrate 2001 and a second resin substrate 2005 are prepared, and a first barrier layer 2002 and a second barrier layer 2004 are respectively formed on the surfaces of the first resin substrate 2001 and the second resin substrate 2005. As a method for manufacturing the first barrier layer 2002 and the second barrier layer 2004, an appropriate manufacturing method is selected according to the materials of the first barrier layer 2002 and the second barrier layer 2004.

[0327] For example, a photosensitive material for forming a hologram is applied to the surface of the first barrier layer 2002 in the first resin substrate 2001 on which the first barrier layer 2002 is formed. In this case, a transparent sealing layer having the same thickness as the hologram layer 2003 may be provided on the periphery of the first barrier layer 2002. In this case, the photosensitive material is applied to the concave portion surrounded by the sealing layer. After the hologram layer 2003 is formed, the sealing layer seals the periphery of the hologram layer 2003. It should be noted that the sealing layer may use the material having excellent gas barrier properties used in the first barrier layer 2002, thereby improving the durability of the hologram layer 2003.

[0328] Thereafter, the second resin substrate 2005 on which the second barrier layer 2004 is formed is placed on the photosensitive material in a state where the second barrier layer 2004 faces the photosensitive material.

[0329] However, the above manufacturing sequence is an example, and for example, after a photosensitive material is applied to the second resin substrate 2005 on which the second barrier layer 2004 is formed, the first resin substrate 2001 on which the first barrier layer 2002 is formed may be placed on the photosensitive material.

[0330] Thereafter, a laminate including the first resin substrate 2001 , the first barrier layer 2002 , the photosensitive material, the second barrier layer 2004 , and the second resin substrate 2005 is bonded together by reduced pressure pressing.

[0331] Thereafter, interference fringes corresponding to the diffraction pattern are formed in the photosensitive material of the laminate, and a diffraction grating is formed in the photosensitive material.

[0332] In this way, the image display light guide plate 2006 is manufactured.

[0333] According to the image display light guide plate 2006, the first barrier layer 2002 and the second barrier layer 2004 are arranged between the first resin substrate 2001 and the hologram layer 2003, and between the second resin substrate 2005 and the hologram layer 2003, respectively.

[0334] The gas barrier properties of the first resin substrate 2001 and the second resin substrate 2005 vary in degree depending on the type of resin material, but are significantly lower than glass. Therefore, the first resin substrate 2001 and the second resin substrate 2005 have higher hygroscopicity and water vapor permeability than glass.

[0335] As a result, the gas outside the image display light guide plate 2006 permeates the first resin substrate 2001 and the second resin substrate 2005 to a certain extent or accumulates inside. In particular, water easily accumulates in the first resin substrate 2001 and the second resin substrate 2005.

[0336] However, even if gas and water that penetrate into the first resin substrate 2001 and the second resin substrate 2005 from the outside diffuses in the image display light guide plate 2006, they are blocked by the first barrier layer 2002 and the second barrier layer 2004. Thus, the penetration of gas and water vapor into the hologram layer 2003 can be suppressed.

[0337] For example, by suppressing the penetration of moisture into the hologram layer 2003, the degradation of the hologram layer 2003 can be prevented.

[0338] Furthermore, since the image display light guide plate 2006 has the above-mentioned layer structure, the hologram layer 2003 does not contact the first resin substrate 2001 and the second resin substrate 2005. Therefore, even if the image display light guide plate 2006 is placed in a high temperature environment, the hologram layer 2003 can be prevented from corroding the first resin substrate 2001 and the second resin substrate 2005.

[0339] In particular, when the refractive indexes of the first barrier layer 2002 and the second barrier layer 2004 are higher than the refractive indexes of the first resin substrate 2001 and the second resin substrate 2005, as described above, the emission angle of light from the first barrier layer 2002 toward the first resin substrate 2001 increases. Similarly, the emission angle of light incident from the second resin substrate 2005 to the second barrier layer 2004 is narrow. Therefore, light incident from the outside on the second resin substrate 2005 side and passing through the image display light guide plate 2006 can be incident in a wider angle range than in the case where the second barrier layer 2004 is not provided, and can be emitted in a wider angle range than in the case where the first barrier layer 2002 is not provided. As a result, the field of view of external light can be further expanded, and the FOV on the display side can also be expanded.

[0340] As described above, the emission angle of the image light from the hologram layer 2003 increases from the first barrier layer 2002 toward the first resin substrate 2001 , and as a result, the FOV of the display screen can be expanded compared to the case where the first barrier layer 2002 is not provided.

[0341] In particular, in the present embodiment, by stacking the first blocking layer 2002 and the second blocking layer 2004 on the hologram layer 2003, the diffusion position of the external light and the image light is close to the diffraction position of the hologram layer 2003 constituting the display screen. Therefore, compared with the case where the first blocking layer 2002 and the second blocking layer 2004 are provided at a position away from the hologram layer 2003, a clearer image can be observed from a wider range of angles.

[0342] Here, an example of a method for measuring the brightness value and FOV in the image display light guide plate 2006 is briefly described.

[0343] Fig.10It is a schematic front view illustrating the method of measuring the brightness value and FOV.

[0344] like Fig.10 As shown, in order to measure the brightness value and FOV of the image display light guide plate 2006, a display device 2010 is manufactured using the image display light guide plate 2006.

[0345] The display device 2010 includes an image light projection unit 2013 and an incident optical system 2012 in addition to the image display light guide plate 2006 .

[0346] The image light projection unit 2013 projects image light to be displayed on the image display light guide plate 2006 based on an image signal sent from a controller (not shown).

[0347] The incident optical system 2012 includes, for example, a prism, etc. The incident optical system 2012 allows the image light emitted from the image light projection unit 2013 to enter an incident portion 2006a provided on the surface of the image display light guide plate 2006. For example, the incident portion 2006a is provided on the surface on the first resin substrate 2001 side.

[0348] The image light incident on the incident portion 2006a reaches the display diffraction grating portion 2003c of the hologram layer 2003 via the waveguide diffraction grating portion 2003b formed on the hologram layer 2003. The image light is diffracted at the position corresponding to each display pixel in the display diffraction grating portion 2003c. The diffracted light is emitted to the outside from the display portion 2006d on the surface of the image display light guide plate 2006. Fig.10 In the illustrated example, the display portion 2006 d is formed on the surface on the first resin base material 2001 side at a position separated from the incident portion 2006 a .

[0349] The brightness value and FOV of the image display light guide plate 2006 are measured by placing the display device 2010 on the measuring device 2015 .

[0350] The measuring device 2015 includes a holding table (not shown), a luminance meter 2014, and a goniometer table (not shown).

[0351] The holding stage holds the display device 2010. The luminance meter 2014 measures the luminance value of the received light. The goniometer stage supports the luminance meter 2014 so as to be swingable on a circle centered on the rotation center thereof.

[0352] The distance d between the luminance meter 2014 and the display surface 2003a is a distance corresponding to the eye position of the user when the display device 2010 is mounted. For example, when the display device 2010 is a head mounted display, the distance d is 15 mm.

[0353] The brightness value of the image display light guide plate 2006 is obtained by placing the brightness meter 2014 at a swing angle of 0° (see Fig.10 The display device 2010 uses the above-mentioned holding table to arrange the center of the display surface 2003a at a position opposite to the luminance meter 2014 on the measurement optical axis of the luminance meter 2014.

[0354] The brightness value is the brightness measured by the brightness meter 2014 when a white image with maximum brightness is displayed on the display device 2010 .

[0355] In the measurement of the FOV of the image display light guide plate 2006, the swing angle θ is changed while a white image with maximum brightness is displayed on the display device 2010. B The brightness is measured. The brightness corresponding to the white image not being observed is used as a threshold value, and the angle range in which the brightness above the threshold value can be obtained is obtained. When the brightness above the threshold value is obtained in the range of -θ1 to +θ2, the FOV is θ1+θ2.

[0356] The FOV of the image display light guide plate 2006 is preferably 24 to 160°, more preferably 35 to 160°. In addition, as the FOV increases, the angle at which the image can be observed increases, the amount of information in the image also increases, and the range of applicable uses also expands. On the other hand, if the FOV is less than the upper limit, the amount of light taken out relative to a certain area tends to increase, and the image becomes brighter, which is preferred.

[0357] For example, the closer the distance between the first barrier layer 2002 and the second barrier layer 2004 and the holographic layer 2003 is, the higher the FOV can be increased by about 10° or more. The distance is preferably 1000 nm or less, more preferably 500 nm or less, and most preferably 100 nm or less.

[0358] As described above, according to the present embodiment, it is possible to provide a light guide plate for image display that can suppress degradation of the hologram layer even when a resin substrate is used.

[0359] <First Modification>

[0360] A first modified example of the second embodiment of the present invention will be described.

[0361] Fig.11 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a first modified example of the second embodiment of the present invention.

[0362] like Fig.11As shown, the image display light guide plate 2016 of the first variant of the second embodiment of the present invention includes a first barrier film 2022 and a second barrier film 2024 instead of the first barrier layer 2002 and the second barrier layer 2004 of the image display light guide plate 2006 of the basic example of the second embodiment of the present invention.

[0363] The following description will focus on the differences from the above-described embodiment.

[0364] The first barrier film 2022 includes a barrier layer 2022A and a resin film 2022B.

[0365] The barrier layer 2022A is configured similarly to the first barrier layer 2002 in the above-described embodiment.

[0366] The resin film 2022B is a base on which the barrier layer 2022A is formed. The material of the resin film 2022B is not particularly limited as long as it is a transparent resin film on which the barrier layer 2022A can be formed.

[0367] For example, as the material of the resin film 2022B, resins such as polypropylene, ABS, amorphous polyester resin, polyimide, polyamide, polyethersulfone (PES), polycarbonate (PC), polynorbornene as a cyclic polyolefin copolymer, cyclic polyolefin resin, polycyclohexene, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), fluororesin, polyarylate (PAR), polyetherketone (PEK) or polyetheretherketone (PEEK) can be used.

[0368] For example, when considering the thermal expansion coefficient, the humidity expansion coefficient, and the glass transition temperature, as materials more suitable for the resin film 2022B, polyamide, polyacetal, polybutylene terephthalate, polyethylene terephthalate, or syndiotactic polystyrene, etc., which are thermoplastic resins, and polyphenylene sulfide, polyetheretherketone, liquid crystal polymer, fluororesin, or polyethernitrile, etc., which are thermosetting resins, can be cited as crystalline resins. For example, polycarbonate or modified polyphenylene ether, etc., which are thermoplastic resins, and polysulfone, polyethersulfone, polyarylate, polyamideimide, polyetherimide, or thermoplastic polyimide, etc., which are thermosetting resins, can be cited as amorphous resins. Among them, polycarbonate has low water absorption, so the humidity expansion coefficient of the first barrier film 2022 formed using it is low, and it is particularly preferred.

[0369] The thickness of the resin film 2022B is not particularly limited, but it is more preferable that the resin film 2022B is thinner than the first resin substrate 2001. For example, the thickness of the resin film 2022B may be 1 to 200 μm.

[0370] As the resin film 2022B, it is more preferable to use a material with high surface smoothness. In this case, the surface smoothness of the barrier layer 2022A is improved, and the thickness of the barrier layer 2022A is easy to be uniform. As for the surface smoothness of the resin film 2022B, it is more preferable to be 2 nm or less in terms of arithmetic mean roughness Ra.

[0371] The surface of the resin film 2022B may be subjected to various surface modification treatments in order to improve the adhesion with the barrier layer 2022A and the adhesion with the first adhesive layer 2026 described later. For example, the surface of the resin film 2022B may be subjected to corona discharge treatment, flame treatment, oxidation treatment, plasma treatment, or lamination of a primer layer.

[0372] Such a first barrier film 2022 is manufactured by forming a resin film 2022B on a barrier layer 2022A. Such a first barrier film 2022 is manufactured by forming a barrier layer 2022A on a resin film 2022B.

[0373] As the film forming method of the barrier layer 2022A, for example, physical vapor deposition (PVD), chemical vapor deposition (CVD), plating, coating, sol-gel, etc. can be cited. In particular, in CVD, the formation efficiency of the barrier layer 2022A is excellent. In CVD, since the heat applied to the resin film 2022B during film formation is less than that in the physical vapor deposition method, the degradation of the resin film 2022B caused by heating can be reduced. Among the CVD methods, the plasma CVD method is more preferred. In the plasma CVD method, after the raw material gas is introduced into the film forming chamber, the high frequency is activated to cause discharge, forming a plasma state, thereby promoting chemical reactions on the surface of the resin film 2022B. Therefore, the temperature in the film forming process is a low temperature of about -10°C to 200°C, and in particular, film formation can be performed even at below 30°C. As a result, it is not easy to apply thermal damage to the resin film 2022B.

[0374] The barrier layer 2022A in the first barrier film 2022 is arranged on the surface of the hologram layer 2003 .

[0375] The resin film 2022B in the first barrier film 2022 is fixed to the surface of the first resin base material 2001 via the first adhesive layer 2026 .

[0376] The material of the first adhesive layer 2026 is not particularly limited as long as it has good adhesion to the resin film 2022B and the first resin base material 2001 .

[0377] For example, preferred materials for the first adhesive layer 2026 include polyester resins, acrylic resins, urethane resins, melamine resins, epoxy resins, and the like.

[0378] The second barrier film 2024 includes a barrier layer 2024A similar to the barrier layer 2022A and a resin film 2024B similar to the resin film 2022B.

[0379] However, the material, thickness, etc. of the barrier layer 2024A may be the same as or different from those of the barrier layer 2022A. The material, thickness, etc. of the resin film 2024B may be the same as or different from those of the resin film 2022B.

[0380] The second barrier film 2024 is fixed to the surface of the second resin base material 2005 via a second adhesive layer 2027 having the same structure as the first adhesive layer 2026 .

[0381] In order to manufacture such a light guide plate 2016 for image display, for example, a first barrier film 2022 and a second barrier film 2024 are prepared in advance, and the first barrier film 2022 and the second barrier film 2024 are bonded to the respective surfaces of the first resin substrate 2001 and the second resin substrate 2005 via a first adhesive layer 2026 and a second adhesive layer 2027, thereby forming a first intermediate laminate P1 and a second intermediate laminate P2.

[0382] Thereafter, the hologram layer 2003 is formed in the same manner as in the basic example of the second embodiment of the present invention, except that the first intermediate laminate P1 and the second intermediate laminate P2 are used instead of the first resin substrate 2001 and the second resin substrate 2005 of the basic example of the second embodiment of the present invention, respectively. Thus, the image display light guide plate 2016 is manufactured.

[0383] According to the image display light guide plate 2016 of the first modified example of the second embodiment of the present invention, the first resin substrate 2001, the barrier layer 2022A, and the hologram layer 2003 are arranged in this order, and the second resin substrate 2005, the barrier layer 2024A, and the hologram layer 2003 are arranged in this order. Therefore, as in the embodiment, the penetration of moisture into the hologram layer 2003 can be suppressed, thereby preventing the degradation of the hologram layer 2003. In addition, since the hologram layer 2003 is not in contact with the first resin substrate 2001 and the second resin substrate 2005, the first resin substrate 2001 and the second resin substrate 2005 can be prevented from being corroded by the material of the hologram layer 2003.

[0384] Therefore, according to the image display light guide plate 2016, a clear image can be displayed even when a resin substrate is used.

[0385] Furthermore, if the refractive index of the barrier layers 2022A and 2024A is made higher than the refractive index of the first resin substrate 2001 and the second resin substrate 2005, the FOV of the image display light guide plate 2016 can be increased, so that a clear image can be observed from a wide range of angles.

[0386] In particular, according to the first modification of the second embodiment of the present invention, in the manufacturing process of the image display light guide plate 2016, the barrier layers 2022A and 2024A are arranged on the first resin substrate 2001 and the second resin substrate 2005 by bonding the first barrier film 2022 and the second barrier film 2024 on the first resin substrate 2001 and the second resin substrate 2005. Therefore, even in the case where the barrier layers 2022A and 2024A cannot be directly formed due to the type, shape, size, etc. of the materials of the first resin substrate 2001 and the second resin substrate 2005, the barrier layers 2022A and 2024A can be easily arranged.

[0387] As described above, according to the first modification of the second embodiment of the present invention, it is possible to provide a light guide plate for image display that can suppress degradation of the hologram layer even when a resin substrate is used.

[0388] It should be noted that, in the basic example and the first variant example of the second embodiment described above, the case where barrier layers are arranged on the surface and back side of the holographic layer is described as an example, but the barrier layer can be arranged between the resin substrate and the holographic layer for the purpose of blocking moisture that penetrates through the resin substrate and preventing the holographic layer from contacting the resin substrate.

[0389] However, in this case, if the hygroscopicity of the transparent layer sandwiched between the barrier layer and the holographic layer is high, moisture may penetrate through the side of the transparent layer. Therefore, the transparent layer between the barrier layer and the holographic layer is preferably formed of a material with low hygroscopicity. In the case where the transparent layer between the barrier layer and the holographic layer is hygroscopic, it is more preferable that the thickness of the transparent layer is thin. In this case, the exposed area of ​​the side that becomes the penetration port of moisture is reduced, so the water content of the absorbed moisture can be reduced.

[0390] [Third Embodiment]

[0391] When the image display light guide plate of the present invention is used, for example, in an eyeglass-type display, a hard coating film may be installed on the surface of the resin substrate on the opposite side to the side where the holographic layer is located in a manner that allows it to be peeled off from the substrate in order to prevent a reduction in optical properties due to scratches on its surface.

[0392] <Basic example>

[0393] Next, a third embodiment of the light guide plate for image display according to the present invention will be described.

[0394] Fig.14 2 shows a layer structure of a light guide plate for image display (hereinafter simply referred to as a “light guide plate”) 3001 according to a third embodiment of the present invention.

[0395] like Fig.14As shown, the light guide plate 3001 includes a hologram layer 3010 , two substrates of a first substrate 3021 and a second substrate 3022 sandwiching the hologram layer 3010 in the thickness direction, and a hard coat film 3030 provided on the first substrate 3021 .

[0396] The first substrate 3021 and the second substrate 3022 are sheet-shaped resin substrates with light transmittance. The first substrate 3021 and the second substrate 3022 can be made of the same material as the resin substrate used in the first and second embodiments. From the perspective of transparency, acrylic is suitable. The thickness of the first substrate 3021 and the second substrate 3022 can be, for example, about 1 mm.

[0397] As the hologram layer 3010, a known structure can be appropriately selected and used, similarly to the first and second embodiments. The optical structure such as the diffraction grating can be appropriately determined in consideration of the wavelength of the light to be guided.

[0398] The hard coating film 3030 includes a film substrate 3031, an adhesive layer 3032, a hard coating layer 3033, and a release layer 3034. The adhesive layer 3032 is provided on a first surface 3031a of the film substrate 3031. The hard coating layer 3033 is provided on a second surface 3031b on the film substrate 3031 opposite to the first surface 3031a. The release layer 3034 is provided on the hard coating layer 3033.

[0399] The hard coating film 3030 is attached to the first substrate 3021 by bonding the adhesive layer 3032 to the first substrate 3021 so as to be removable from the first substrate 3021 .

[0400] Each part of the hard coating film 3030 will be described in detail below.

[0401] (Film substrate 3031)

[0402] As the film substrate 3031, a film or sheet formed of various organic polymers can be used. For example, the substrate commonly used in optical components such as displays can be cited. Considering the optical properties such as transparency and refractive index of light, as well as various properties such as impact resistance, heat resistance, and durability, the following organic polymers can be used to form a film or sheet: polyethylene, polypropylene and other polyolefin systems, cyclic polyolefin systems, polyethylene terephthalate, polyethylene naphthalate and other polyester systems, triacetyl cellulose, diacetyl cellulose, cellophane and other cellulose systems, 6-nylon, 6,6-nylon and other polyamide systems, polymethyl methacrylate and other acrylic systems, polystyrene, polyvinyl chloride, polyimide, polyvinyl alcohol, polycarbonate, ethylene vinyl alcohol, etc. It is particularly preferred to use polyethylene terephthalate (PET), polycarbonate (PC), polymethyl methacrylate (PMMA) as the material.

[0403] In addition, a film substrate 3031 may be formed by adding known additives such as ultraviolet absorbers, infrared absorbers, plasticizers, lubricants, colorants, antioxidants, flame retardants, etc. to these organic polymers to add functions. In addition, the film substrate 3031 may be formed of one or a mixture of two or more selected from the above-mentioned organic polymers or a polymer, or may be formed by laminating two or more layers.

[0404] The film base material 3031 preferably has a small birefringence and good transparency. The thickness of the first substrate 3021 and the second substrate 3022 is preferably in the range of 5 to 200 μm.

[0405] (Adhesive layer 3032)

[0406] The adhesive layer 3032 bonds the film base material 3031 to the first substrate 3021 so that the film base material 3031 can be peeled off with a small force. The adhesive layer 3032 is bonded to the surface of the first substrate 3021 opposite to the surface facing the hologram layer 3010.

[0407] The adhesive layer 3032 can be formed of adhesives such as rubber adhesives, polyester adhesives, epoxy adhesives, acrylic adhesives, silicone adhesives, urethane adhesives, vinyl alkyl ether adhesives, polyvinyl alcohol adhesives, polyacrylamide adhesives, cellulose adhesives, etc. Among these, ultraviolet curing or heat curing acrylic adhesives are preferred from the perspective of optical properties such as transparency.

[0408] Examples of acrylic adhesives include adhesives formed from an adhesive composition (hereinafter referred to as the "present adhesive composition") using a (meth)acrylate polymer (hereinafter referred to as "acrylate (co)polymer" including copolymers) as a base resin.

[0409] The acrylate (co)polymer as the base resin can be prepared by appropriately selecting the type, composition ratio, and polymerization conditions of the acrylic acid monomer or methacrylic acid monomer used for polymerization, thereby appropriately adjusting the physical properties such as the glass transition temperature (Tg) and molecular weight.

[0410] Examples of acrylic acid monomers or methacrylic acid monomers used to polymerize acrylic acid ester (co)polymers include 2-ethylhexyl acrylate, n-octyl acrylate, isooctyl acrylate, n-butyl acrylate, ethyl acrylate, methyl methacrylate, methyl acrylate, etc. In addition, acrylic acid monomers having a hydrophilic group or an organic functional group, such as hydroxyethyl acrylate, acrylic acid, glycidyl acrylate, acrylamide, acrylonitrile, methacrylonitrile, fluoroacrylate, silicone acrylate, etc., can be copolymerized with the above acrylic acid monomers. Among them, various vinyl monomers such as vinyl acetate, alkyl vinyl ether, and hydroxyalkyl vinyl ether can also be suitably used for polymerization.

[0411] As the polymerization treatment using these monomers, known polymerization methods such as solution polymerization, emulsion polymerization, bulk polymerization, and suspension polymerization can be adopted. In this case, an acrylate copolymer can be obtained by using a polymerization initiator such as a thermal polymerization initiator or a photopolymerization initiator according to the polymerization method.

[0412] The thickness of the adhesive layer 3032 is preferably in the range of 1 to 50 μm, and more preferably in the range of 1 to 30 μm.

[0413] As a method for forming an adhesive layer on the film substrate 3031, a conventionally known coating method such as reverse gravure coating, direct gravure printing, roll coating, die coating, rod coating, curtain coating, etc. can be used. Regarding the coating method, there is a recorded example in "Coating Method (Coating Method)" (Maki Shoten, Harazaki Yuji, published in 1979).

[0414] The method for drying the adhesive is not particularly limited, and it is usually dried at 30 to 160°C. In addition, as a method for curing the adhesive, a known method can be appropriately selected according to the composition of the above-mentioned adhesive. For example, if the above-mentioned adhesive is an active energy ray-curable material, it can be cured by irradiating it with active energy rays (visible light, ultraviolet rays, X-rays, gamma rays). At this time, the irradiation amount of the active energy ray can be appropriately adjusted according to the characteristics of the adhesive, and it is usually preferably 10 to 10000 mJ / m 2 amount of irradiation.

[0415] From the viewpoint of easy peeling of the hard coat film, the peel strength of the adhesive layer 3032 is preferably 0.01 to 50 N / 20 mm width when peeling in a 180-degree direction is measured (peeling speed 50 mm / min).

[0416] (Hard coating 3033)

[0417] The hard coating layer 3033 has a hardness sufficient to prevent scratches caused by contact with other structures, etc. Such hardness is generally H or higher when expressed in terms of pencil hardness (load 750 g) specified in JIS K 5600-5-4:1999. Therefore, the pencil hardness of the hard coating layer is preferably H or higher, more preferably 2H or higher.

[0418] The hard coat layer 3033 can be formed of a cured product formed using various hard coat agents. For example, the hard coat layer 3033 can be formed using a hard coat agent containing an active energy ray-curable composition or a thermosetting composition.

[0419] The hard coating agent may be an organic-inorganic hybrid material.

[0420] A polymerizable monomer or polymerizable oligomer that forms a cured product by irradiation with active energy rays can also be used as a material for the hard coat layer 3033. As the above-mentioned polymerizable monomer, for example, a (meth)acrylate monomer having a free radical polymerizable unsaturated group in the molecule can be cited. As the above-mentioned polymerizable oligomer, a (meth)acrylate oligomer having a free radical polymerizable unsaturated group in the molecule can be cited.

[0421] Examples of the (meth)acrylate monomer having a free radical polymerizable unsaturated group in the molecule include at least one monomer selected from the group consisting of urethane (meth)acrylate, polyester (meth)acrylate, epoxy (meth)acrylate, melamine (meth)acrylate, polyfluoroalkyl (meth)acrylate and silicone (meth)acrylate.

[0422] As the above-mentioned (meth) acrylate oligomer having a free radical polymerizable unsaturated group in the molecule, for example, an oligomer comprising a structural unit of at least one monomer selected from the group consisting of carbamate (meth) acrylate, polyester (meth) acrylate, epoxy (meth) acrylate, melamine (meth) acrylate, polyfluoroalkyl (meth) acrylate and silicone (meth) acrylate can be cited. The above-mentioned polymerizable monomer or the above-mentioned polymerizable oligomer can also be used in combination of two or more. Among these, for reasons such as high surface hardness, preferably a monomer or oligomer of carbamate (meth) acrylate.

[0423] Examples of the urethane (meth)acrylate include urethane (meth)acrylates obtained by reacting a polyisocyanate compound with a (meth)acrylate compound having one hydroxyl group in its molecular structure, and urethane (meth)acrylates obtained by reacting a polyisocyanate compound with a (meth)acrylate compound having one hydroxyl group in its molecular structure and a polyol compound.

[0424] The hard coating layer 3033 may include a cured product of a multifunctional (meth)acrylate.

[0425] Examples of the polyfunctional (meth)acrylate include trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, tripentaerythritol 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and tripentaerythritol 1,6-hexanediol di(meth)acrylate. Tetraol octa(meth)acrylate, pentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerol tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate or di(trimethylolpropane) tetra(meth)acrylate, or those modified with PO, EO or caprolactone.

[0426] Among these, tri- to hexa-functional polyfunctional (meth)acrylates are preferred because they can appropriately satisfy the surface hardness. Specific examples thereof include pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPPA), trimethylolpropane tri(meth)acrylate, tripentaerythritol octa(meth)acrylate, and tetrapentaerythritol deca(meth)acrylate.

[0427] In the formation of the hard coating layer 3033, additives such as cross-linking agents, polymerization initiators, lubricants, plasticizers, organic particles, inorganic particles, antifouling agents, antioxidants or catalysts, or additives such as silicone or fluorine for preventing dirt and adhesion can be added to the hard coating agent within a range that does not hinder the physical properties.

[0428] In addition, the hard coating agent may contain a solvent as required. Examples of the solvent include alcohols (methanol, ethanol, propanol, isopropanol, n-butanol, sec-butanol, tert-butanol, benzyl alcohol, PGME, ethylene glycol, diacetone alcohol); ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, heptanone, diisobutyl ketone, diethyl ketone, diacetone alcohol); esters (methyl acetate, ethyl acetate, butyl acetate, n-propyl acetate, isopropyl acetate, methyl formate, PGMEA); aliphatic hydrocarbons (hexane, cyclohexane); halogenated hydrocarbons (dichloromethane, chloroform, carbon tetrachloride); aromatic hydrocarbons (benzene, toluene, xylene); amides (dimethylformamide, dimethylacetamide, N-methylpyrrolidone); ethers (diethyl ether, dioxane, tetrahydrofuran); ether alcohols (1-methoxy-2-propanol); carbonates (dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate), and the like. These solvents may be used alone or in combination of two or more.

[0429] The thickness of the hard coating layer 3033 is preferably 1 μm to 50 μm, more preferably 2 μm to 40 μm, and further preferably 3 μm to 25 μm. By making the thickness of the hard coating layer 3033 satisfy this range, it is possible to effectively prevent scratches on the first substrate 3021 and also to suppress scratches on the hard coating film 3030 itself. In addition, when the hard coating layer 3033 is formed, the occurrence of warping of the hard coating film caused by the curing shrinkage of the hard coating agent can be suppressed.

[0430] The process of providing the hard coating layer 3033 on the film substrate 3031 may be substantially the same as the process of providing the adhesive layer 3032. As for the coating method, the drying method, and the curing method, the various methods described above may also be used.

[0431] (Anti-sticking layer 3034)

[0432] When the hard coat film is rolled up during production or storage, the release layer 3034 facilitates the peeling of the adhesive layer of the superimposed hard coat film.

[0433] The anti-adhesive layer 3034 can be formed, for example, as follows: a resin and a surfactant such as a silicone resin, a fluororesin, an aminoalkyd resin, a polyester resin, a paraffin wax, an acrylic resin, a carbamate resin, a melamine resin, a urea resin, a urea-melamine system, a cellulose, a benzoguanamine, etc. are dissolved in an organic solvent or water alone or with a mixture thereof as the main component, and the obtained coating is applied and dried by a common printing method such as a gravure printing method, a screen printing method, an offset printing method, etc. to form the anti-adhesive layer. It should be noted that a curable coating film such as a thermosetting resin, an ultraviolet curable resin, an electron beam curable resin, a radiation curable resin, etc. can be cured to form.

[0434] In particular, it is preferable to perform release treatment using a silicone, fluorine compound, or alkyd resin-based release treatment agent or the like.

[0435] The hard coating 3030 affects the visibility of the surrounding real image observed through the light guide plate 3001 and the image displayed on the light guide plate, so it is preferred that it has specific optical properties. As an example, when sandwiched by 0.5 mm thick soda-lime glass, it is preferred to satisfy the following (A), and more preferably satisfy the following (B) and (C).

[0436] (A) The retardation value is within the range of 0 to 100 nm.

[0437] (B) The total light transmittance measured in accordance with JIS K 7361-1:1997 is 85% or more.

[0438] (C) The haze value measured in accordance with JIS K 7136:2000 is 5% or less.

[0439] In the light guide plate 3001 of the third embodiment of the present invention, the hard coating film 3030 mounted on the first substrate 3021 can prevent the first substrate 3021 from being scratched, and appropriately maintain the optical properties of the first substrate 3021. The hard coating film 3030 has a hard coating layer 3033, so it is not easy to be scratched. In addition, since the adhesive layer 3032 is peelably bonded to the first substrate 3021, when the hard coating film 3030 is scratched, the scratched hard coating film can be easily peeled off from the first substrate 3021 and replaced with another hard coating film that is not scratched. This can prevent the clarity of the light guide plate from being deteriorated.

[0440] <First Modification>

[0441] A first modified example of the third embodiment of the present invention will be described. In the following description, the same reference numerals are given to the same components as those already described, and duplicate descriptions will be omitted.

[0442] Fig.15 Detailed Description of the Invention A hard coating film 3130 according to a first modified example of the third embodiment of the present invention is shown in FIG.

[0443] The hard coating film 3130 includes an adhesive layer 3032, a hard coating layer 3033, and a release layer 3034. The hard coating film 3130 of the first modified example of the third embodiment of the present invention is different from the hard coating film 3030 of the basic example in that it does not include a film substrate 3031.

[0444] An example of a process for producing the hard coating film 3130 is shown below.

[0445] On the anti-adhesive surface of the resin film to which the anti-adhesive treatment is applied, a coating material for forming an anti-adhesive layer 3034 and a hard coating agent for forming a hard coating layer 3033 are sequentially applied, thereby forming an anti-adhesive layer 3034 and a hard coating layer 3033 on the resin film. Next, an adhesive composition for forming an adhesive layer 3032 is applied on the hard coating layer 3033, thereby forming an adhesive layer 3032. Finally, the resin film is peeled off, thereby completing the hard coating film 3130.

[0446] As another configuration, the hard coating layer 3033 and the adhesive layer 3032 may be formed on the non-treated surface of a resin film subjected to a release treatment on one side by the above process, and the resin film may be made into the release layer 3034 .

[0447] The usage and function of the hard coating film 3130 of the first variant of the third embodiment of the present invention are substantially the same as those of the hard coating film 3030 of the basic example, and the same effects are exerted. In addition, since the film is attached to the light guide plate, it also has the effect of preventing fragments from scattering when the light guide plate is damaged.

[0448] <Hard coating formed by overlapping multiple sheets>

[0449] The hard coating films of the basic example and the modified example described above may be mounted on the first substrate 3021 in a state where a plurality of pieces are overlapped. Fig.16 FIG. 3 shows a hard coating film 3030 formed by overlapping two sheets. Fig.17 2 overlapped hard coating films 3130 are shown in FIG. In either case, since the anti-adhesive layer 3034 is present at the contact portion of the two overlapping hard coating films, the second hard coating films 3030B and 3130B located on the upper side can be easily peeled off from the first hard coating films 3030A and 3130A located on the lower side.

[0450] By making the hard coating film have such a structure, when the hard coating film located on the outermost surface is scratched, the hard coating film located therebelow that is not scratched can be used as a new outermost surface simply by peeling it off. Therefore, after removing the scratched hard coating film, it is not necessary to install another hard coating film, and the surface state of the light guide plate can be simply maintained.

[0451] In this configuration, the number of hard coating films to be overlapped is not limited to two as shown in the figure, but may be three or more.

[0452] The method for obtaining two or more hard coating films stacked on top of each other is not particularly limited, and examples thereof include a method of laminating another hard coating film on one hard coating film, or a method of winding a hard coating film into a roll and then cutting the roll.

[0453] In addition, a method of forming a layer corresponding to more than two hard coatings at one time may also be used. In this case, a method of curing all the layers of the continuous stacking in an uncured state by using active energy rays after stacking; a method of curing the lower layer by using active energy rays, applying the upper layer, and curing it again by using active energy rays; a method of applying each layer to a release film or a base film, and then bonding the layers to each other in an uncured or semi-cured state, etc., and from the aspect of improving the interlayer adhesion, it is preferred to use an active energy ray to cure after stacking in an uncured state. As a method of stacking in an uncured state, a known method such as successive coating of the upper layer after coating the lower layer, or multi-layer coating while overlapping and coating more than two layers by multiple slits at the same time can be applied, but it is not limited thereto.

[0454] [Fourth embodiment]

[0455] In the image display light guide plate of the present invention, the holographic layer turns yellow during its manufacture and long-term use, and this yellowing may have an adverse effect on the displayed image. However, by introducing an absorption layer having an absorption peak in the wavelength range of 500 to 600 nm, this yellowing can be reduced without deteriorating the holographic layer.

[0456] <Basic example>

[0457] Next, a fourth embodiment of the light guide plate for image display according to the present invention will be described.

[0458] The image display light guide plate according to the fourth embodiment of the present invention comprises a first resin substrate, a hologram layer, and a first absorption layer. The first absorption layer, the first resin substrate, and the hologram layer are preferably arranged in this order in the thickness direction.

[0459] The image display light guide plate according to the fourth embodiment of the present invention may further include a second resin substrate. The first absorption layer, the first resin substrate, the holographic layer, and the second resin substrate are preferably laminated in this order in the thickness direction.

[0460] In the fourth embodiment of the present invention, the first resin substrate and the second resin substrate may be collectively referred to as “resin substrate.” In addition, in this embodiment, the first absorption layer and the second absorption layer may be collectively referred to as “absorption layer.”

[0461] The image display light guide plate according to the fourth embodiment of the present invention may further include a suitable transparent layer. Examples of the transparent layer include a barrier layer, an adhesive layer, a hard coat layer, and an anchor coat layer.

[0462] The image display light guide plate according to the fourth embodiment of the present invention may further include a glass substrate.

[0463] The image display light guide plate has an incident portion for incident image light, and an image display output portion for displaying an image based on the image light. The holographic layer is arranged between the incident portion and the image display output portion. A diffraction grating pattern is formed in the holographic layer, which guides at least the image light incident from the incident portion to the image display output portion and emits it from the image display output portion. The diffraction grating pattern of the image display output portion transmits at least a portion of the external light incident from the outside of the image display light guide plate. It should be noted that the external light incident portion refers to the surface opposite to the image display output portion.

[0464] The image light incident on the incident portion is guided into the holographic layer and emitted to the outside from the display image emitting portion. On the other hand, the external light also passes through the resin substrate and the display image emitting portion, and as a result, an observer of the display image emitting portion can observe both the image light and the external light in the field of view.

[0465] The image display light guide plate of the fourth embodiment of the present invention can be appropriately used in a display device using VR technology, AR technology or MR technology. For example, in addition to being used for display purposes, the image display light guide plate of the fourth embodiment of the present invention can also be used in devices such as a holographic optical element (HOE) represented by a combiner of a head-up display (HUD) for automobiles or a reflective plate for a reflective liquid crystal display device.

[0466] The material of the resin substrate is not particularly limited as long as it is a transparent material.

[0467] The material used for the resin substrate can be appropriately selected from the substrates used in the first to third embodiments. The material used for the resin substrate preferably contains at least one resin selected from the group consisting of acrylic resins, cyclic polyolefin resins, and polycarbonate resins.

[0468] In the image display light guide plate according to the fourth embodiment of the present invention, when the resin substrate includes two sheets of a first resin substrate and a second resin substrate, the hologram layer may be disposed between the first resin substrate and the second resin substrate.

[0469] In the image display light guide plate according to the fourth embodiment of the present invention, when the image display light guide plate includes a first resin substrate and a glass substrate, the hologram layer may be disposed between the first resin substrate and the glass substrate.

[0470] The resin substrate and the hologram layer, or the glass substrate and the hologram layer, may be in contact with each other, or an appropriate transparent layer may be disposed therebetween.

[0471] The hologram layer is interposed between the first resin substrate and the second resin substrate, or between the first resin substrate and the glass substrate.

[0472] The holographic layer uses a known hologram-forming resin material as in the first to third embodiments. Examples of the hologram-forming resin material include a solvent-soluble thermosetting resin having at least one cationically polymerizable ethylene oxide ring in a structural unit, and a hologram recording material composed of an ethylenic monomer capable of free radical polymerization (Japanese Patent Application Publication Nos. 8-1676, 8-1677, 8-1678, and 8-1679).

[0473] The absorption layer has a wavelength characteristic of absorbing a yellow component of light that has passed through at least a portion of the image display light guide plate.

[0474] (Absorption peak)

[0475] The absorption layer has an absorption peak in a wavelength range of 500 to 600 nm (hereinafter sometimes referred to as "wavelength range A").

[0476] Here, "absorption peak" refers to a spectral distribution where the minimum value is the smallest in a U-shaped spectral distribution in which the transmittance changes from decreasing to increasing via a minimum value in the spectral transmittance curve of the absorption layer in the visible light region (400 to 800 nm). It is more preferred that the U-shaped spectral distribution is formed at one place in the visible light region.

[0477] In this specification, the case where the wavelength giving the minimum value (peak top) of such an "absorption peak" is within a specific wavelength range is defined as "having an absorption peak in a specific wavelength range".

[0478] The absorption peak is more preferably in the wavelength range of 550 to 585 nm (hereinafter sometimes referred to as "wavelength range B").

[0479] The half-value width of the absorption peak is preferably 100 nm or less, more preferably 70 nm or less, particularly preferably 40 nm or less.

[0480] Here, the half-width of the absorption peak refers to the wavelength width of the absorption peak at which the transmittance is Th=(100-Tp) / 2 or less, assuming that the transmittance of the peak top of the absorption peak is Tp(%).

[0481] When the half-value width is 100 nm or less, the color balance and brightness of the transmitted light can be well secured.

[0482] The transmittance in the absorption peak is preferably 80% or less, more preferably 70% or less, particularly preferably 60% or less.

[0483] (Transmittance characteristics)

[0484] The average transmittance of the absorption layer in the wavelength range of 590 to 700 nm (hereinafter sometimes referred to as "wavelength range C") is preferably 20% or more, more preferably 50% or more, and even more preferably 70% or more.

[0485] This is because, in the wavelength range C, when the average transmittance is 20% or more, the brightness of red light can be maintained.

[0486] The average transmittance of the absorption layer in the wavelength range of 470 to 550 nm (hereinafter sometimes referred to as "wavelength range D") is preferably 20% or more, more preferably 50% or more, and further preferably 70% or more.

[0487] This is because, in the wavelength range D, when the average transmittance is 20% or more, the color balance and brightness of the transmitted light can be ensured.

[0488] Regarding the transmittance characteristics of the absorption layer, the lower the transmittance of ultraviolet light that is less likely to cause light degradation, the more preferably. For example, the transmittance of the absorption layer in the wavelength range below 380 nm is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less.

[0489] (Yellowness)

[0490] The YI value (JIS K 7373: 2006) indicating the yellowness of the absorbing layer is preferably 10 or less, more preferably 5 or less, and particularly preferably 3 or less.

[0491] (Absorbance)

[0492] The absorbance of the absorption layer at a wavelength of 580 nm is preferably 0.5 or less, more preferably 0.3 or less, and particularly preferably 0.2 or less.

[0493] (b* in the L*a*b* colorimetric system)

[0494] The b* of the absorbing layer is preferably 5 or less, more preferably 3 or less, and particularly preferably 1 or less.

[0495] The structure of the absorption layer is not particularly limited as long as it has an absorption peak in the wavelength range A.

[0496] For example, the absorption layer may have a structure in which a colorant is dispersed in a transparent base resin.

[0497] The material of the base resin is not particularly limited as long as it is transparent, and the refractive index of the base resin is also not particularly limited.

[0498] For example, the base resin may have a refractive index that is higher than or lower than the refractive index of the resin substrate.

[0499] For example, as the base resin, a resin material having a higher surface hardness than the resin base material may be used.

[0500] For example, as the base resin, a resin material with low hygroscopicity can be used.

[0501] The colorant is not particularly limited as long as the above-mentioned wavelength characteristics can be obtained. For example, dyes, pigments, etc. are used as the colorant. As the colorant, a bluing agent is particularly preferably used.

[0502] For example, the absorption layer may be formed of a multilayer thin film in which a high refractive index material and a low refractive index material are stacked in multiple layers.

[0503] (Bluing agent)

[0504] The bluing agent used in the absorbing layer is not particularly limited, but anthraquinone dyes are generally more preferred because they are easily available.

[0505] As specific bluing agents, for example, generic name solvent violet 13 [CA.No (Dye Index Number) 60725], generic name solvent violet 31 [CA.No 68210], generic name solvent violet 33 [CA.No 60725], generic name solvent blue 94 [CA.No61500], generic name solvent violet 36 [CA.No 68210], generic name solvent blue 97 ["Macrolex Violet RR" manufactured by Bayer AG], generic name solvent blue 45 [CA.No61110], etc. can be cited as representative examples. These bluing agents can be used alone or in combination of two or more. These bluing agents are mixed in the base resin in an appropriate amount to obtain the desired optical properties in the absorption layer. For example, when the base resin is a polycarbonate resin, 0.1×10 -5 ~2×10 -4 The components are mixed in the proportion of parts by mass.

[0506] Examples of other bluing agents include Diaresin (registered trademark) Blue N (trade name; manufactured by Mitsubishi Chemical Corporation), Diaresin (registered trademark) Blue G (trade name; manufactured by Mitsubishi Chemical Corporation), Macrolex (registered trademark) Blue RR (trade name; manufactured by Bayer AG), Macrolex (registered trademark) Blue 3R (trade name; manufactured by Bayer AG), Polysynthren (registered trademark) Blue RLS (trade name; manufactured by Clariant AG), and the like.

[0507] The absorption layer is provided in a range that transmits at least image light and external light. For example, the absorption layer may be arranged in a range that overlaps with the display image emission portion in the holographic layer in the thickness direction.

[0508] However, the absorbing layer may be arranged in a range covering the entire resin substrate or the hologram layer when viewed in the thickness direction.

[0509] The arrangement of the absorption layer in the thickness direction of the image display light guide plate is not particularly limited.

[0510] For example, the absorption layer may be provided at least one of a position closer to the incident surface of the external light than the hologram layer and a position closer to the emitting surface of the image light than the hologram layer.

[0511] When the absorption layer is arranged outside the resin substrate, the absorption layer, the resin substrate and the holographic layer can be arranged in order in the thickness direction of the image display light guide plate. That is, the absorption layer can be arranged outside the resin substrate in the thickness direction. For example, the absorption layer can be arranged at the outermost part of the image display light guide plate in the thickness direction.

[0512] When the colorant is dispersed inside the resin substrate to form an absorption layer, the colorant may be uniformly dispersed in the resin substrate or dispersed in a biased manner in the thickness direction. When the colorant is biased in the thickness direction, the colorant is more preferably biased outside the thickness direction of the image display light guide plate.

[0513] The barrier layer can be made of the same material as in the second embodiment, and is preferably made of a transparent inorganic material. The barrier layer preferably has a refractive index of 1.48 or more.

[0514] As the material of the barrier layer, a water vapor barrier material is more preferably used. The barrier layer more preferably contains one or more substances selected from the group consisting of silicon oxide, silicon oxynitride, and diamond-like carbon (DLC).

[0515] The barrier layer may be disposed on the resin film. In this case, the resin film is more preferably disposed between the barrier layer and the resin substrate.

[0516] The barrier layer is more preferably disposed in the order of the resin substrate, the barrier layer, and the hologram layer in the thickness direction of the image display light guide plate. The barrier layer is particularly preferably disposed on the surface of the hologram layer.

[0517] The barrier layer may be provided in two layers with the hologram layer sandwiched therebetween. The barrier layer is more preferably disposed on the front and back surfaces of the hologram layer.

[0518] When a glass substrate is provided, since the glass substrate itself has a barrier property, the glass substrate can be provided on the surface of the hologram layer opposite to the surface facing the barrier layer.

[0519] The following is based on Fig.18 The example shown will explain the detailed structure of an example of the light guide plate for image display according to the fourth embodiment of the present invention. Fig.18 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a fourth embodiment of the present invention.

[0520] Fig.18 In the image display light guide plate 4005 shown, the first absorption layer 4004, the first resin substrate 4001, the hologram layer 4002, and the second resin substrate 4003 are arranged in this order in the thickness direction. The image display light guide plate 4005 is an example of a case where no barrier layer is provided.

[0521] The planar shape of the image display light guide plate 4005 is not particularly limited. For example, the image display light guide plate 4005 may be shaped into a shape that can be mounted in a display device to be used.

[0522] For example, the image display light guide plate 4005 may be a rectangular plate larger than the shape to be mounted on the display device. In this case, the image display light guide plate 4005 may be cut into a shape that can be mounted on the display device before being mounted on the display device.

[0523] The image display light guide plate 4005 may be in the form of a flat plate, or may be in the form of a curved plate as required.

[0524] The following description will take as an example a case where the image display light guide plate 4005 is composed of a flat plate that is rectangular in plan view.

[0525] The first absorption layer 4004 is arranged at the outermost portion in the thickness direction of the image display light guide plate 4005. The first absorption layer 4004 is arranged on the surface of the image display light guide plate 4005 on which the display image is emitted.

[0526] The thickness of the first absorbing layer 4004 is not particularly limited. For example, the thickness of the first absorbing layer 4004 may be 0.1 to 10 μm.

[0527] exist Fig.18 In the illustrated example, the first absorption layer 4004 is formed on the entire surface of a first resin base material 4001 described later.

[0528] The method for forming the first absorbing layer 4004 is not particularly limited. For example, the first absorbing layer 4004 can be formed by applying a coating liquid composed of a base resin material mixed with a colorant to a film-forming surface (the surface of the first resin substrate 4001) and then curing the coating liquid.

[0529] As a coating method for the coating liquid, an appropriate coating method can be selected according to the viscosity of the coating liquid, for example, as a coating method, existing well-known coating methods such as rod coating, dip coating, reverse gravure coating, direct gravure printing, roller coating, die coating, curtain coating, etc. can be used.

[0530] As the base resin material, for example, a polymerizable monomer or polymerizable oligomer such as a (meth)acrylate monomer having a free radical polymerizable unsaturated group in the molecule or a (meth)acrylate oligomer having a free radical polymerizable unsaturated group in the molecule, which forms a cured product by irradiation with active energy rays, or a curable resin material such as urethane, epoxy resin or polyester can be used. As the colorant mixed in the base resin material, for example, the above-mentioned bluing agent can be used.

[0531] The first resin substrate 4001 has the same outer shape as that of the image display light guide plate 4005 .

[0532] Image light Ld emitted from the hologram layer 4002 and external light Lo transmitted through the second resin substrate 4003 and the hologram layer 4002 described later are transmitted through the first resin substrate 4001 .

[0533] The thickness of the first resin substrate 4001 is not particularly limited, and for example, the thickness of the first resin substrate 4001 may be 0.01 to 10 mm.

[0534] The material forming the first resin substrate 4001 can be appropriately selected from the same materials as those in the first to third embodiments, and there is no particular limitation as long as it is a transparent resin material. Examples of the material forming the first resin substrate 4001 include: polyolefin resins such as homopolymers or copolymers of olefins such as ethylene, propylene or butene; amorphous polyolefin resins such as cyclic polyolefins; polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN); polyamide resins such as nylon 6, nylon 66, nylon 12, and copolymerized nylon; partial hydrolyzate of ethylene-vinyl acetate copolymer (EVOH), polyimide resins, polyetherimide resins, polysulfone resins, polyether imide resins, Sulfone resin, polyetheretherketone resin, polycarbonate resin, polyvinyl butyral resin, polyarylate resin, fluororesin, poly(meth)acrylic resin, polystyrene resin, polyvinyl alcohol, ethylene vinyl alcohol copolymer, polyvinyl chloride, cellulose, acetyl cellulose, polyvinylidene chloride, polyphenylene sulfide, polyurethane, phenol resin, epoxy resin, polyarylate resin, polynorbornene, styrene-isobutylene-styrene block copolymer (SIBS), allyl diglycol carbonate, and organic materials such as biodegradable resin. It should be noted that the first resin substrate 4001 can be formed of two or more materials, or can be a laminated structure formed by laminating two or more materials.

[0535] Polycarbonate or poly(meth)acrylic resin is preferred from the perspective of transparency of the first resin substrate 4001. In addition, poly(meth)acrylic resin, epoxy resin or cyclic polyolefin is preferred from the perspective of process resistance of the first resin substrate 4001.

[0536] The hologram layer 4002 is laminated on the surface of the first resin substrate 4001 opposite to the surface on which the first absorption layer 4004 is formed. The configuration of the hologram layer 4002 is as described above and is not particularly limited. The hologram layer 4002 is formed with a suitable diffraction grating corresponding to the function required of the image display light guide plate 4005.

[0537] The second resin substrate 4003 is laminated on the surface of the hologram layer 4002 on the opposite side to the surface on which the first resin substrate 4001 is disposed. As the second resin substrate 4003, the same configuration as that exemplified in the description of the first resin substrate 4001 is used. However, the thickness, material, etc. of the second resin substrate 4003 may be different from those of the first resin substrate 4001. In particular, since the second resin substrate 4003 is disposed on the surface on the external light incident side opposite to the side on which the displayed image is emitted in the image display light guide plate 4005, a material having a higher surface hardness than the first resin substrate 4001 may be used.

[0538] Such an image display light guide plate 4005 can be manufactured, for example, as follows.

[0539] The first resin substrate 4001 and the second resin substrate 4003 are prepared, and a coating liquid for forming the first absorption layer 4004 is adjusted.

[0540] For example, a coating liquid is applied to the surface of the first resin substrate 4001. The coating liquid is then cured to form the first absorption layer 4004.

[0541] For example, a photopolymer material for forming a hologram is applied to the surface of the first resin substrate 4001 on the side opposite to the side where the first absorption layer 4004 is formed. In this case, a transparent sealing layer having the same thickness as the hologram layer 4002 may be provided on the outer periphery of the surface of the first resin substrate 4001. In this case, the photopolymer material is applied to the concave portion surrounded by the sealing layer. After the hologram layer 4002 is formed, the sealing layer seals the outer periphery of the hologram layer 4002. Thereafter, the second resin substrate 4003 is placed on the photopolymer material.

[0542] However, the above manufacturing sequence is an example. For example, a photopolymer material may be applied to the surface of the second resin substrate 4003, and the first resin substrate 4001 on which the first absorption layer 4004 is formed may be placed on the photopolymer material.

[0543] Thereafter, the laminate including the first absorbing layer 4004, the first resin substrate 4001, the photopolymer material, and the second resin substrate 4003 is bonded together by pressing under reduced pressure.

[0544] Thereafter, interference fringes corresponding to the diffraction pattern are formed in the photopolymer material of the laminate, and a diffraction grating is formed in the photopolymer material.

[0545] In this way, the light guide plate 4005 for image display is manufactured.

[0546] Next, an example of a display device including the light guide plate 4005 for image display will be described.

[0547] Fig.19 This is a schematic cross-sectional view showing an example of a display device including a light guide plate for image display according to a fourth embodiment of the present invention.

[0548] like Fig.19 As shown, the display device 4010 includes an image light projection unit 4012 and an incident optical system 4011 in addition to the light guide plate 4005 for image display.

[0549] The image light projection unit 4012 projects the image light Li to be displayed on the image display light guide plate 4005 based on an image signal sent from a controller (not shown).

[0550] The incident optical system 4011 includes an optical element such as a prism for causing the image light Li to enter the image display light guide plate 4005. The incident optical system 4011 causes the image light Li to enter an incident portion 4005a formed on the surface of the image display light guide plate 4005. For example, the incident portion 4005a is provided on the first absorption layer 4004.

[0551] The image light Li incident on the incident portion 4005a is guided to the display diffraction grating portion 4002b of the hologram 4002 via the waveguide diffraction grating portion 4003a formed on the hologram 4002. The image light Li is diffracted at a position corresponding to each display pixel in the display diffraction grating portion 4002b to form image light Ld. The image light Ld is transmitted through the hologram 4002, the first resin substrate 4001, and the first absorption layer 4004, and is emitted as image light Ld' to the outside of the image display light guide plate 4005. Therefore, the display diffraction grating portion 4002b in the thickness direction, and the region of the first resin substrate 4001 and the first absorption layer 4004 that are opposite to the display diffraction grating portion 4002b in the thickness direction constitute the display image emission portion 4005b that displays the image light Ld. The display image emission portion 4005 b is formed at a position separated from the incident portion 4005 a in the surface direction which is a direction perpendicular to the thickness direction.

[0552] On the other hand, external light Lo enters the image display light guide plate 4005 via the second resin substrate 4003. The external light Lo passes through the second resin substrate 4003, the hologram layer 4002, the first resin substrate 4001 and the first absorption layer 4004, and is emitted to the outside of the image display light guide plate 4005 as external light Lo'.

[0553] The user of the display device 4010 can observe an image based on the image light Ld' and the external light Lo'. Therefore, the user whose display image emitting unit 4005b falls into the field of view can observe an image in which the external scene based on the external light Lo' and the image based on the image light Ld' are superimposed.

[0554] The transparent materials used in the image display light guide plate 4005 are photo-degraded over time due to the influence of ultraviolet light, etc. A typical photo-degradation is yellowing of the material. In particular, since the hologram layer 4002 is formed of a photopolymer material, a certain degree of yellowing occurs immediately after manufacturing. Therefore, the light passing through the first resin substrate 4001, the second resin substrate 4003 and the hologram layer 4002 is yellowed.

[0555] Since yellow has a high luminosity function, human vision is sensitive to yellowing, so the contrast (brightness) of the yellowed image is reduced, making the observed image unclear.

[0556] However, in the fourth embodiment of the present invention, since the first absorption layer 4004 is provided in the display image emitting portion 4005b, the yellow component of the image light Ld and the external light Lo is reduced in the image light Ld' and the external light Lo', respectively. In this way, the first absorption layer 4004 is used to offset the yellow component of the yellowing image light Ld and the external light Lo, thereby eliminating the influence of yellowing of the first resin substrate 4001, the second resin substrate 4003 and the hologram layer 4002.

[0557] Specifically, the first absorption layer 4004 absorbs light mainly in the wavelength range of 500 to 600 nm, thereby reducing the yellow tint and relatively increasing the blue tint, thereby improving the white balance and contrast of the image.

[0558] In addition, even if the photodegradation of transparent materials such as the first resin substrate 4001 and the second resin substrate 4003 progresses over time due to exposure to ultraviolet light or the like when the display device 4010 is used, the degree of image degradation due to yellowing can be reduced compared to the case where the first absorption layer 4004 is not provided.

[0559] As described above, according to the fourth embodiment of the present invention, it is possible to provide a light guide plate for image display that can reduce the influence of yellowing of a transparent material on a displayed image.

[0560] In particular, in the fourth embodiment of the present invention, the first absorption layer 4004 is disposed at the outermost portion of the image display light guide plate 4005. Therefore, for example, when a material having a higher hardness than the first resin substrate 4001 is used as the first absorption layer 4004, it is possible to prevent the surface of the first resin substrate 4001 from being scratched. For example, when the transmittance of ultraviolet light in the wavelength characteristics of the first absorption layer 4004 is low, since the incidence of ultraviolet light from the first resin substrate 4001 side can be suppressed, the light degradation over time in the image display light guide plate 4005 can be reduced.

[0561] <First Modification>

[0562] A first modified example of the fourth embodiment will be described.

[0563] Fig. 20 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a first modified example of the fourth embodiment of the present invention.

[0564] like Fig. 20 As shown, the image display light guide plate 4007 according to the first modified example of the fourth embodiment of the present invention further includes a second absorption layer 4006 in the image display light guide plate 4005 according to the basic example of the fourth embodiment of the present invention.

[0565] The following description will focus on the differences from the basic example of the fourth embodiment of the present invention described above.

[0566] The second absorption layer 4006 is laminated on the surface of the second resin substrate 4003 opposite to the surface on which the hologram layer 4002 is disposed. That is, the second absorption layer 4006 is disposed at the outermost portion of the image display light guide plate 4007, similarly to the first absorption layer 4004. In the image display light guide plate 4007, a laminate formed of the first resin substrate 4001, the hologram layer 4002, and the second resin substrate 4003 is sandwiched between the first absorption layer 4004 and the second absorption layer 4006.

[0567] As the second absorption layer 4006, the same structure as that exemplified in the description of the first absorption layer 4004 is used.

[0568] However, the thickness, material, etc. of the second absorption layer 4006 may be different from those of the first absorption layer 4004. For example, since the second absorption layer 4006 is disposed on the surface of the image display light guide plate 4007 on the side opposite to the side from which the displayed image is emitted, a material having a higher surface hardness than the second resin substrate 4003 or the first absorption layer 4004 may be used.

[0569] In the first variation of the fourth embodiment of the present invention, since the first absorption layer 4004 and the second absorption layer 4006 are arranged at the outermost part of the image display light guide plate 4007, it is more preferable that the transmittance of ultraviolet light in the wavelength characteristics of the first absorption layer 4004 and the second absorption layer 4006 is low.

[0570] The image display light guide plate 4007 is manufactured in the same manner as the image display light guide plate 4005 in the basic example of the fourth embodiment of the present invention, except that the second absorption layer 4006 is formed on the second resin substrate 4003. The second absorption layer 4006 is formed by the same method as the first absorption layer 4004.

[0571] The image display light guide plate 4007 according to the first modification of the fourth embodiment of the present invention has the same configuration as the image display light guide plate 4005 except for having the second absorption layer 4006. Therefore, the image light Ld is transmitted through the first absorption layer 4004 as in the image display light guide plate 4005, thereby reducing the yellow component (image light Ld').

[0572] On the other hand, the external light Lo further passes through the second absorption layer 4006 and then enters the second resin substrate 4003. Therefore, the yellow component of the external light Lo is reduced when passing through the second absorption layer 4006. When the external light Lo passes through the second resin substrate 4003, the hologram layer 4002, and the first resin substrate 4001, the yellow component increases according to the degree of yellowing of each, and then the yellow component is reduced by the first absorption layer 4004.

[0573] Since the second resin substrate 4003 is arranged on the incident side of the external light Lo during use, light degradation is likely to progress due to the external light Lo. Therefore, the yellowing of the second resin substrate 4003 may progress more easily over time than the yellowing of the first resin substrate 4001. When the yellowing of the second resin substrate 4003 is accelerated, the yellow component of the external light Lo that has passed through the second resin substrate 4003 may become stronger than that of the image light Ld that has not passed through the second resin substrate 4003.

[0574] However, in the first variant of the fourth embodiment of the present invention, since the second absorption layer 4006 is provided, the second absorption layer 4006 can be used to offset the increase in yellow hue caused by the yellowing of the second resin substrate 4003. Therefore, the yellow hue of the external light Lo" emitted by the first absorption layer 4004 is lower than that of the external light Lo' emitted by the light guide plate 4005 for image display. As a result, the yellow hue of each of the image light Ld' and the external light Lo" can be well balanced.

[0575] In particular, when the transmittance of ultraviolet light in the wavelength characteristics of the second absorption layer 4006 is low, the optical degradation of the second resin base material 4003 due to the external light Lo can be reduced.

[0576] As described above, according to the first modification of the fourth embodiment of the present invention, it is possible to provide a light guide plate for image display capable of reducing the influence of yellowing of a transparent material on a displayed image.

[0577] <Second Modification>

[0578] A second modified example of the fourth embodiment will be described.

[0579] Fig.21 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a second modified example of the fourth embodiment of the present invention.

[0580] like Fig.21 As shown in FIG. 1 , the image display light guide plate 4020 of the second variant of the fourth embodiment of the present invention further includes a first barrier layer 4008 and a second barrier layer 4009 in the image display light guide plate 4007 of the first variant. In the second variant of the fourth embodiment of the present invention, the first barrier layer 4008 and the second barrier layer 4009 are sometimes collectively referred to as "barrier layers". In addition, in the second variant of the fourth embodiment of the present invention, the first resin substrate 4001 and the second resin substrate 4003 are sometimes collectively referred to as "resin substrates". In addition, in the second variant of the fourth embodiment of the present invention, the first absorption layer 4004 and the second absorption layer are sometimes collectively referred to as "absorption layers".

[0581] The following description will focus on the differences from the first variant of the fourth embodiment of the present invention described above.

[0582] The first barrier layer 4008 is disposed between the first resin substrate 4001 and the hologram layer 4002, and is in close contact with the surfaces of the first resin substrate 4001 and the hologram layer 4002. The first barrier layer 4008 prevents gas that has penetrated from the outside of the image display light guide plate 4020 and the first resin substrate 4001 from penetrating into the hologram layer 4002.

[0583] The material of the first barrier layer 4008 is not particularly limited as long as it can block the gas that causes degradation of the holographic layer 4002. The first barrier layer 4008 preferably includes a transparent inorganic material, and more preferably includes at least one inorganic material selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon (DLC), aluminum oxide, and glass, as in the barrier layer in the second embodiment described above.

[0584] In addition, the barrier layer may be disposed on the resin film. In this case, the resin film is more preferably disposed between the barrier layer and the resin substrate.

[0585] For example, the smaller the oxygen permeability and water vapor permeability are, the more preferably the first barrier layer 4008. In particular, it is more preferable that the first barrier layer 4008 is made of a material having excellent water vapor barrier properties (low water vapor permeability).

[0586] For example, the oxygen permeability of the first barrier layer 4008 may be 1 cm 3 / m 2 · Below the day.

[0587] For example, the water vapor permeability of the first barrier layer 4008 may be 1 g / m 2 The water vapor permeability of the first barrier layer 4008 is more preferably 0.5 g / m 2 · Below the day.

[0588] The inorganic material used in the first barrier layer 4008 may have a higher refractive index than the first resin substrate 4001. For example, the refractive index of the first barrier layer 4008 may be 1.48 to 3.00. When the first barrier layer 4008 has a high refractive index, light that passes through the first resin substrate 4001 via the first barrier layer 4008 enters the optically sparse first resin substrate 4001 from the optically dense first barrier layer 4008, so the emission angle of light from the first barrier layer 4008 toward the first resin substrate 4001 increases according to the refractive index difference between the first barrier layer 4008 and the first resin substrate 4001. As a result, the FOV (Field Of View) in the image display light guide plate 4020 can be expanded.

[0589] Regarding the material of the first blocking layer 4008, as described above, it can be an oxide such as zinc oxide, antimony oxide, indium oxide, cerium oxide, calcium oxide, cadmium oxide, silver oxide, gold oxide, chromium oxide, silicon oxide, cobalt oxide, zirconium oxide, tin oxide, titanium oxide, iron oxide, copper oxide, nickel oxide, platinum oxide, palladium oxide, bismuth oxide, magnesium oxide, manganese oxide, molybdenum oxide, vanadium oxide or barium oxide.

[0590] When the first barrier layer 4008 is formed of silicon oxide, the thickness thereof may be 10 to 300 nm. If the thickness is less than 10 nm, the moisture resistance may be insufficient. If the thickness is greater than 300 nm, the silicon oxide film may be prone to cracking and may be easily peeled off from the film-forming surface.

[0591] A particularly preferred layer thickness is 20 to 200 nm.

[0592] The method for forming the first barrier layer 4008 from the silicon oxide is not particularly limited. For example, the first barrier layer 4008 can be formed by any conventionally known method such as vacuum evaporation, sputtering, ion plating, or plasma CVD. When the first barrier layer 4008 is formed from the silicon oxide, in order to improve the adhesion between the film-forming surface and the silicon oxide, a surface treatment such as applying a corona discharge treatment or a low-temperature plasma treatment to the film-forming surface, coating a silane coupling agent on the film-forming surface, or coating a mixture of a saturated polyester and an isocyanate on the film-forming surface may be performed.

[0593] For example, when a silicon oxide thin film is formed by vacuum evaporation, silicon, silicon monoxide, silicon dioxide, or a mixture thereof is used as an evaporation substance, and the vacuum evaporation temperature is 1.0×10 -3 ~1.0×10 -5 It is heated and evaporated by electron beam, resistance heating or high frequency heating under a vacuum of Torr.

[0594] Alternatively, a reactive vapor deposition method may be employed while supplying oxygen gas.

[0595] The silicon oxide forming the first barrier layer 4008 may contain calcium, magnesium, or oxides thereof as impurities in an amount of 10 mass % or less.

[0596] When the first barrier layer 4008 is formed of silicon oxynitride, the same structure as the first barrier layer 4008 containing silicon oxide as a main component is used except that the silicon oxide is replaced with the silicon oxynitride.

[0597] DLC is generally an amorphous carbon material formed of a ternary structure of a diamond-like structure, a graphite-like structure, and a polyethylene-like polymer structure containing hydrogen atoms in the structure. In the production of the above-mentioned DLC, when hydrocarbons such as ethylene, acetylene or benzene are used as a carbon source, a substantially ternary structure containing hydrogen is generally formed.

[0598] The DLC is excellent in hardness, lubricity, wear resistance, chemical stability, heat resistance and surface smoothness. Since the DLC forms the dense polymer structure, it is also excellent in gas barrier properties and water vapor barrier properties.

[0599] The method for forming the first barrier layer 4008 of the DLC is not particularly limited. As the coating method of the DLC, for example, a known appropriate coating method such as a plasma CVD method or a physical vapor deposition method such as an ion plating method or an ion beam sputtering method can be used.

[0600] When the first barrier layer 4008 is formed of aluminum oxide, the first barrier layer 4008 may be formed of, for example, only Al2O3, or may be formed by mixing two or more selected from the group consisting of Al, AlO, and Al2O3. The atomic ratio of Al:O in the aluminum oxide layer varies depending on the conditions for producing the aluminum oxide layer. The aluminum oxide layer that can be used as the first barrier layer 4008 may contain a trace amount (up to 3% relative to the total components) of other components within a range that does not impair the barrier performance.

[0601] The thickness of the aluminum oxide layer can be set according to the requirements of the barrier performance. For example, the thickness of the aluminum oxide layer can be 5 to 800 nm.

[0602] The method for forming the first barrier layer 4008 from aluminum oxide is not particularly limited. For example, the first barrier layer 4008 may be formed by PVD (physical vapor deposition) such as vacuum deposition, sputtering, or ion plating, or CVD (chemical vapor deposition).

[0603] For example, in the vacuum evaporation method, Al, Al2O3, etc. can be used as the evaporation source material, and resistance heating, high-frequency induction heating, electron beam heating, etc. can be used as the heating method of the evaporation source. In the vacuum evaporation method, oxygen, nitrogen, or water vapor can be introduced as a reactive gas, or reactive evaporation using means such as ozone addition or ion assistance can be used. In addition, a bias voltage can be applied to the film-forming surface, the temperature of the film-forming surface can be increased, or it can be cooled. The same is true for other film-forming methods such as PVD and CVD methods other than vacuum evaporation methods such as sputtering.

[0604] When the first barrier layer 4008 is formed of glass, examples of the material of the first barrier layer 4008 include borosilicate glass, alkali-free glass, low-alkali glass, soda-lime glass, sol-gel glass, or glass obtained by appropriately heat-treating or surface-treating these glasses. As the material of the first barrier layer 4008, alkali-free glass is particularly preferred from the viewpoint of avoiding coloration due to impurities.

[0605] When the first barrier layer 4008 is formed of glass, the thickness thereof may be 10 to 200 μm. When the thickness is 10 μm or more, the mechanical strength and gas barrier properties tend to be excellent. The thickness is preferably 10 μm or more, and more preferably 30 μm or more. In addition, when the thickness is 200 μm or less, the optical properties as a light guide plate, such as light transmittance, tend to be excellent. The thickness is preferably 200 μm or less, more preferably 100 μm or less, further preferably 75 μm or less, and particularly preferably 50 μm or less.

[0606] The method for forming the first barrier layer 4008 from glass is not particularly limited. As a method for forming the first barrier layer 4008 from glass, for example, a slit-down method, a fusion method, or a float method can be used. In addition, the glass used can be commercially available glass as it is, or commercially available glass can be ground into a desired thickness for use. Examples of the above-mentioned commercially available glass include "EAGLE2000" manufactured by Corning, "AN100" manufactured by Asahi Glass, "OA10G" manufactured by Nippon Electric Glass, and "D263" manufactured by Schott.

[0607] The second barrier layer 4009 is laminated on the surface of the hologram layer 4002 opposite to the surface of the hologram layer 4002 on which the first barrier layer 4008 is formed.

[0608] The second barrier layer 4009 has the same structure as that exemplified in the description of the first barrier layer 4008. However, the second barrier layer 4009 may be different from the first barrier layer 4008 in terms of material, thickness, and the like.

[0609] Such an image display light guide plate 4020 can be manufactured, for example, as follows.

[0610] A first resin substrate 4001 and a second resin substrate 4003 are prepared, and a first barrier layer 4008 and a second barrier layer 4009 are formed on the surfaces of the first resin substrate 4001 and the second resin substrate 4003, respectively. As a method for manufacturing the first barrier layer 4008 and the second barrier layer 4009, an appropriate manufacturing method is selected according to the materials of the first barrier layer 4008 and the second barrier layer 4009.

[0611] For example, a photopolymer material for forming a hologram is applied to the surface of the first barrier layer 4008 in the first resin substrate 4001 on which the first barrier layer 4008 is formed. In this case, a transparent sealing layer having the same thickness as the hologram layer 4002 may be provided on the periphery of the first barrier layer 4008. In this case, the photopolymer material is applied to the concave portion surrounded by the sealing layer. After the hologram layer 4002 is formed, the sealing layer seals the periphery of the hologram layer 4002.

[0612] Thereafter, the second resin substrate 4003 on which the second barrier layer 4009 is formed is placed on the photopolymer material in a state in which the second barrier layer 4009 faces the photopolymer material.

[0613] However, the above manufacturing sequence is an example, and for example, after a photopolymer material is applied to the second resin substrate 4003 on which the second barrier layer 4009 is formed, the first resin substrate 4001 on which the first barrier layer 4008 is formed may be placed on the photopolymer material.

[0614] Thereafter, a laminate including the first absorbing layer 4004, the first resin substrate 4001, the first barrier layer 4008, the photopolymer material, the second barrier layer 4009, the second resin substrate 4003, and the second absorbing layer 4006 is bonded together by reduced pressure pressing.

[0615] Thereafter, interference fringes corresponding to the diffraction pattern are formed in the photopolymer material of the laminate, and a diffraction grating is formed in the photopolymer material.

[0616] In this way, the light guide plate 4020 for image display is manufactured.

[0617] The image display light guide plate 4020 has the same structure as the image display light guide plate 4007 according to the first modification example, except that a first barrier layer 4008 and a second barrier layer 4009 are added.

[0618] The first barrier layer 4008 and the second barrier layer 4009 are made of a transparent inorganic material such as DLC or silicon oxide, but they easily absorb blue light in the wavelength range of 400 nm to 480 nm, so the transmittance of the blue component decreases, resulting in yellowish transmitted light.

[0619] In this way, the first blocking layer 4008 tends to increase the yellow tint of the external light Lo and the image light Ld, and the second blocking layer 4009 tends to increase the yellow tint of the external light Lo. However, since the second modified example of the fourth embodiment of the present invention includes the first absorption layer 4004 and the second absorption layer 4006 as in the first modified example, the increase in the yellow tint caused by the first blocking layer 4008 and the second blocking layer 4009 can be offset by appropriately adjusting the wavelength characteristics of the first absorption layer 4004 and the second absorption layer 4006. That is, the yellow tint of the external light Lo'' and the image light Ld'' emitted from the first absorption layer 4004 can be reduced. In addition, the balance of the yellow tint of the external light Lo''' and the image light Ld'' can be made good as in the first modified example.

[0620] As described above, according to the second variation of the fourth embodiment of the present invention, it is possible to provide a light guide plate for image display that can reduce the influence of yellowing of a transparent material on a displayed image.

[0621] Furthermore, according to the image display light guide plate 4020, since the first barrier layer 4008 and the second barrier layer 4009 are provided, it is possible to suppress the time-dependent degradation of the hologram layer 4002.

[0622] The gas barrier properties of the first resin substrate 4001 and the second resin substrate 4003 vary in degree depending on the type of resin material, but are significantly lower than glass. Therefore, the first resin substrate 4001 and the second resin substrate 4003 have higher hygroscopicity and water vapor permeability than glass.

[0623] As a result, the gas outside the image display light guide plate 4005 permeates through the first resin substrate 4001 and the second resin substrate 4003 to a certain extent or accumulates inside. In particular, water easily accumulates in the first resin substrate 4001 and the second resin substrate 4003.

[0624] However, even if gas and water that penetrate into the first resin substrate 4001 and the second resin substrate 4003 from the outside diffuses in the image display light guide plate 4020, they are blocked by the first barrier layer 4008 and the second barrier layer 4009. Thus, the penetration of gas and water vapor into the hologram layer 4002 can be suppressed.

[0625] For example, by suppressing the penetration of moisture into the hologram layer 4002, the degradation of the hologram layer 4002 can be prevented.

[0626] Furthermore, since the image display light guide plate 4020 has the above-mentioned layer structure, the hologram layer 4002 does not contact the first resin substrate 4001 and the second resin substrate 4003. Therefore, even if the image display light guide plate 4020 is placed in a high temperature environment, the hologram layer 4002 can be prevented from corroding the first resin substrate 4001 and the second resin substrate 4003.

[0627] In particular, when the refractive indexes of the first barrier layer 4008 and the second barrier layer 4009 are higher than the refractive indexes of the first resin substrate 4001 and the second resin substrate 4003, as described above, the emission angle of light from the first barrier layer 4008 toward the first resin substrate 4001 increases. Similarly, the emission angle of light incident from the second resin substrate 4003 to the second barrier layer 4009 is narrow. Therefore, light incident from the outside on the second resin substrate 4003 side and passing through the image display light guide plate 4005 can be incident in a wider angle range than in the case where the second barrier layer 4009 is not provided, and can be emitted in a wider angle range than in the case where the first barrier layer 4008 is not provided. As a result, the field of view of external light can be further expanded, and the FOV on the display side can also be expanded.

[0628] As described above, regarding the image light from the hologram layer 4002 , the emission angle of the light increases from the first barrier layer 4008 toward the first resin substrate 4001 , and as a result, the FOV of the display screen can be expanded compared to the case where the first barrier layer 4008 is not provided.

[0629] In particular, in the second variant of the fourth embodiment of the present invention, by stacking the first blocking layer 4008 and the second blocking layer 4009 on the hologram layer 4002, the diffusion position of the external light and the image light is close to the diffraction position of the hologram layer 4002 constituting the display screen. Therefore, compared with the case where the first blocking layer 4008 and the second blocking layer 4009 are provided at a position away from the hologram layer 4002, a clearer image can be observed from a wider range of angles.

[0630] Here, a method for measuring the brightness value and FOV in the light guide plate 4020 for image display is briefly described.

[0631] The brightness value in the image display light guide plate 4020 is measured using a display device and a brightness meter similar to the display device 4010 in the basic example of the fourth embodiment of the present invention, except that the image display light guide plate 4005 is replaced by the image display light guide plate 4020.

[0632] In the measurement of the brightness value, in the above-mentioned display device, the center of the display image emitting portion of the image display light guide plate 4020 is arranged at a position opposite to the above-mentioned brightness meter on the measurement optical axis of the above-mentioned brightness meter. The distance between the above-mentioned display image emitting portion and the above-mentioned brightness meter is a distance corresponding to the eye position of the user when the above-mentioned display device is installed. For example, when the above-mentioned display device is a head-mounted display, the distance is 15 mm.

[0633] The brightness value is the brightness measured by the brightness meter when a white image with maximum brightness is displayed on the display device.

[0634] In measuring the FOV of the image display light guide plate 4020, the brightness is measured by tilting the measurement optical axis of the brightness meter relative to the display image emission portion while the white image with the maximum brightness is displayed on the display device. For example, the brightness meter is supported by the goniometer or the like so as to be tilted and swingable at an appropriate angle from a position perpendicular to the image display light guide plate 4020.

[0635] The FOV is obtained as follows: the brightness corresponding to the inability to observe the above-mentioned white image is used as a threshold, and the FOV is obtained in the form of an angle range in which a brightness above the threshold is obtained. When the brightness above the threshold is obtained in the range of -θ1 to +θ2, the FOV is θ1+θ2. Here, regarding the angle, the normal angle of the image display light guide plate 4020 is assumed to be 0°.

[0636] <Third Modification>

[0637] A third modified example of the fourth embodiment will be described.

[0638] Fig. 22 This is a schematic cross-sectional view showing an example of a light guide plate for image display according to a third modified example of the fourth embodiment of the present invention.

[0639] like Fig. 22 As shown, the image display light guide plate 4024 of the third variant example eliminates the first absorption layer 4004 of the image display light guide plate 4005 of the basic example of the fourth embodiment of the present invention, and is provided with a first resin substrate (absorption layer) 4021 and a second resin substrate (absorption layer) 4023 to replace the first resin substrate 4001 and the second resin substrate 4003.

[0640] The following description will focus on the differences from the basic example of the fourth embodiment of the present invention described above.

[0641] The first resin substrate (absorbing layer) 4021 includes the same base resin as the first resin substrate 4001 and a colorant dispersed in the base resin.

[0642] The colorant contained in the first resin substrate (absorption layer) 4021 is the same colorant as that of the first absorption layer 4004 in the basic example of the fourth embodiment of the present invention. The mixing amount of the colorant is set so that the first resin substrate (absorption layer) 4021 has the same light absorption property as that of the first absorption layer 4004 in the basic example of the fourth embodiment of the present invention.

[0643] The second resin base material (absorption layer) 4023 has the same structure as the first resin base material (absorption layer) 4021 .

[0644] In the image display light guide plate 4024, the first resin substrate (absorption layer) 4021 and the second resin substrate (absorption layer) 4023 prepared by the substrate preparation step are molded using a material obtained by adding a colorant to each base resin, and the absorption layer forming step is not performed. Except for this, it is manufactured in the same manner as the image display light guide plate 4005 in the basic example of the fourth embodiment of the present invention.

[0645] The image display light guide plate 4024 is an example in which the absorption layer is formed using the first resin base material (absorption layer) 4021 and the second resin base material (absorption layer) 4023 .

[0646] According to the image display light guide plate 402, since the first resin base material (absorption layer) 4021 and the second resin base material (absorption layer) 4023 serve as absorption layers, the yellow tint in the external light and the image light can be reduced similarly to the first modification.

[0647] As described above, according to the third variation of the fourth embodiment of the present invention, it is possible to provide a light guide plate for image display that can reduce the influence of yellowing of a transparent material on a displayed image.

[0648] It should be noted that, in the basic example and various variations of the fourth embodiment of the present invention, the absorption layer is arranged at the outermost portion of the image display light guide plate. However, the absorption layer can reduce the yellow hue of the light emitted from the image display light guide plate regardless of where it is arranged as long as it is on the optical path of the external light Lo and the image light Ld.

[0649] In the basic example and various modified examples of the fourth embodiment of the present invention, the absorption layer is in contact with the resin substrate. However, the absorption layer may be laminated on a transparent resin film. In this case, for example, the absorption layer can be formed on the resin film and then fixed to the configuration surface by an adhesive, so that the absorption layer can be easily formed.

[0650] In the second modification, the barrier layer is arranged on the front and back of the hologram layer. However, the barrier layer may be arranged between the resin substrate and the hologram layer for the purpose of shielding water and the like that penetrates through the resin substrate and preventing the hologram layer from contacting the resin substrate.

[0651] However, in this case, if the hygroscopicity of the transparent layer sandwiched between the barrier layer and the holographic layer is high, moisture may penetrate through the side of the transparent layer. Therefore, the transparent layer between the barrier layer and the holographic layer is preferably formed of a material with low hygroscopicity. In the case where the transparent layer between the barrier layer and the holographic layer is hygroscopic, it is more preferable that the thickness of the transparent layer is thin. In this case, the exposed area of ​​the side that becomes the penetration port of moisture is reduced, so the water content of the absorbed moisture can be reduced.

[0652] In the second modification, the barrier layer is described as being in contact with the holographic layer and the resin substrate. However, the barrier layer may also be laminated on a transparent resin film. In this case, for example, the barrier layer may be formed on the resin film and then fixed to the resin substrate by an adhesive, so that the barrier layer is easily formed.

[0653] Example

[0654] The present invention will be described in more detail below by way of examples, but the present invention is not limited to the examples described below, and various modifications may be made as long as the gist of the present invention is not changed.

[0655] [Examples and Comparative Examples of the First Embodiment (Examples 1 to 3, Comparative Examples 1 to 3)]

[0656] Next, examples and comparative examples of the first embodiment will be described.

[0657] Table 1 below shows the constitutions and evaluation results of the resin substrates used in Examples 1 to 3 and Comparative Examples 1 to 3.

[0658]

[0659] Mitsubishi Chemical…Mitsubishi Chemical Corporation

[0660] KURARAY…KURARAY Co., Ltd.

[0661] Sumitomo Chemical…Sumitomo Chemical Co., Ltd.

[0662] Asahi Kasei…Asahi Kasei Co., Ltd.

[0663] Acrylite, Comoglas, Sumipex and Delaglas are registered trademarks of their respective companies in Japan.

[0664] <Example 1>

[0665] Example 1 is an example corresponding to the image display light guide plate 1004 of the basic example of the first embodiment.

[0666] As shown in Table 1, acrylic resin (PMMA) was used as the material of the first resin substrate 1001 and the second resin substrate 1003 ("resin substrate" in Table 1). The thickness of the first resin substrate 1001 and the second resin substrate 1003 was 1 mm.

[0667] The hologram layer 1002 is common in each embodiment and each comparative example. As the material of the hologram layer 1002, 100 parts by mass of bisphenol epoxy resin jER1007 (polymerization degree n=10.8, epoxy equivalent: 1750-2200, trade name of Mitsubishi Chemical), 50 parts by mass of triethylene glycol diacrylate, 5 parts by mass of 4,4'-bis(tert-butylphenyl)iodonium hexafluorophosphate, and 0.5 parts by mass of 3,3'-carbonylbis(7-diethylamino)coumarin are mixed and dissolved in 100 parts by mass of 2-butanone, and used as a photosensitive material for a hologram. The thickness of the hologram layer 1002 is 5 μm. The top view size of the hologram layer 1002 is 50 mm×50 mm.

[0668] (Substrate manufacturing process)

[0669] The first resin substrate 1001 and the second resin substrate 1003 of Example 1 were produced as follows.

[0670] 100 parts of MMA (methyl methacrylate) were added to a reactor (polymerization kettle) equipped with a cooling tube, a thermometer and a stirrer and stirred. After bubbling with nitrogen, heating was started. When the internal temperature reached 80°C, 0.05 parts of 2,2'-azobis-(2,4-dimethylvaleronitrile) as a free radical polymerization initiator was added. After further heating to an internal temperature of 100°C, it was maintained for 10 minutes. Thereafter, the reactor was cooled to room temperature to obtain a syrup. The polymerization rate of the syrup was about 20% by mass.

[0671] Thereafter, 0.2 parts by mass of tert-hexyl peroxypivalate and 0.01 parts by mass of dioctyl sodium sulfosuccinate were added to the slurry and completely dissolved at room temperature to form a polymerizable raw material.

[0672] After the dissolved air in the polymerizable raw material was removed under reduced pressure, the raw material was injected into a continuous polymerization apparatus equipped with a pair of mirror-finished stainless steel endless belts.

[0673] Here, the continuous polymerization apparatus used in this example is described.

[0674] Figure 8 This is a schematic longitudinal sectional view showing an example of a manufacturing apparatus for a resin substrate according to Example 1.

[0675] like Figure 8 As shown, the continuous polymerization device 1100 is provided with a pair of endless belts 1101 and 1102 at the top and bottom. The endless belts 1101 and 1102 are respectively driven to run at the same speed by applying tension through main pulleys 1103, 1104, 1105, and 1106. Two or more carrier rollers 1107 are respectively arranged on the inner periphery of each of the endless belts 1101 and 1102. Each carrier roller 1107 is opposed to each other in a manner of sandwiching the mutually opposed endless belts 1101 and 1102 therebetween. Each carrier roller 1107 horizontally supports the endless belts 1101 and 1102 in operation, is at right angles to the belt running direction (from left to right in the figure) of the endless belts 1101 and 1102, and applies at least one linear load to the belt surface from the vertical direction of the belt surface.

[0676] The linear load may be 0.001 to 10.0 kg / cm, and more preferably 0.01 kg / cm or more.

[0677] The more times the linear load is applied, the more preferred it is. When the number of times the linear load is applied increases, the planarity of the obtained resin substrate improves. For example, the number of times the linear load is applied is more preferably 10 times or more.

[0678] A raw material injection device 1114 provided in the continuous polymerization device 1100 supplies a polymerizable raw material between the endless belts 1101 and 1102. The vicinities of both side ends of the endless belts 1101 and 1102 are sealed by two gaskets 1112 having elasticity.

[0679] As the endless belts 1101 and 1102 run, the polymerizable raw material is polymerized by heating it in the first polymerization zone 1108 by means of hot water spray 1109. In addition, the polymerizable raw material is polymerized by heating it in the second polymerization zone 1110 located downstream in the belt running direction by means of a hot air heater. The polymerizable raw material is cooled in the downstream cooling zone 1111 located further downstream in the belt running direction and is taken out in the form of a plate-like polymer 1113.

[0680] The specific production conditions of the polymerizable raw material in Example 1 are as follows.

[0681] In the continuous polymerization device 1100, at the part where the polymerizable raw material is supplied by the raw material injection device 1114, the interval between the belt surfaces of the annular belts 1101 and 1102 is adjusted to 1.6 mm, and at the part where the polymerization is completed and the plate-like polymer is taken out, the interval is continuously adjusted so that the final plate-like polymer is 1 mm.

[0682] In the first polymerization zone 1108, the linear load based on each carrier roller 1107 was 0.3 kg / cm. The hot water temperature of the hot water spray 1109 was 80° C. While the polymerizable raw material stayed in the first polymerization zone 1108, the hot water was continuously applied to the inner peripheral surface of the endless belts 1101 and 1102. The residence time of the polymerizable raw material in the first polymerization zone 1108 was 40 minutes.

[0683] In the second polymerization zone 1110, hot air at a temperature of 120°C was blown toward the inner peripheral surface of the belt from a hot air heater, and the residence time of the polymerizable raw material was set to 10 minutes, and polymerization was completed under this condition.

[0684] In this way, a plate-shaped polymer 1113 having a thickness of 1 mm was obtained.

[0685] The plate-like polymer 1113 was cut into a 200 mm×200 mm rectangle to form evaluation samples 1A of the first resin substrate 1001 and the second resin substrate 1003. The evaluation sample 1A was used for the MC value measurement, the arithmetic mean roughness Ra measurement, and the heat shrinkage measurement described later.

[0686] The plate-like polymer 1113 was cut into a 60 mm×60 mm rectangle to form an evaluation sample 1B. The evaluation sample 1B formed the image display light guide plate 1004 and was used for image evaluation of the image display light guide plate 1004 (described later).

[0687] Next, a description will be given of a manufacturing process of the image display light guide plate 1004 in Example 1. The image display light guide plate 1004 is manufactured by sequentially performing a substrate preparation process and a light guide plate manufacturing process described below.

[0688] (Substrate preparation process)

[0689] In the substrate preparation step, the evaluation sample 1B made of acrylic resin and having a size of 60 mm×60 mm×1 mm in thickness obtained in the substrate production step was cleaned and dried.

[0690] Evaluation Sample 1B was immersed in a 5% aqueous surfactant solution of Semi Clean (registered trademark) M-LO (trade name; manufactured by Yokohama Oil & Fats Industries, Ltd.) as a neutral detergent, and ultrasonic cleaning was performed for 5 minutes.

[0691] After that, the evaluation sample 1B was immersed in ultrapure water and ultrasonically cleaned for 5 minutes. The evaluation sample 1B was further rinsed with ultrapure water, air-dried, and then dried in an oven at 100° C. under a nitrogen atmosphere. The air-dried evaluation sample 1B was then UV-ozone cleaned for 1 minute using a UV ozone cleaner.

[0692] The substrate preparation process is completed as described above.

[0693] (Light guide plate manufacturing process)

[0694] In the light guide plate manufacturing step, two evaluation samples 1B were used to manufacture the image display light guide plate 1004 .

[0695] A sealing layer having a width of 5 mm and a thickness of 5 μm was applied to the peripheral portion of one evaluation sample 1B.

[0696] The sealing layer is formed of a transparent material and is not particularly limited as long as the material can bond the evaluation samples 1B to each other. In Example 1, an epoxy resin or a silicone resin is used.

[0697] In this way, an acrylic resin substrate with a sealing layer step having an opening of 50 mm×50 mm in size surrounded by the sealing layer was prepared.

[0698] Then, an acrylic photosensitive material as a photopolymer material for hologram was applied on the acrylic substrate by spin coating. The acrylic photosensitive material was applied so as to have a thickness of 5 μm after drying.

[0699] Then, another evaluation sample 1B was laminated on the sealing layer and the acrylic photosensitive material, and press-bonded under reduced pressure. The press-bonding conditions were an absolute pressure of 5 kPa, a temperature of 70° C., and a press pressure of 0.04 MPa.

[0700] After that, a diffraction grating is recorded on the photopolymer material of the laminated body after being pressed and bonded. In this process, the temperature of the laminate is maintained at 20°C. As for the diffraction grating, two kinds of lasers are irradiated to the laminated body, and the irradiation angle and intensity of each are adjusted, thereby forming interference fringes in a manner to form a desired diffraction pattern. In this way, the diffraction grating is recorded on the photopolymer material.

[0701] As a specific diffraction grating, each light of red, green and blue wavelength regions incident as image light incident to the incident portion is diffracted, and a diffraction grating for color display emitted from the display image emission portion is formed at a position corresponding to a pixel of the image light.

[0702] Thereafter, the laminate was kept at 20° C. and irradiated with ultraviolet light (wavelength 365 nm, irradiance 80 W / cm 2 ). As a light source of ultraviolet light, a high pressure mercury lamp is used.

[0703] The acrylic photosensitive material is thereby cured, and the image display light guide plate 1004 of Example 1 is formed.

[0704] <Example 2>

[0705] Example 2 is an example corresponding to the image display light guide plate 1014 of the first modified example of the first embodiment.

[0706] As shown in Table 1, Example 2 is the same as Example 1 except that a hard coat is applied to both surfaces of the first resin substrate 1001 in the thickness direction.

[0707] Evaluation sample 1A of Example 2 was obtained by applying a hard coating layer described later to both surfaces of evaluation sample 1A of Example 1 in the thickness direction.

[0708] The evaluation sample 1B of the second embodiment was manufactured in the same manner as the first embodiment except that the evaluation sample 1A of the second embodiment was used instead of the evaluation sample 1A of the first embodiment. Figure 7 Different from the embodiment shown, the first hard coating layer 1011A and the second hard coating layer 1011B are also laminated on the second resin substrate 1003 .

[0709] The substrate manufacturing process of Example 2 will be described below, focusing on the differences from Example 1.

[0710] (Substrate manufacturing process)

[0711] The abbreviations used below are explained.

[0712] “C6DA” refers to 1,6-hexanediol diacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name: Biscoat #230).

[0713] “U6HA” refers to a urethane compound obtained by reacting 3 mol of 2-hydroxypropyl 3-acryloyloxymethacrylate with 1 mol of triisocyanate obtained by trimerizing hexamethylene diisocyanate (manufactured by Shin-Nakamura Chemical Co., Ltd., trade name: NK OLIGO U-6HA).

[0714] “M305” refers to a mixture of pentaerythritol triacrylate and pentaerythritol tetraacrylate (manufactured by Toagosei Co., Ltd., trade name: Aronix (registered trademark) M-305).

[0715] C6DA (60 parts by mass), U6HA (30 parts by mass), M305 (10 parts by mass), 0.5 parts by mass of bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and 5 parts by mass of 1-hydroxycyclohexyl phenyl ketone were mixed to prepare a hard coating solution.

[0716] The hard coating solution was applied to the endless belts 1101 and 1102 of the continuous polymerization device 1100 at a thickness of 20 μm. 2 The hard coating liquid is cured by irradiating ultraviolet light with a high-pressure mercury lamp, thereby forming a hard coating layer on the endless belt.

[0717] The resin substrate was polymerized in the same manner as in Example 1 except that the hard coating layer was formed on the endless belts 1101 and 1102 , thereby obtaining a plate-like polymer 1113 having a thickness of 1 mm and a hard coating layer laminated on the surface.

[0718] Evaluation samples 1A and 1B of Example 2 were formed from the plate-like polymer 1113 of Example 2 in the same manner as in Example 1.

[0719] <Example 3>

[0720] Example 3 is an example corresponding to the image display light guide plate 1004 of the basic example of the first embodiment.

[0721] As shown in Table 1, in Example 3, an acrylic resin plate processed by cutting and grinding was used as the resin substrate, and the other points were the same as those in Example 1. The resin substrate in Example 3 was a 2 mm thick continuous cast acrylic resin plate, i.e., Acrylite (registered trademark) L, processed by cutting and grinding to a substrate having a thickness of 1 mm.

[0722] <Comparative Examples 1 to 3>

[0723] As shown in Table 1, Comparative Examples 1 to 3 were the same as Example 1 except that a conventional extruded acrylic resin plate was used as the resin substrate. Therefore, the substrate manufacturing process of each comparative example was performed for extrusion molding different for each manufacturer.

[0724] As the resin substrate in Comparative Example 1, Comoglas (registered trademark) P (trade name; manufactured by KURARAY CO., LTD.), which is an extruded acrylic resin plate having a thickness of 3 mm, was used.

[0725] As the resin substrate in Comparative Example 2, Sumipex (registered trademark) E (trade name; manufactured by Sumitomo Chemical Co., Ltd.), which is an extruded acrylic resin plate having a thickness of 3 mm, was used.

[0726] As the resin substrate in Comparative Example 3, a 3 mm thick extruded acrylic resin plate, namely, Delaglas (registered trademark) A (trade name; manufactured by Asahi Kasei Corporation) was used.

[0727] In each comparative example, evaluation samples 1A and 1B having the same shape as that of Example 1 were prepared except that the thickness was 3 mm.

[0728] The light guide plate manufacturing process in each comparative example was carried out in the same manner as in Example 1 except that the evaluation sample 1B of each comparative example was used.

[0729] <Evaluation method>

[0730] Next, the evaluation methods of Examples 1 to 3 and Comparative Examples 1 to 3 will be described. As evaluations, MC value, Ra, heat shrinkage rate, and clarity of displayed images were evaluated.

[0731] (MC value)

[0732] The evaluation of the MC value was performed by the evaluation method described in the "Specifications for Carrying Out the Invention" of this specification. As the measurement sample S, the evaluation sample 1A of each example and each comparative example was used.

[0733] As specific evaluation conditions, the distances d1 and d2 are 1 m, and the elevation angle θ A is 20°.

[0734] Since Comparative Examples 1 to 3 have tooth patterns, the evaluation sample 1A of each comparative example is arranged in the evaluation device 1200 with the tooth patterns facing the Y direction.

[0735] In contrast, no tooth pattern was observed in Examples 1 to 3. However, in order to make the directionality during production uniform, the evaluation sample 1A of each example was arranged so that the direction perpendicular to the running direction of the continuous polymerization device 1100 was oriented in the Y direction.

[0736] Regarding the measurement range of brightness distribution, the Y direction in the configuration of the evaluation sample 1A in the evaluation device 1200 is made horizontal (the extension direction of the line segments AD and BC), and the direction orthogonal to the horizontal on the evaluation sample 1A is made vertical (the extension direction of the line segments AB and DC), so that it becomes a rectangular area with a vertical width of 180 mm and a horizontal width of 80 mm.

[0737] The measurement range is set at 41 locations shifted by 2 mm in the lateral direction on the measurement sample S. In each measurement range, a measurement line is selected so as to divide the measurement range into 40 equal parts in the lateral direction.

[0738] Table 1 shows the maximum value of the MC value obtained from the brightness distribution of each measurement line in each measurement range.

[0739] (Ra)

[0740] In the evaluation of Ra, the arithmetic mean roughness Ra of the surface of each evaluation sample 1A was measured.

[0741] As a measuring device, a white light interferometric surface profile measuring instrument Zygo NewView (registered trademark) 6300 (trade name; manufactured by Zygo Corporation) was used. The objective lens had a magnification of 2.5 times and the observation range was a rectangular range of 2.8 mm×2.1 mm.

[0742] (Heat shrinkage)

[0743] The heat shrinkage rate was evaluated by measuring the dimensional change (shrinkage) in accordance with Appendix A “Measurement of dimensional change (shrinkage) during heating” of JIS K 6718:2015.

[0744] (Display image clarity)

[0745] The image display light guide plates of Examples 1 to 3 and Comparative Examples 1 to 3 are installed in an image display device. The image display device is provided with an optical system for causing image light to be displayed to enter an incident portion of the image display light guide plate 1004, a driving power source, and a circuit system for supplying image information for obtaining image light.

[0746] As input images used for evaluation, a white image and a text display image were used.

[0747] The evaluation was performed by visually judging the visual effects of the white image and the text display image. As the text image, "ABCDE" was displayed within a size of 10 mm×100 mm.

[0748] When no rainbow color was seen in the white image and the characters in the character display image were clearly visible, it was judged as good (good, described as "A" in Table 1).

[0749] When rainbow color was slightly observed in the white image and the characters in the character display image were clearly visible, it was judged as fair (described as "B" in Table 1).

[0750] When rainbow color was observed in at least a part of the white image and the outline of the characters was observed vaguely in the character display image, it was determined as unacceptable (no good, described as "C" in Table 1).

[0751] <Evaluation Results>

[0752] As shown in Table 1, the MC values ​​of Examples 1 to 3 are 0.074, 0.103, and 0.060, respectively, all less than 0.120. In contrast, the MC values ​​of Comparative Examples 1 to 3 are 0.126, 0.183, and 0.148, respectively, all greater than 0.120.

[0753] No tooth pattern was observed in Examples 1 to 3, and accordingly, the MC value was less than 0.120. The reason is believed to be that the resin substrate of each embodiment is manufactured by a continuous casting method or cutting and grinding. In the continuous casting method, for example, the surface shape of the endless belts 1101 and 1102 is transferred to the surface of the raw material of the resin substrate of each embodiment. Therefore, the flatness of the surface of the resin substrate is equivalent to the flatness of the endless belts 1101 and 1102. The flatness of the surface of the resin substrate can be greatly improved by cutting and grinding.

[0754] In contrast, since toothing was observed in Comparative Examples 1 to 3, it is considered that the MC value increased due to toothing. The reason why toothing was formed in Comparative Examples 1 to 3 is considered to be due to, for example, large uneven driving of rollers in contact with the extruded material in the extruder.

[0755] The arithmetic mean roughness Ra of Examples 1 to 3 is 4.9 nm, 4.7 nm, and 2.6 nm, respectively, all less than 10 nm. In contrast, the Ra of Comparative Examples 1 to 3 is 5.5 nm, 2.9 nm, and 2.3 nm, respectively, all less than 10 nm. Therefore, regarding the smoothness represented by Ra, there is no significant difference between Examples 1 to 3 and Comparative Examples 1 to 3.

[0756] The heat shrinkage rates of Examples 1 to 3 were all less than 3%. In contrast, the heat shrinkage rates of Comparative Examples 1 to 3 were all 3% or more. This is believed to be because the resin substrates of Comparative Examples 1 to 3 were manufactured by extrusion molding, thereby accumulating strain in the resin substrates.

[0757] The clarity of the displayed images of Examples 1 to 3 was judged as "good (A)". In contrast, the clarity of the displayed images of Comparative Examples 1 to 3 was judged as "unacceptable (C)". This is believed to be because the MC values ​​in Comparative Examples 1 to 3 were larger than those in the Examples, so the diffraction direction of the image light was chaotic.

[0758] For example, it is believed that although the smoothness is better in Examples 1 and 2 because the Ra of the resin substrates of Comparative Examples 2 and 3 is smaller than that of Examples 1 and 2, the planarity (i.e., MC value) contributes more to the clarity of the displayed image. It is believed that at least when Ra is 10 nm or less, the size of Ra has no significant difference in clarity.

[0759] [Example of the second embodiment]

[0760] Next, an example of the second embodiment will be described.

[0761] The following Tables 2A to 2C show the configurations of the resin substrates and barrier layers used in Examples 4 to 7 and 12 to 21, and the evaluation results.

[0762] [Table 2A]

[0763]

[0764] [Table 2B]

[0765]

[0766] In the column of "auxiliary layer" in Table 2B, "EVOH-based" means "ethylene vinyl alcohol-based" and "F-based" means "fluorine-based".

[0767] [Table 2C]

[0768]

[0769] <Example 4>

[0770] Example 4 is an example corresponding to the image display light guide plate 2006 of the basic example of the second embodiment.

[0771] As shown in Table 2A, acrylic resin (PMMA) was used as the material of the first resin substrate 2001 and the second resin substrate 2005 ("resin substrate" in Table 2A).

[0772] The first resin base material 2001 and the second resin base material 2005 are both in the shape of a rectangular plate of 60 mm×60 mm×1 mm.

[0773] The first barrier layer 2002 and the second barrier layer 2004 ("barrier layer" in Table 2B) of this example are DLC films with a thickness of 40 nm.

[0774] Hologram layer 2003 is common in Examples 4 to 7 and 12 to 21. As a material for hologram layer 2003, 100 parts by mass of bisphenol epoxy resin jER (registered trademark) 1007 (polymerization degree n = 10.8, epoxy equivalent: 1750 to 2200, trade name of Mitsubishi Chemical), 50 parts by mass of triethylene glycol diacrylate, 5 parts by mass of 4,4'-bis(tert-butylphenyl)iodonium hexafluorophosphate, and 0.5 parts by mass of 3,3'-carbonylbis(7-diethylamino)coumarin were mixed and dissolved in 100 parts by mass of 2-butanone to serve as a photosensitive material for hologram. The thickness of hologram layer 2003 is 5 μm. The size of hologram layer 2003 in plan view is 50 mm×50 mm.

[0775] Next, a description will be given of a manufacturing process of the image display light guide plate 2006 in Example 4. The image display light guide plate 2006 is manufactured by sequentially performing a substrate preparation process, a barrier layer formation process, and a light guide plate manufacturing process described below.

[0776] (Substrate preparation process)

[0777] In the substrate preparation step, the first resin substrate 2001 and the second resin substrate 2005 are cleaned and dried. Hereinafter, when it is not necessary to distinguish between the first resin substrate 2001 and the second resin substrate 2005, the symbols are omitted and they are simply described as resin substrates.

[0778] The resin substrate was immersed in a 5% aqueous surfactant solution of Semi Clean (registered trademark) M-LO (trade name; manufactured by Yokohama Oil & Fats Industries, Ltd.) as a neutral cleaning agent, and ultrasonic cleaning was performed for 5 minutes.

[0779] After that, the resin substrate was immersed in ultrapure water and ultrasonically cleaned for 5 minutes. The resin substrate was further rinsed with ultrapure water, air-dried, and then dried in an oven at 100° C. under a nitrogen atmosphere. The air-dried evaluation sample 2B was then UV-ozone cleaned for 1 minute using a UV ozone cleaner.

[0780] The substrate preparation process is completed as described above.

[0781] (Barrier Layer Formation Step)

[0782] In the barrier layer forming step, a DLC film is formed on the surface of the resin substrate.

[0783] In space volume 350cm 3 , equipped with high frequency power supply (13.56MHz), internal electrode (Also used as gas introduction tube, front end fine hole ) was placed in a plasma chemical vapor deposition device and vacuum evacuated. After the pressure of the plasma chemical vapor deposition device reached 15 Pa, a 2:1 mixed gas of high-purity acetylene and tetramethylsilane was introduced at a flow rate of 45 sccm, and a DLC film with a film thickness of 40 nm was formed under the conditions of a plasma generation setting power of 100 W and a film formation time of 0.8 seconds.

[0784] The barrier layer forming step is completed as described above.

[0785] Hereinafter, the resin substrate on which the barrier layer is formed is referred to as an intermediate laminate.

[0786] (Light guide plate manufacturing process)

[0787] In the light guide plate manufacturing step, two intermediate laminates are used to manufacture the image display light guide plate 2006 .

[0788] A sealing layer having a width of 5 mm and a thickness of 5 μm was applied to the peripheral portion of the barrier layer of one intermediate laminate.

[0789] The sealing layer is formed of a transparent material and is not particularly limited as long as it can bond the barrier layers of the intermediate laminate to each other. In Example 3, optical adhesive Hard Lock (registered trademark) OP-1045K (trade name; manufactured by Denki Kagaku Kogyo Co., Ltd.) was used.

[0790] In this way, an intermediate laminate with a sealant layer step having an opening of 50 mm×50 mm in size surrounded by the sealant layer was prepared.

[0791] Then, the above-mentioned photosensitive material as a photopolymer material for hologram was applied on the intermediate laminate by spin coating. The photosensitive material was applied so as to have a thickness of 5 μm after drying.

[0792] Then, another intermediate laminate was laminated on the sealing layer and the photosensitive material so that its barrier layer faced the barrier layer of the intermediate laminate with the sealing layer, and pressed under reduced pressure. The pressing conditions were an absolute pressure of 5 kPa, a temperature of 70° C., and a pressing pressure of 0.04 MPa.

[0793] After that, the diffraction grating is recorded on the photosensitive material of the laminated body after being pressed. In this process, the temperature of the laminated body is maintained at 20°C. Regarding the diffraction grating, the laminated body is irradiated with two kinds of lasers, and the irradiation angle and intensity of each are adjusted to form interference fringes in a manner to form the required diffraction pattern. In this way, the diffraction grating is recorded on the photosensitive material.

[0794] As a specific diffraction grating, the diffraction grating diffracts each light of red, green, and blue wavelength regions incident as image light incident on the incident portion, and forms a diffraction grating for color display emitted from the display portion at a position corresponding to a pixel of the image light.

[0795] Thereafter, while the laminate was maintained at 20° C., the entire surface of the laminate was irradiated with ultraviolet light (wavelength 365 nm, irradiance 80 W / cm 2 ). As a light source of ultraviolet light, a high pressure mercury lamp was used.

[0796] The sealing layer is thereby cured, thereby forming the image display light guide plate 2006 of Example 3.

[0797] <Example 5>

[0798] In Example 5, the structure is the same as that of Example 4 except that each DLC film is formed of silicon oxide with a thickness of 10 nm.

[0799] The following describes the substrate manufacturing process of Example 5, focusing on the differences from Example 4.

[0800] The image display light guide plate 2006 of Example 5 is manufactured by sequentially performing a substrate preparation step similar to that of Example 4, a barrier layer formation step described later, and a light guide plate manufacturing step similar to that of Example 4.

[0801] (Barrier Layer Formation Step)

[0802] In the barrier layer forming step of this embodiment, a silicon oxide thin film layer is formed on the surface of the resin substrate.

[0803] After the resin substrate is placed in a vacuum deposition device, silicon oxide is vacuum deposited. The ultimate vacuum degree of the chamber of the vacuum deposition device is set to 1.0×10 -4 In this vacuum, silicon monoxide with a purity of 99.9% was heated and evaporated by high-frequency induction heating to form a 50 nm thick silicon oxide thin film on the surface of the resin substrate. Thus, an intermediate laminate having a silicon oxide thin film layer was obtained.

[0804] The barrier layer forming step is completed as described above.

[0805] The light guide plate manufacturing process of this embodiment is the same as the light guide plate manufacturing process of the fourth embodiment except that the intermediate laminate formed in the above-mentioned barrier layer forming process is used, and thus the description thereof is omitted.

[0806] <Examples 6 and 7>

[0807] As shown in Table 2A, Examples 6 and 7 are the same as Example 5 except that the arrangement of the barrier layer is different.

[0808] Fig.12 Schematic cross-sectional view showing a light guide plate for image display according to Example 6. Fig.13 Schematic cross-sectional view showing a light guide plate for image display according to Example 7.

[0809] The following description will focus on the differences from Example 5.

[0810] like Fig.12 As shown, in the image display light guide plate 2101 of Example 6, the first barrier layer 2002, the first resin substrate 2001, the hologram layer 2003, the second resin substrate 2005 and the second barrier layer 2004 are stacked in this order.

[0811] As the first barrier layer 2002 and the second barrier layer 2004, a silicon oxide thin film layer with a thickness of 50 nm similar to that of Example 5 was used.

[0812] When manufacturing the image display light guide plate 2101, an intermediate laminate is formed in the same manner as in Example 5. After that, a sealing layer is provided on the resin substrate of one intermediate laminate, and a photosensitive material is applied, and then another intermediate laminate is laminated so that the resin substrates face each other. Then, reduced pressure pressing and formation of a diffraction grating are performed in the same manner as in Example 5, thereby manufacturing the image display light guide plate 2101.

[0813] like Fig.13 As shown, the image display light guide plate 2102 of Example 7 is provided with a third blocking layer 2032 covering the entire side surface (the peripheral surface in the direction perpendicular to the thickness direction) of the image display light guide plate 2101 of Example 6, and other aspects are the same as Example 6.

[0814] The third barrier layer 2032 is formed of a silicon oxide thin film layer similar to the first barrier layer 2002 of the sixth embodiment.

[0815] The image display light guide plate 2102 is manufactured by forming a silicon oxide thin film layer on the side surface of the image display light guide plate 2101 after manufacturing the image display light guide plate 2101.

[0816] <Example 12>

[0817] In Example 12, the structure is the same as that of Example 4 except that each DLC film is formed of aluminum oxide with a thickness of 40 nm.

[0818] The following describes the substrate manufacturing process of Example 12, focusing on the differences from Example 4.

[0819] The image display light guide plate 2006 of Example 12 is manufactured by sequentially performing the same substrate preparation step as that of Example 4, the barrier layer formation step described later, and the light guide plate manufacturing step of Example 4.

[0820] (Barrier Layer Formation Step)

[0821] In the barrier layer forming step of this example, an aluminum oxide film is formed on the surface of the resin substrate.

[0822] The resin substrate and α-alumina particles with a purity of 99.999% and a particle size of 2 mm as a deposition source were placed in an electron beam deposition device in appropriate amounts and then evacuated. The distance from the deposition source to the shutter was about 8 cm, and the distance from the deposition source to the surface of the resin substrate was about 35 cm.

[0823] The pressure in the electron beam evaporation device reached 3×10 -3 After Pa, the filament current of the electron beam was increased to about 35mA, the shutter was opened, and aluminum oxide film was formed. After the temperature of the wall surface in the device reached 50°C, the shutter was closed to cut off the filament current of the electron beam. After cooling to below 30°C, the filament current of the electron beam was increased to about 35mA, the evaporation source was heated, the shutter was opened, and aluminum oxide film was formed. This operation was repeated to form an aluminum oxide film with a film thickness of 40nm.

[0824] The light guide plate manufacturing process of this embodiment is the same as the light guide plate manufacturing process of Embodiment 4 except that the intermediate laminate formed by the above-mentioned barrier layer forming process is used, and therefore the description thereof is omitted.

[0825] <Example 13>

[0826] In Example 13, the structure is the same as that of Example 4 except that each DLC film is formed of silicon oxide with a thickness of 70 nm.

[0827] The following describes the substrate manufacturing process of Example 13, focusing on the differences from Example 4.

[0828] The image display light guide plate 2006 of Example 13 is manufactured by sequentially performing the same substrate preparation step as in Example 4, the barrier layer formation step described later, and the same light guide plate manufacturing step as in Example 4.

[0829] (Barrier Layer Formation Step)

[0830] In the barrier layer formation process of this embodiment, silicon oxide is formed on the surface of the resin substrate. The resin substrate is placed in a plasma chemical vapor deposition device equipped with a high-frequency power supply (13.56MHz) and vacuum evacuated. After the pressure of the plasma chemical vapor deposition device reaches 1Pa, helium is used for bubbling, thereby introducing the generated tetraethoxysilane (TEOS) gas at a flow rate of 6sccm, and oxygen is introduced at a flow rate of 95sccm, and a silicon oxide film with a film thickness of 70nm is formed under the condition of a plasma generation setting power of 250W.

[0831] The barrier layer forming step is completed as described above.

[0832] The light guide plate manufacturing process of this embodiment uses the intermediate laminate formed in the above-mentioned barrier layer forming process, and is the same as the light guide plate manufacturing process of Example 4, so the description is omitted.

[0833] <Example 14>

[0834] In Example 14, the structure is the same as that of Example 4, except that the silicon oxide film is formed from silicon oxide with a thickness of 140 nm.

[0835] The following describes the substrate manufacturing process of Example 14, focusing on the differences from Example 4.

[0836] The image display light guide plate 2006 of Example 14 is manufactured by sequentially performing a substrate preparation step similar to that of Example 4, a barrier layer formation step described later, and a light guide plate manufacturing step similar to that of Example 4.

[0837] (Barrier Layer Formation Step)

[0838] In the barrier layer forming process of this embodiment, silicon oxide is formed on the surface of the resin substrate. The resin substrate is placed in a plasma chemical vapor deposition device equipped with a high-frequency power supply (13.56MHz) and vacuum evacuated. After the pressure of the plasma chemical vapor deposition device reaches 1Pa, helium gas is used for bubbling, thereby the generated TEOS gas is introduced at a flow rate of 6sccm, and oxygen is introduced at a flow rate of 95sccm, and a silicon oxide film with a film thickness of 140nm is formed under the condition of a plasma generation setting power of 250W.

[0839] The barrier layer forming step is completed as described above.

[0840] The light guide plate manufacturing process of this embodiment uses the intermediate laminate formed by the above-mentioned barrier layer forming process, and other than this, it is the same as the substrate manufacturing process of Example 4, so the description is omitted.

[0841] <Example 15>

[0842] In Example 15, the structure is the same as that of Example 4, except that the silicon oxide film is formed of silicon oxide with a thickness of 170 nm.

[0843] The following describes the substrate manufacturing process of Example 15, focusing on the differences from Example 4.

[0844] The image display light guide plate 2006 of Example 15 is manufactured by sequentially performing a substrate preparation step similar to that of Example 4, a barrier layer formation step described later, and a light guide plate manufacturing step similar to that of Example 4.

[0845] (Barrier Layer Formation Step)

[0846] In the barrier layer forming process of this embodiment, silicon oxide is formed on the surface of the resin substrate. The resin substrate is placed in a plasma chemical vapor deposition device equipped with a high-frequency power supply (13.56MHz) and vacuum evacuated. After the pressure of the plasma chemical vapor deposition device reaches 1Pa, helium gas is bubbled to introduce the generated TEOS gas at a flow rate of 6sccm, and oxygen gas is introduced at a flow rate of 95sccm, and a silicon oxide film with a film thickness of 170nm is formed under the condition of a plasma generation setting power of 250W.

[0847] The barrier layer forming step is completed as described above.

[0848] The light guide plate manufacturing process of this embodiment uses the intermediate laminate formed by the above-mentioned barrier layer forming process, and other than this, it is the same as the substrate manufacturing process of Example 4, so the description is omitted.

[0849] <Example 16>

[0850] Example 16 has the same structure as Example 14 except that the barrier layer has an auxiliary layer.

[0851] The following describes the substrate manufacturing process of Example 16, focusing on the differences from Example 14.

[0852] The image display light guide plate 2006 of Example 16 is manufactured by sequentially performing the same substrate preparation step as in Example 4, the barrier layer formation step described later, and the same light guide plate manufacturing step as in Example 4.

[0853] (Barrier Layer Formation Step)

[0854] In the barrier layer forming step of this example, an auxiliary layer was formed on the surface of the inorganic material layer prepared by the same method as in Example 14. N-phenyl-3-aminopropyltrimethoxysilane (KBM-573, Shin-Etsu Chemical Co., Ltd.) was added to an aqueous solution of ethylene-vinyl alcohol copolymer so that the solid content concentration was 10 wt % relative to the total solid content in the protective coating layer to prepare an auxiliary coating agent 1. The auxiliary coating agent 1 was applied to the surface of the inorganic material layer and dried to form an auxiliary layer with a thickness of 0.5 μm.

[0855] The barrier layer forming step is completed as described above.

[0856] The light guide plate manufacturing process of this embodiment uses a barrier layer having a multi-layer structure formed by the above-mentioned barrier layer forming process. Other than this, the process is the same as the substrate manufacturing process of Example 4, and thus the description thereof is omitted.

[0857] <Example 17>

[0858] In Example 17, the barrier layer has the same structure as that of Example 14, except that the barrier layer has a fluorine-based water-repellent and moisture-proof coating as an auxiliary layer.

[0859] The following describes the substrate manufacturing process of Example 17, focusing on the differences from Example 14.

[0860] The image display light guide plate 2006 of Example 17 is manufactured by sequentially performing a substrate preparation step similar to that of Example 4, a barrier layer formation step described later, and a light guide plate manufacturing step similar to that of Example 4.

[0861] (Barrier Layer Formation Step)

[0862] In the protective layer forming step of this example, a fluorine-based water-repellent and moisture-proof coating is formed on the surface of the barrier layer produced by the same method as in Example 14.

[0863] The barrier layer forming step is completed as described above.

[0864] The substrate manufacturing process of this embodiment uses a barrier layer having a multilayer structure formed by the above-mentioned barrier layer forming process. Except for this, the substrate manufacturing process of this embodiment is the same as that of Embodiment 4, and thus the description thereof is omitted.

[0865] <Example 18>

[0866] In Example 18, the structure is the same as that of Example 14 except that an anchor coating layer is disposed between the barrier layer and the resin substrate.

[0867] The following is an explanation of the substrate manufacturing process of Example 18, focusing on the differences from Example 14.

[0868] The image display light guide plate 2006 of Example 18 is manufactured by sequentially performing the same substrate preparation step as in Example 14, the anchor coat layer formation step and the barrier layer formation step described later, and the same light guide plate manufacturing step as in Example 4.

[0869] (Anchor Coat Formation Step)

[0870] In the anchor coating formation step of this embodiment, an anchor coating is formed on the surface of a resin substrate. A saturated polyester (Vylon 300 manufactured by Toyobo Co., Ltd.) and an isocyanate compound (CORONETL manufactured by Tosoh Corporation) are mixed at a mass ratio of 1:1 to prepare an anchor coating agent. The anchor coating agent is applied and dried on the corona-treated surface of the resin substrate to form an anchor coating layer having a thickness of 100 nm.

[0871] The anchor coating process is completed as described above.

[0872] (Barrier Layer Formation Step)

[0873] A barrier layer was formed on the anchor coating layer using the same method as in Example 14.

[0874] The light guide plate manufacturing process of this embodiment uses an intermediate laminate formed by the above-mentioned anchor coat layer forming process and barrier layer forming process. Other than this, the process is the same as the substrate manufacturing process of Embodiment 4, and thus the description thereof is omitted.

[0875] <Example 19>

[0876] In Example 19, the structure is the same as that of Example 16 except that an anchor coating layer is disposed between the barrier layer and the resin substrate.

[0877] The following is an explanation of the substrate manufacturing process of Example 19, focusing on the differences from Example 16.

[0878] The image display light guide plate 2006 of Example 19 is manufactured by sequentially performing the same substrate preparation step as in Example 4, the anchor coating layer forming step, the inorganic material layer forming step and the barrier layer forming step described later, and the same light guide plate manufacturing step as in Example 4.

[0879] (Anchor Coat Formation Step)

[0880] An anchor coating layer was formed on the surface of the resin substrate by the same method as in Example 18.

[0881] (Inorganic Material Layer Formation Step)

[0882] An inorganic material layer was prepared on the anchor coating layer using the same method as in Example 14.

[0883] (Barrier Layer Formation Step)

[0884] An auxiliary layer is prepared on the surface of the above-mentioned inorganic material layer using the same method as in Example 16 to form a barrier layer.

[0885] The light guide plate manufacturing process of this embodiment uses an intermediate laminate formed by the above-mentioned anchor coating layer forming step, inorganic material layer forming step and barrier layer forming step. Other than this, the process is the same as the substrate manufacturing process of Example 4, and thus the description is omitted.

[0886] <Example 20>

[0887] In Example 20, the structure is the same as that of Example 4, except that each silicon oxide film is formed by sputtering to have a thickness of 100 nm and is made of silicon oxide.

[0888] The following describes the substrate manufacturing process of Example 20, focusing on the differences from Example 4.

[0889] The image display light guide plate 2006 of Example 20 is manufactured by sequentially performing the same substrate preparation step as in Example 4, the barrier layer formation step described later, and the same light guide plate manufacturing step as in Example 4.

[0890] (Barrier Layer Formation Step)

[0891] In the barrier layer forming step of this embodiment, a silicon oxide film is formed on the surface of the resin substrate by sputtering at a vacuum pressure of 4.0×10 -5 A silicon oxide film having a film thickness of 100 nm was formed under a vacuum pressure of 0.1 Torr.

[0892] The light guide plate manufacturing process of this embodiment uses the intermediate laminate formed by the above-mentioned barrier layer forming process, and other than this, it is the same as the substrate manufacturing process of Example 4, so the description is omitted.

[0893] <Example 21>

[0894] In Example 21, the structure is the same as that of Example 20 except that an anchor coating layer is disposed between the barrier layer and the resin substrate.

[0895] The following describes the substrate manufacturing process of Example 21, focusing on the differences from Example 20.

[0896] The image display light guide plate 2006 of Example 21 is manufactured by sequentially performing the same substrate preparation step as Example 20, the same anchor coating formation step as Example 18, the barrier layer formation step described later, and the same light guide plate manufacturing step as Example 20.

[0897] (Barrier Layer Formation Step)

[0898] A barrier layer was formed on the anchor coating layer using the same method as in Example 20.

[0899] The light guide plate manufacturing process of this embodiment uses an intermediate laminate formed by the above-mentioned barrier layer forming process. Other than this, it is the same as the substrate manufacturing process of Example 20, so the description is omitted.

[0900] <Evaluation method>

[0901] Next, the evaluation method of each example is described. As the evaluation, brightness value measurement, FOV evaluation, and display image clarity evaluation are performed.

[0902] (Brightness value)

[0903] Regarding the samples for measuring the brightness values, three types of samples were prepared: samples subjected to a humidity test ("after humidification" in Table 2C), samples subjected to a heating test ("after heating" in Table 2C), and samples subjected to neither a humidity test nor a heating test ("initial" in Table 2C).

[0904] The humidity test and the heating test were conducted using a small environmental tester SH-241 (trade name; manufactured by Espec Corporation).

[0905] The test conditions of the humidity test were 60° C., 90% RH, and 500 hours.

[0906] The test conditions of the heating test were 85° C. and 500 hours.

[0907] The brightness value of the measurement sample is measured based on the above-mentioned measurement method in the embodiment.

[0908] Each measurement sample was installed in the above-mentioned display device.

[0909] A luminance meter BM-8 (trade name; manufactured by Topcon Co., Ltd.) was used as the luminance meter 2014. The measurement angle was 1°, and the distance d from the display surface 2003a was 15 mm.

[0910] When the brightness value was 3500 nit or more, it was judged as very good (described as "S" in Table 2C).

[0911] When the brightness value was 3000 nit or more and less than 3500 nit, it was judged as good (good, described as "A" in Table 2C).

[0912] When the brightness value was 1000 nit or more and less than 3000 nit, it was judged as fair (described as "B" in Table 2C).

[0913] When the brightness value was less than 1000 nit, it was judged as unacceptable (no good, recorded as "C" in Table 2C).

[0914] (FOV)

[0915] The measurement of FOV was performed using a display device equipped with a sample for measuring the brightness value on which neither the humidity test nor the heating test was performed.

[0916] The FOV is measured based on the above-mentioned measurement method in the embodiment.

[0917] A luminance meter BM-8 (trade name; manufactured by Topcon Co., Ltd.) was used as the luminance meter 2014. The measurement angle was 1°, and the distance d from the display surface 2003a was 15 mm.

[0918] When the FOV was 45° or more, it was judged as very good (described as "S" in Table 2C).

[0919] When the FOV was 35° or more and less than 45°, it was judged as good (good, described as "A" in Table 2C).

[0920] When the FOV was 24° or more and less than 35°, it was judged as fair (described as "B" in Table 2C).

[0921] When the FOV is less than 24°, it is judged as unacceptable (no good, recorded as "C" in Table 2C).

[0922] (Clarity)

[0923] The clarity of the displayed image is measured using the display device used for the FOV measurement.

[0924] As input images used for evaluation, a white image and a text display image were used.

[0925] The evaluation was performed by visually judging the visual effects of the white image and the text display image. As the text image, "ABCDE" was displayed within a size of 10 mm×100 mm.

[0926] When no rainbow color was seen in the white image and the characters in the character display image were clearly visible, it was judged as good (good, recorded as "A" in Table 2C).

[0927] When a slight rainbow color was observed in the white image and the characters in the character display image were clearly visible, it was judged as fair (described as "B" in Table 2C).

[0928] When rainbow color was observed in at least a part of the white image and the outline of the characters was observed vaguely in the character display image, it was determined as unacceptable (no good, described as "C" in Table 2C).

[0929] <Evaluation Results>

[0930] As shown in Table 2C, the brightness values ​​of Examples 4 and 5 and Examples 12 to 21 were all evaluated as "S" or "A" regardless of whether the humidity test and the heating test were performed.

[0931] This is considered to be because, in these embodiments, the barrier layer prevents moisture from penetrating into the hologram layer and the hologram layer from corroding the resin substrate, resulting in good diffraction performance of the hologram layer without causing disturbance of the optical path in the resin substrate.

[0932] Furthermore, in these examples, the hologram layer is not in contact with the resin substrate, so that even if heated, the material of the hologram layer does not corrode the resin substrate.

[0933] In contrast, the brightness values ​​of Examples 5 and 6 were inferior to those of Examples 4, 5, and Examples 12 to 21 in the measurement samples after either the humidity test or the heating test, but were evaluated as "B" without the humidity test or the heating test, which was a practical level.

[0934] As shown in Table 2C, the FOVs of Examples 4 and 5 and Examples 12 to 21 were evaluated as "S" and "A", respectively.

[0935] On the other hand, the FOV of Examples 6 and 7 was evaluated as "B", which is a practical level.

[0936] The reason is believed to be the same as the reason for the difference in the brightness value evaluation described above. That is, in Examples 4, 5 and Examples 12 to 21, the barrier layer can prevent moisture from penetrating into the holographic layer and corroding the resin substrate to a very high level, and as a result, no reduction in FOV is observed.

[0937] It is believed that the FOV of Example 4 is better than that of Example 5 because of the difference in the material of the barrier layer. It is believed that the DLC film has a higher refractive index than the silicon oxide thin film layer, so the FOV is increased and improved.

[0938] Furthermore, the clarity of the displayed images of Examples 4 and 5 and Examples 12 to 21 (“clarity” in Table 2C) were all judged as “A”, which was a better result than that of Examples 6 and 7.

[0939] The reason is believed to be the same as the reason for the difference in the brightness value evaluation described above. That is, in Examples 4 and 5 and Examples 12 to 21, the barrier layer can prevent water penetration into the hologram layer and corrosion of the resin substrate to a very high level, and as a result, clear images are observed.

[0940] [Example of the third embodiment]

[0941] Next, an example of the third embodiment will be described.

[0942] <Example 8>

[0943] (Preparation of First Substrate and Second Substrate)

[0944] Two acrylic resin plates (manufactured by Mitsubishi Chemical Corporation) processed into 60 mm × 60 mm × 1 mm (thickness) were immersed in a 5% surfactant aqueous solution of Semi Clean M-L0 (manufactured by Yokohama Oil & Fats Industry Co., Ltd.) and ultrasonically cleaned for 5 minutes. Then, ultrasonically cleaned for 5 minutes while immersed in ultrapure water. Further rinsed with ultrapure water, air-dried, and dried in a 100°C oven under a nitrogen atmosphere. Then, the air-dried substrates were UV-ozone cleaned for 1 minute using a UV ozone cleaner to prepare the first substrate and the second substrate.

[0945] (Formation of holographic layer)

[0946] The holographic layer is common in each embodiment. As the material of the holographic layer, 100 parts by mass of bisphenol epoxy resin (polymerization degree n=10.8, epoxy equivalent: 1750-2200, trade name jER1007 manufactured by Mitsubishi Chemical Corporation), 50 parts by mass of triethylene glycol diacrylate, 5 parts by mass of 4,4'-bis(tert-butylphenyl)iodonium hexafluorophosphate, and 0.5 parts by mass of 3,3'-carbonylbis(7-diethylamino)coumarin were mixed and dissolved in 100 parts by mass of 2-butanone to serve as a photosensitive material for the hologram.

[0947] A sealing layer with a width of 5 mm and a thickness of 5 μm was applied to the periphery of the second substrate. The photosensitive material forming the holographic layer was applied to the 50 mm × 50 mm opening surrounded by the sealing layer by spin coating so that the thickness after drying was 5 μm. After the photosensitive material was dried, the first substrate was laminated and pressed under reduced pressure (absolute pressure 5 kPa, temperature 70°C, pressing pressure 0.04 MPa).

[0948] The first substrate and the second substrate sealed with the photosensitive material are kept at 20°C and irradiated with two kinds of lasers. Interference fringes are formed by adjusting the irradiation angle and intensity of each laser, and the desired diffraction grating is recorded on the photosensitive material to form a hologram layer.

[0949] (Preparation of hard coating)

[0950] As a film substrate, a biaxially oriented polyethylene terephthalate film manufactured by Mitsubishi Chemical Corporation (product name: "Diafoil T612 type", thickness: 50 μm) was prepared.

[0951] A curable composition for forming a hard coat layer was prepared using an organic-inorganic hybrid ultraviolet curable resin composition (UVHC7800G manufactured by MOMENTIVE, content of inorganic silica having a reactive functional group: 30-40% by mass). The refractive index of the cured resin layer formed by curing the composition was 1.54.

[0952] The curable composition was applied to the second surface of the film substrate using a bar coater so that the film thickness after drying was 3 μm, and then heated at 90° C. for 1 minute to dry. 2 ) Accumulated light dose 400mJ / cm 2 Ultraviolet rays form a hard coating.

[0953] Next, a coating liquid for forming a release layer having the following composition was applied on the hard coat layer and dried to form a release layer. The thickness of the obtained release layer was 500 nm.

[0954] Release agent: 10 parts by mass of an alkyd resin containing a long-chain alkyl group ("Tesfine" 303 manufactured by Hitachi Chemical Co., Ltd.) (based on solid content)

[0955] Acid catalyst p-toluenesulfonic acid ("Dryer" 900 manufactured by Hitachi Chemical Co., Ltd.) 0.12 parts by mass (based on solid content)

[0956] Solvent toluene 45 parts by mass

[0957] Next, the adhesive-forming composition was applied on the first surface of the film substrate so that the film thickness after drying would be 0.5 μm, and dried to form an adhesive layer.

[0958] The adhesive-forming composition was prepared as follows.

[0959] To 1 kg of an adhesive solution formed from an acrylic copolymer (SK-DYNE1882 manufactured by Soken Chemical Co., Ltd., with a solid content concentration of approximately 17%), 1.85 g of an isocyanate crosslinking agent (L-45 manufactured by Soken Chemical Co., Ltd.) and 0.5 g of an epoxy crosslinking agent (E-5XM manufactured by Soken Chemical Co., Ltd.) were added and mixed uniformly.

[0960] The adhesive layer of the obtained hard coat film was bonded to the first substrate, and the hard coat film was attached to the first substrate, thereby obtaining a light guide plate for image display of Example 8.

[0961] <Example 9>

[0962] In Example 9, only the structure of the hard coating film was different. The method of preparing the hard coating film is shown below.

[0963] A release layer, a hard coat layer and an adhesive layer were formed on a process release film (MRA100 manufactured by Mitsubishi Chemical Corporation, thickness 100 μm) in the same manner as above, and the adhesive layer was bonded to the first substrate. The process release film was peeled off after ultraviolet irradiation to obtain the image display light guide plate of Example 9.

[0964] <Evaluation method>

[0965] The following evaluations were performed on each example.

[0966] (Image display clarity)

[0967] Three light guide plates of each example are prepared, and after forming holographic layers in a manner that diffracts light in the red, green, and blue wavelength regions, the three light guide plates are stacked. An image display device, an optical system that inputs displayed information to the light guide plates, and a circuit system that drives a power supply and supplies image information are attached to the stacked light guide plates to assemble the image display device of each example.

[0968] An image having characters written on a white background was displayed on the light guide plate. The displayed image was visually observed from the first substrate side, and sensitivity evaluation was performed using the following three levels.

[0969] A (good): There is no rainbow-colored part in the image, and the text is clearly visible.

[0970] B (average): There is a slight rainbow-colored portion in the image, but the text is clearly visible

[0971] C (bad): There are parts that are clearly observed to be rainbow-colored in the image, and the outline of the text also looks blurred.

[0972] The clarity was evaluated before and after the scratch resistance evaluation described below. In Examples 8 and 9, the hard coating film was peeled off after the scratch resistance evaluation, and a new hard coating film was attached before the evaluation.

[0973] (Damage resistance)

[0974] For the surface of the hard coating film or hard coating layer on the outermost surface of the image display device of each example, steel wool #0000 attached to the cross section of a cylinder with a diameter of 11 mm was reciprocated 10 times under the conditions of a load of 400 g and 100 mm / second. Thereafter, the state of the hard coating film or hard coating layer surface was observed within a test range of 100 mm in length and 20 mm in width, and judged according to the following three levels.

[0975] A (good): no scratches

[0976] B (average): less than 20 scars

[0977] C (bad): 20 or more scars

[0978] (Drop resistance)

[0979] A steel ball with a diameter of 50 mm and a weight of 230 g was dropped to collide with the outermost surface of the image display device of each example. Thereafter, cracks of the first substrate and the second substrate were confirmed. The evaluation was made into the following two levels.

[0980] A (good): No cracks were observed in either the first substrate or the second substrate.

[0981] C (bad): Cracks were observed in at least one of the first substrate and the second substrate.

[0982] (Pencil hardness)

[0983] The pencil hardness of the measured surface was measured under a load of 750 g in accordance with JIS K 5600-5-4:1999.

[0984] Table 3 shows the results of each evaluation.

[0985]

[0986] In Examples 8 and 9, scratches occurred on the hard coating film or hard coating layer during the scratch resistance evaluation. By re-attaching the hard coating film, the situation where the scratches deteriorate the clarity can be prevented. Regarding the light guide plate for image display of each example, the substrate made of resin did not crack during the drop resistance evaluation, so it is highly safe when used in eyeglass-type displays.

[0987] In the light guide plate of the third embodiment of the present invention, the second substrate may be made of glass instead of resin. Even in such a configuration, by configuring a glasses-type display with the first substrate facing the wearer, it is possible to achieve weight reduction and improve the safety of the wearer.

[0988] In the light guide plate of the present invention, a hard coating film may be provided on the second substrate. In this case, the hard coating films on the first substrate and the second substrate may have different structures and the number of overlapping sheets.

[0989] [Example of the fourth embodiment]

[0990] Next, Examples 9 and 10 of the fourth embodiment will be described. The present invention is not limited to these Examples.

[0991] Table 4 below shows the configurations of the resin substrate and the absorption layer in each example and the evaluation results.

[0992]

[0993] <Example 10>

[0994] Example 10 is an example corresponding to the image display light guide plate 4005 of the fourth embodiment.

[0995] As shown in Table 4, acrylic resin (PMMA) was used as the material of the first resin substrate 4001 and the second resin substrate 4003 (“resin substrate” in Table 4).

[0996] The first resin base material 4001 and the second resin base material 4003 are both in the shape of a rectangular plate of 60 mm×60 mm×1 mm.

[0997] The hologram layer 4002 is common in each embodiment. As the material of the hologram layer 4002, 100 parts by mass of bisphenol epoxy resin jER (registered trademark) 1007 (polymerization degree n = 10.8, epoxy equivalent: 1750-2200, trade name of Mitsubishi Chemical), 50 parts by mass of triethylene glycol diacrylate, 5 parts by mass of 4,4'-bis (tert-butylphenyl) iodonium hexafluorophosphate, and 0.5 parts by mass of 3,3'-carbonylbis (7-diethylamino) coumarin are mixed and dissolved in 100 parts by mass of 2-butanone, and used as a photosensitive material for the hologram. The thickness of the hologram layer 4002 is 5 μm. The size of the hologram layer 4002 in a plan view is 50 mm × 50 mm.

[0998] Next, a description will be given of a manufacturing process of the image display light guide plate 4005 in Example 10. The image display light guide plate 4005 is manufactured by sequentially performing a substrate preparation process, an absorption layer formation process, and a light guide plate manufacturing process described below.

[0999] (Substrate preparation process)

[1000] In the substrate preparation step, the first resin substrate 4001 and the second resin substrate 4003 are cleaned and dried. Hereinafter, when it is not necessary to distinguish between the first resin substrate 4001 and the second resin substrate 4003, the symbols are omitted and they are simply described as resin substrates.

[1001] The resin substrate was immersed in a 5% surfactant aqueous solution of Semi Clean (registered trademark) M-LO (trade name; manufactured by Yokohama Oil & Fats Industries, Ltd.) as a neutral cleaning agent, and ultrasonic cleaning was performed for 5 minutes.

[1002] After that, the resin substrate was immersed in ultrapure water and ultrasonically cleaned for 5 minutes. The resin substrate was further rinsed with ultrapure water, and then air-dried and dried in an oven at 100° C. under a nitrogen atmosphere. After that, the air-dried evaluation sample B was UV-ozone cleaned for 1 minute using a UV ozone cleaner.

[1003] The substrate preparation process is completed as described above.

[1004] (Absorption layer forming step)

[1005] In the absorption layer forming step, a first absorption layer 4004 (“absorption layer” in Table 4) is formed on the surface of the first resin substrate 4001 .

[1006] To 100 parts by mass of acrylate (Upimer (registered trademark) UV-HH2100 (trade name; manufactured by Mitsubishi Chemical Corporation)) were added 5 parts by mass of a photopolymerization initiator and 0.05 parts by mass of Diaresin (registered trademark) blue as a colorant to prepare a curable resin composition (coating liquid).

[1007] The curable resin composition was applied onto the first resin substrate 4001 using a metal bar coater, dried at 90° C. for 1 minute, and then irradiated with ultraviolet light at 500 mJ / cm 2 The film was exposed at an exposure dose of 1000 to obtain a laminate having an absorbing layer with a thickness of 5 μm.

[1008] The absorption layer forming step is completed as described above.

[1009] Hereinafter, the resin substrate on which the absorption layer is formed is referred to as an intermediate laminate.

[1010] (Light guide plate manufacturing process)

[1011] In the light guide plate manufacturing step, the image display light guide plate 4005 is manufactured using the intermediate laminate and the second resin substrate 4003 .

[1012] A sealing layer having a width of 5 mm and a thickness of 5 μm was applied to the peripheral portion of the surface of the intermediate laminate on the side opposite to the absorbing layer.

[1013] The sealing layer is formed of a transparent material and is not particularly limited as long as it can bond the resin substrates to each other. In Example 1, optical adhesive Hard Lock (registered trademark) OP-1045K (trade name; manufactured by Denki Kagaku Kogyo Co., Ltd.) was used.

[1014] In this way, an intermediate laminate with a sealant layer step having an opening surrounded by the sealant layer and a size of 50 mm×50 mm was prepared.

[1015] Then, the photosensitive material as a photopolymer material for hologram was applied on the intermediate laminate by spin coating. The photosensitive material was applied so as to have a thickness of 5 μm after drying.

[1016] Then, the second resin substrate 4003 was laminated on the sealing layer and the photosensitive material so as to face the barrier layer of the intermediate laminate with sealing layer, and pressed under reduced pressure. The pressing conditions were absolute pressure 5 kPa, temperature 70° C., and pressing pressure 0.04 MPa.

[1017] After that, a diffraction grating is recorded on the photosensitive material of the laminated body after being pressed and bonded. In this process, the temperature of the laminated body is maintained at 20°C. As for the diffraction grating, two kinds of lasers are irradiated to the laminated body, and the irradiation angle and intensity of each are adjusted, thereby forming interference fringes in a manner of forming a desired diffraction pattern. Thus, the diffraction grating is recorded on the photosensitive material.

[1018] As a specific diffraction grating, the diffraction grating diffracts each light of red, green, and blue wavelength regions incident as image light incident on the incident portion, and forms a diffraction grating for color display emitted from the display portion at a position corresponding to a pixel of the image light.

[1019] Thereafter, the laminate was kept at 20° C. and irradiated with ultraviolet light (wavelength 365 nm, irradiance 80 W / cm 2 ). As a light source of ultraviolet light, a high pressure mercury lamp is used.

[1020] The sealing layer is thereby cured, thereby forming the image display light guide plate 4005 of Example 1.

[1021] <Example 11>

[1022] Example 11 is an example corresponding to the image display light guide plate 4007 of the first modified example of the fourth embodiment.

[1023] As shown in Table 4, in Example 11, absorption layers are provided on both surfaces. Specifically, the second absorption layer 4006 is formed on the surface of the second resin substrate 4003 opposite to the hologram layer 4002 .

[1024] In this example, the second absorption layer 4006 ("absorption layer" in Table 4) is configured similarly to the first absorption layer 4004 of Example 10.

[1025] Therefore, the substrate preparation process of Example 11 is the same as that of Example 10.

[1026] The absorbent layer forming step of Example 11 is different from Example 10 in that, in addition to forming an intermediate laminate having a first absorbent layer 4004, an intermediate laminate composed of a second resin substrate 4003 having a second absorbent layer 4006 is formed.

[1027] The eleventh embodiment is different from the tenth embodiment in that two intermediate laminates are used in the light guide plate manufacturing process.

[1028] <Evaluation method>

[1029] Next, the evaluation method of each example is described. As the evaluation, clarity evaluation was performed.

[1030] (Clarity Evaluation)

[1031] The clarity of the displayed image is improved by each display device using each image display light guide plate. Each display device has the same configuration as the display device 4010 except that the image display light guide plate of each embodiment is used.

[1032] As images used for evaluation, a display image based on image light diffracted by the hologram layer and an external light image through which external light is transmitted are used.

[1033] As input images for displaying images, a white image and a text image are used.

[1034] As the ambient light image, a scene of a room, a street, or a forest at a distance of 0.5 m to 50 m from the display device was used. In the evaluation of the ambient light image, a white image or a text image was displayed and evaluated.

[1035] The visual effects of the white image and the character image and the visual effect of the external light image are visually evaluated. The character image is represented by hiragana, katakana, kanji, Arabic numerals or letters in a size converted to a visual acuity of 0.1 to 2.0.

[1036] (Criteria for evaluating the clarity of displayed images)

[1037] The clarity of the displayed image was evaluated in three levels.

[1038] When no rainbow color was seen in the white image and the characters in the character image were clearly visible, it was judged as good (good, described as "A" in Table 4).

[1039] When a slight rainbow color was observed in the white image and the characters in the character image were clearly visible, it was judged as fair (described as "B" in Table 4).

[1040] When rainbow color was observed in at least a part of the white image and the outline of the characters was observed vaguely in the character image, it was determined as unacceptable (no good, described as "C" in Table 4).

[1041] (Criteria for evaluating the clarity of ambient light images)

[1042] The clarity of the external light image was evaluated in 4 levels.

[1043] When the color tone of the scenery in the ambient light image was not uncomfortable and was clearly visible, it was judged as very good (described as "S" in Table 4).

[1044] When the scene in the ambient light image was observed to be slightly dark, it was determined to be good (good, described as "A" in Table 4).

[1045] When the scenery in the ambient light image is dark and the color tone is slightly uncomfortable, it is judged as fair (described as "B" in Table 4).

[1046] If the scene based on the external light image looks blurry, it is determined to be unacceptable (no good, described as "C" in Table 4).

[1047] (Weather resistance test)

[1048] As the light guide plates for image display used for the clarity evaluation, samples subjected to the weather resistance test ("after the weather resistance test" in Table 4) and samples not subjected to the weather resistance test ("before the weather resistance test" in Table 4) were prepared.

[1049] The weather resistance test was performed using an ultraviolet fading meter U48AU (trade name; manufactured by SUGA TEST INSTRUMENTS Co., Ltd.) The test conditions were set at a BP temperature of 63° C.±3° C. The test time was set at 500 hours.

[1050] <Evaluation Results>

[1051] As shown in Table 4, the clarity of Example 10 was evaluated as "A" for both the displayed image and the ambient light image before and after the weathering test. The clarity of Example 11 was evaluated as "A" except for the ambient light image which was "S" before the weathering test.

[1052] From the evaluation results, it can be seen that the display image and the external light image have good clarity due to the presence of the absorption layer in Examples 10 and 11. In particular, in Example 10, since the absorption layer is also provided on the incident side of the external light, the clarity of the external light image is improved compared with Example 10 before the weather resistance test.

[1053] Although the preferred embodiments and examples of the present invention have been described above, the present invention is not limited to these embodiments and examples, and additions, omissions, substitutions, and other changes to the configuration may be made without departing from the spirit of the present invention.

[1054] It should be noted that the present invention is not limited by the above description but is limited only by the claims.

[1055] Industrial Applicability

[1056] The image display light guide plate of the present invention can display a clear image even when a resin substrate is used, and can suppress the degradation of the holographic layer, and is useful in display device applications such as VR and AR applications. For example, the image display light guide plate of the present invention is useful in display device applications such as entertainment activities, remote operation, work support, and guidance support using a head-up display, a wearable display, or a head-mounted display.

[1057] Explanation of symbols

[1058] 1001 No.1 resin base material

[1059] 1001a1st surface

[1060] 1001b Surface 2

[1061] 1002 Holographic Layer

[1062] 1003 2nd resin base material

[1063] 1004,1014 Light guide plate for image display

[1064] 1011A 1st hard coating

[1065] 1011B Second hard coating

[1066] 1100 Continuous Polymerization Unit

[1067] 1101,1102 Annular belt

[1068] 1103,1104,1105,1106 Main pulley

[1069] 1107 Carrier Roller

[1070] 1108 1st Polymerization Zone

[1071] 1109 hot water spray

[1072] 1110 Second Polymerization Zone

[1073] 1111 Downstream cooling zone

[1074] 1112 Gasket

[1075] 1113 Plate-like polymer

[1076] 1114 Raw material injection device

[1077] 1200 Evaluation device

[1078] 1201 Light Source

[1079] 1202 Screen

[1080] 1203 Camera

[1081] 1204 Calculation Processing Unit

[1082] 1210 Curve

[1083] 2001 No.1 resin substrate

[1084] 2002 No.1 Barrier

[1085] 2003 Holographic Layer

[1086] 2003a Display surface

[1087] 2003b Waveguide Diffraction Grating Division

[1088] 2003c Diffraction grating for display

[1089] 2004 Barrier 2

[1090] 2005 No. 2 Resin Base Material

[1091] 2006,2016Light guide plate for image display

[1092] 2006a Incident

[1093] 2006d Display Department

[1094] 2010 Display Devices

[1095] 2012 Incident Optical System

[1096] 2013 Image Light Projection Department

[1097] 2014 Luminance Meter

[1098] 2015 Measurement Device

[1099] 2022 No.1 Barrier Film

[1100] 2022A Barrier layer

[1101] 2022B Resin Film

[1102] 2024 2nd Barrier Film

[1103] 2024A Barrier layer

[1104] 2024B resin film

[1105] 20261st bonding layer

[1106] 2027 2nd bonding layer

[1107] 2032 3rd barrier layer

[1108] 2101,2102 Light guide plate for image display

[1109] 3001 Light guide plate for image display (light guide plate)

[1110] 3010 Holographic Layer

[1111] 3021 First Substrate

[1112] 3022 Second substrate

[1113] 3030,3130 hard coating

[1114] 3030A,3130A first hard coating

[1115] 3030B,3130B second hard coating

[1116] 3031 Film substrate

[1117] 3031a Page 1

[1118] 3031b Side 2

[1119] 3032 Adhesive layer

[1120] 3033 Hard Coating

[1121] 3034 Anti-sticking layer

[1122] 4001 No.1 resin base material

[1123] 4002 Holographic Layer

[1124] 4002b Diffraction grating unit for display

[1125] 4003 2nd resin base material

[1126] 4003a Waveguide diffraction grating unit

[1127] 40041st Absorption Layer

[1128] 4005,4007,4020,4024 Light guide plate for image display

[1129] 4005a Incident part

[1130] 4005b Display image emitting unit

[1131] 4006 2nd Absorption Layer

[1132] 4008 1st barrier layer

[1133] 4009 2nd barrier layer

[1134] 4010 Display Device

[1135] 4011 Incident Optical System

[1136] 4012 Image Light Projection Department

[1137] 4021 1st resin substrate (absorption layer)

[1138] 4023 Second resin substrate (absorption layer)

[1139] I Transmission Projection Image

[1140] Ib High brightness part

[1141] Is Low brightness part

[1142] Ld Image Light

[1143] Ld' Image Light

[1144] Ld" image light

[1145] Li image light

[1146] Lo outside light

[1147] Lo' exterior light

[1148] Lo" exterior light

[1149] Lo"'outdoor light

[1150] O optical axis

[1151] P1 The first intermediate laminate

[1152] P2 Second intermediate laminate

[1153] S determination sample

Claims

1. A light guide plate for image display, comprising a first resin substrate and a holographic layer, in, The first resin substrate has an MC value of 0.120 or less as determined by dark tone contrast evaluation, and an arithmetic mean roughness Ra of the surface of 5 nm or less. 2 . The image display light guide plate according to claim 1 , further comprising a first barrier layer.

3. The image display light guide plate according to claim 2, in, The first resin substrate, the first barrier layer, and the holographic layer are arranged in this order in the thickness direction.

4. The image display light guide plate according to claim 3, in, The light guide plate further comprises a second resin substrate and a second barrier layer. The first resin substrate, the first barrier layer, the holographic layer, the second barrier layer, and the second resin substrate are arranged in order in the thickness direction.

5. The image display light guide plate according to any one of claims 2 to 4, in, The refractive index of the first barrier layer is higher than the refractive index of the first resin substrate.

6. The image display light guide plate according to any one of claims 2 to 5, in, The refractive index of the first barrier layer is greater than or equal to 1.

48.

7. The image display light guide plate according to any one of claims 2 to 6, in, The first barrier layer includes an inorganic material.

8. The light guide plate for image display according to claim 7, in, The first barrier layer includes at least one inorganic material selected from the group consisting of silicon oxide, silicon oxynitride, diamond-like carbon, aluminum oxide, and glass.

9. The image display light guide plate according to any one of claims 2 to 8, in, The first barrier layer is disposed on the resin film.

10. The image display light guide plate according to any one of claims 2 to 9, in, As the material of the first barrier layer, a water vapor barrier material is used.

11. The image display light guide plate according to any one of claims 2 to 10, in, The first barrier layer is disposed on the holographic layer.

12. The image display light guide plate according to any one of claims 1 to 11, in, The refractive index of the first resin substrate is 1.48 to 1.

70.

13. The image display light guide plate according to any one of claims 1 to 12, in, The first resin substrate includes at least one resin selected from the group consisting of poly(meth)acrylic resins, epoxy resins, cyclic polyolefins, and polycarbonates.

14. The image display light guide plate according to any one of claims 1 to 13, in, The first resin substrate has a heat shrinkage rate of less than 3% as measured in accordance with Appendix A of JIS K 6718-1:2015.

15. The image display light guide plate according to any one of claims 1 to 14, in, The MC value is 0.070 or less.

16. The image display light guide plate according to any one of claims 2 to 15, in, The first barrier layer has an auxiliary layer. 17 . AR glasses comprising the image display light guide plate according to claim 1 .