Method for optimizing energy storage performance of all-organic composite dielectric thin film based on asymmetric heterostructure

By designing an all-organic composite dielectric film with asymmetric heterostructure in dielectric capacitors, using the combination of ferroelectric polymer and linear dielectric polymer, the problems of low energy storage density and breakdown strength are solved, and high-efficiency energy storage and Combination of high discharge efficiency.

CN118969506APending Publication Date: 2024-11-15HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411009771.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing dielectric capacitors have low energy storage density, low breakdown strength, and low dielectric constant of linear dielectric materials, and poor polarization strength and energy storage capacity.

Method used

Design an all-organic composite dielectric film based on asymmetric heterostructure, including an insulating layer, a transition layer and a polarization layer. The insulating layer is a ferroelectric polymer, the polarization layer is a linear dielectric polymer, and the transition layer is a ferroelectric polymer. A mixture of substance and linear dielectric polymer provides high energy density through polarization layer, intermediate transition layer homogenizes electric field, and linear dielectric layer provides high discharge efficiency.

Benefits of technology

It significantly improves the breakdown strength and energy density, improves the energy storage performance of the material, achieves an efficient charging and discharging process, and maintains the mechanical properties of the polymer matrix.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention discloses an energy storage performance optimization method of an all-organic composite dielectric film based on an asymmetric heterostructure, and belongs to the technical field of dielectric energy storage materials. In order to effectively improve the energy storage capability of the composite medium, the invention constructs a novel asymmetric heterostructure of an insulating layer, a transition layer and a polarization layer. Wherein the insulating layer is a linear dielectric medium with high breakdown strength and good insulating property; due to the middle transition layer, the electric field distribution of the asymmetric heterogeneous three-layer composite material is more uniform, and excessive concentration of interlayer voltage is effectively avoided; the polarization layer is made of ferroelectric polymer with excellent polarization intensity. According to the PMMA / 30wt.% PMMA-PVDF / PVDF composite dielectric material disclosed by the invention, under the field intensity of 579.7 kV / mm, the discharge energy density is up to 15.3 J / cm < 3 >, the charge-discharge efficiency is up to 77.4%, the discharge energy density is improved by 88.9% compared with that of a PVDF material, and the efficiency is improved by 86.5%. The construction of the asymmetric heterostructure combines the advantages of the ferroelectric polymer and the linear dielectric, the energy storage performance and the charge-discharge efficiency of the polymer are remarkably improved by utilizing the structural advantages, and the preparation strategy of the asymmetric heterostructure all-organic medium composite film provides a new way for realizing a medium energy storage material with better performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of dielectric capacitors, and in particular to a method for optimizing energy storage performance of an all-organic composite dielectric film based on an asymmetric heterostructure. Background Art

[0002] In modern electronic and power systems, polymer-based dielectric capacitors with excellent performance play an indispensable role. They have the advantages of large dielectric constant, good flexibility, low density, and easy processing, and have been widely used in the field of dielectric capacitors. Therefore, how to further improve the performance of dielectric materials used in capacitors is still a promising research direction. In experimental studies, it was found that polyvinylidene fluoride (PVDF), a semi-crystalline polymer, has excellent polarization strength and energy storage capacity, but when its polarization strength increases, its breakdown strength will also decrease, so there are still disadvantages such as low charging and discharging efficiency and high loss. For most of the current linear dielectric materials, although they have the advantages of high breakdown strength, low loss and high efficiency, they also have the disadvantages of low dielectric constant, poor polarization strength and energy storage capacity. Therefore, using the above characteristics, a new dielectric optimization scheme is proposed. The present invention selects PVDF as the basic energy storage unit and polymethyl methacrylate (PMMA), a linear dielectric material with excellent insulating properties, as the optimized material, explores the influence of heterogeneous material compatibility on performance, and designs the microstructure of the composite medium to effectively improve its breakdown field strength, reduce dielectric loss during charging and discharging, and greatly improve the energy storage performance of the material. In the present invention, a new and unique asymmetric heterogeneous insulation-transition-polarization structure is designed, in which the top layer is a linear dielectric as an insulating layer, providing high breakdown strength and low loss, the middle transition layer can make the electric field inside the structure more uniform, thereby reducing electric field distortion and significantly improving Eb, and the bottom layer is a polarization layer that provides excellent energy storage and polarization capabilities for the heterogeneous structure. Compared with the traditional symmetrical sandwich structure, the new asymmetric heterogeneous structure has higher η and U. d The asymmetric three-layer all-polymer design strategy is to obtain high η and high U d This opens up a new path for dielectric energy storage materials. Summary of the invention

[0003] In order to solve the problems of low dielectric energy storage density and low breakdown strength in the prior art, the present invention provides a method for optimizing the energy storage performance of an all-organic composite dielectric film based on an asymmetric heterostructure. The present invention provides high energy density through a polarization layer, an intermediate transition layer homogenizes the electric field, and a linear dielectric layer provides high discharge efficiency. In particular, based on the principle that the interface polarization effect of an asymmetric heterostructure can effectively make the electric field distribution uniform, thereby greatly improving the breakdown strength and energy density, a method for optimizing the energy storage performance of an all-organic composite dielectric film based on an asymmetric heterostructure is provided.

[0004] One of the purposes of the present invention is to provide an all-organic composite dielectric film based on an asymmetric heterostructure, which includes an insulating layer, a transition layer and a polarization layer, wherein the transition layer is arranged between the insulating layer and the polarization layer; wherein the insulating layer is made of a ferroelectric polymer, the polarization layer is made of a linear dielectric polymer, and the transition layer is made of a mixture of a ferroelectric polymer and a linear dielectric polymer.

[0005] In a preferred embodiment of the present invention,

[0006] The ferroelectric polymer is polyvinylidene fluoride, commonly known as polyvinylidene fluoride resin, with a density of 1.0-1.2 g / cm 3 , molecular formula C2H2F2, dielectric constant 8-15, molecular weight 60-65, crystallinity 40-54%, melting point 166-170℃.

[0007] The linear dielectric polymer is polymethyl methacrylate with a density of 1.0 to 1.3 g / cm 3 , molecular formula C5H8O2, dielectric constant 2~6, molecular weight 100~105, melting point 100~110℃.

[0008] In the mixture of the ferroelectric polymer and the linear dielectric polymer, the mass ratio of the ferroelectric polymer to the linear dielectric polymer is in the range of 1:9 to 3:7.

[0009] In a preferred embodiment of the present invention,

[0010] The thickness of the insulating layer, transition layer and polarization layer are the same or different, and are independently 8 to 10 μm (referring to the thickness before hot pressing); and / or,

[0011] The thickness of the all-organic composite dielectric film is 25-30 μm.

[0012] The second object of the present invention is to provide a method for preparing an all-organic composite dielectric film based on an asymmetric heterostructure according to the first object of the present invention, comprising:

[0013] The ferroelectric polymer, the linear dielectric polymer and the mixture of the ferroelectric polymer and the linear dielectric polymer are respectively made into single-layer films by a solution dispersion method, and then the ferroelectric polymer film, the mixture film of the ferroelectric polymer and the linear dielectric polymer and the linear dielectric polymer film are sequentially laminated and hot-pressed to obtain the all-organic composite dielectric film based on the asymmetric heterostructure.

[0014] In a preferred embodiment of the present invention,

[0015] The method comprises:

[0016] 1) dissolving a ferroelectric polymer in a solvent A to obtain a ferroelectric polymer solution, then scraping the ferroelectric polymer solution to form a film and removing the solvent to obtain a ferroelectric polymer film;

[0017] 2) dissolving a linear dielectric polymer in solvent B to obtain a linear dielectric polymer solution, then scraping the linear dielectric polymer solution to form a film and removing the solvent to obtain a linear dielectric polymer film;

[0018] 3) dissolving a mixture of a ferroelectric polymer and a linear dielectric polymer in a solvent C to obtain a mixture solution, and then scraping the mixture solution to form a film and removing the solvent to obtain a mixture film of the ferroelectric polymer and the linear dielectric polymer;

[0019] 4) The ferroelectric polymer film, the mixture film of the ferroelectric polymer and the linear dielectric polymer, and the linear dielectric polymer film are sequentially laminated, then subjected to hot pressing treatment, and finally quenched to obtain the all-organic composite dielectric film based on the asymmetric heterostructure.

[0020] In a preferred embodiment of the present invention,

[0021] In step 1),

[0022] The solvent A is at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and / or,

[0023] The concentration range of the ferroelectric polymer solution is 0.1-0.2 g / ml; and / or,

[0024] The conditions for removing the solvent include: temperature of 80-120° C., time of 8-10 h; and / or,

[0025] The thickness of the ferroelectric polymer film is in the range of 8 to 10 μm.

[0026] In a preferred embodiment of the present invention,

[0027] In step 2),

[0028] The solvent B is at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and / or,

[0029] The concentration range of the linear dielectric polymer solution is 0.05-0.1 g / ml; and / or,

[0030] The conditions for removing the solvent include: temperature of 80-120° C., time of 8-10 h; and / or,

[0031] The thickness of the linear dielectric polymer film is in the range of 8 to 10 μm.

[0032] In a preferred embodiment of the present invention,

[0033] In step 3),

[0034] The solvent C is at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and / or,

[0035] The concentration range of the mixture solution of the ferroelectric polymer and the linear dielectric polymer is 0.075-0.15 g / ml; and / or,

[0036] In the mixture of the ferroelectric polymer and the linear dielectric polymer, the mass ratio of the ferroelectric polymer to the linear dielectric polymer is in the range of 1:9 to 3:7; and / or,

[0037] The conditions for removing the solvent include: temperature of 80-120° C., time of 8-10 h; and / or,

[0038] The thickness of the mixture film of the ferroelectric polymer and the linear dielectric polymer is in the range of 8 to 10 μm.

[0039] In a preferred embodiment of the present invention,

[0040] In step 4),

[0041] The gradient temperature increase hot pressing treatment comprises: placing the laminated three-layer film into a tablet press, in the first stage, the hot pressing temperature is 60-90° C., maintaining the pressure at 1-15 MPa for 10-15 min, releasing the pressure to remove bubbles, removing the applied pressure, keeping the temperature at 60-90° C., and removing bubbles for 10-15 min; in the second stage, the hot pressing temperature is 90-120° C., maintaining the pressure at 1-15 MPa for 10-15 min, releasing the pressure to remove bubbles, removing the applied pressure, keeping the temperature at 90-120° C., and removing bubbles for 10-15 min; in the third stage, the hot pressing temperature is 120-150° C., maintaining the pressure at 1-15 MPa for 10-15 min, releasing the pressure to remove bubbles, removing the applied pressure, keeping the temperature at 120-150° C., and removing bubbles for 10-15 min; and / or,

[0042] The quenching comprises: rapidly cooling the composite film after the gradient temperature increase hot pressing treatment to room temperature through a water cooling device, and maintaining the pressure at 1 to 15 MPa for 1 to 5 minutes.

[0043] The present invention can adopt the following specific technical solutions:

[0044] Step 1:

[0045] Take a certain amount of polyvinylidene fluoride [PVDF] and polymethyl methacrylate [PMMA] and place them in a plastic bag, bake them in a blast drying oven at a certain temperature for a period of time, and then take five identical beakers to weigh the calculated mass of PVDF and PMMA powders, dissolve them in a certain amount of N, N-dimethylformamide (DMF) solution, and stir them magnetically at an appropriate temperature until the powder is evenly dispersed. Set the stirring temperature, stir for a period of time until the solute is completely dissolved to obtain the desired solution;

[0046] Step 2:

[0047] The solution obtained in step 1 is placed in a vacuum drying oven, and the temperature and time are set to vacuum the solution to remove excess bubbles, so as to prevent the bubbles in the solution from affecting the quality of the scraped film. The solution is allowed to stand for several hours, and the colloid is taken out for use after the bubbles in the solution are completely precipitated;

[0048] Step 3:

[0049] The organic composite medium wet film is prepared by the scraping method. The cleaned glass plate is placed on the automatic coating machine, the scraper is leveled, the number of rotation grids of the scraper is determined, and the wet film prepared by the scraping method is placed in a blast drying oven at a suitable temperature for drying and heat treatment for several hours by adjusting the advancing speed and advancing position of the automatic coating machine.

[0050] Step 4:

[0051] The hot pressing and quenching process is used to hot press composite dielectric films with different mass fractions and components, and a gradient temperature increase hot pressing treatment is performed. Finally, the temperature of the composite film is quickly reduced to room temperature through a water cooling device, and the pressure is maintained under a certain pressure to obtain a dielectric composite medium with suitable thickness, uniformity and density, and high energy storage density.

[0052] Furthermore, as described in step 1, polyvinylidene fluoride [PVDF] and polymethyl methacrylate [PMMA] are placed in a forced air drying oven at 60°C for heat treatment for 6 hours. Afterwards, five portions of 1-2g of polyvinylidene fluoride powder and polymethyl methacrylate powder are weighed in sequence on a digital balance and placed on weighing paper, 10-20ml of N,N-dimethylformamide (DMF) solution is weighed in a beaker with a pipette, 1-2g of dried polymethyl methacrylate and 1-2g of polyvinylidene fluoride powder are added to DMF in sequence and stirred at room temperature until completely dissolved, and stirred at room temperature for 12 hours until the solution is evenly dispersed.

[0053] Furthermore, in step 2, the organic medium solution obtained in step 1 is transferred into a vacuum drying oven, evacuated and allowed to stand for 3 hours, and then taken out for use after the bubbles of the organic solution are precipitated.

[0054] Furthermore, the prepared clean glass plate is wiped clean with alcohol, and after confirming that the surface is smooth, it is placed on the automatic coating machine, and the coating machine push knife forward speed is set to 3 to 8 cm / s, and the push knife forward distance is 20 to 30 cm. The scraper is taken out and placed on the glass plate, the scraper is leveled, and the scraper spiral scale is rotated 10 to 30 grids. The organic solution prepared in step 2 is poured on the surface of the glass plate, and the glass plate is appropriately tilted to allow the organic solution to flow to the scraper, and then the coating process is performed.

[0055] Furthermore, the film prepared by the doctor blade coating method was marked according to different categories and transferred to a blast drying oven, with the temperature set to 60-120°C and the time set to 4-12 hours. The glass plate was then taken out and transferred to a vacuum drying oven, evacuated, and the temperature set to 60-150°C. After heat treatment in the vacuum drying oven for 12 hours, it was taken out and peeled off with a blade under the action of deionized water and placed in a polyester film for standby use; the thickness of the prepared single-layer film was 8-12 μm.

[0056] Furthermore, in step 4, a hot pressing process is used to place the multilayer composite film in a hot pressing template and perform a gradient temperature increase hot pressing process:

[0057] The gradient temperature rise hot pressing treatment comprises: placing the laminated three-layer film into a tablet press, hot pressing at a temperature of 60 to 90° C. in the first stage, maintaining the pressure at 1 to 15 MPa for 10 to 15 minutes, releasing the pressure to remove bubbles, removing the applied pressure, maintaining the temperature at 60 to 90° C., and removing bubbles for 10 to 15 minutes; hot pressing at a temperature of 90 to 120° C. in the second stage, maintaining the pressure at 1 to 15 MPa for 10 to 15 minutes, releasing the pressure to remove bubbles, removing the applied pressure, maintaining the temperature at 90 to 120° C., and removing bubbles for 10 to 15 minutes. nn; The third stage hot pressing temperature is 120-150°C, the pressure is maintained at 1-15MPa for 10-15min, the pressure is released to remove bubbles, the applied pressure is removed, the temperature is maintained at 120-150°C, and the bubbles are removed for 10-15min; and / or, the quenching includes: the composite film after the gradient temperature increase hot pressing treatment is quickly cooled to room temperature through a water cooling device, and the pressure is maintained at 1-15MPa for 1-5min; the thickness of the all-organic composite dielectric film based on the asymmetric heterostructure after hot pressing is in the range of 25-30μm.

[0058] The third object of the present invention is to provide an all-organic composite dielectric film based on an asymmetric heterostructure according to one of the objects of the present invention, or an all-organic composite dielectric film based on an asymmetric heterostructure obtained by the preparation method described in the second object of the present invention, and use it in a capacitor.

[0059] The breakdown strength of pure PVDF ranges from 300kV / mm to 450kV / mm, the breakdown strength of pure PMMA ranges from 350kV / mm to 550kV / mm, the breakdown strength of asymmetric heterogeneous composite medium PMMA / 10wt% PMMA-90wt% PVDF / PVDF composite medium prepared by hot pressing of the above materials ranges from 400kV / mm to 550kV / mm; the breakdown strength of PMMA / 20wt% PMMA-80wt% PVDF / PVDF composite medium ranges from 500kV / mm to 575kV / mm; and the breakdown strength of PMMA / 30wt% PMMA-70wt% PVDF / PVDF composite medium ranges from 500kV / mm to 600kV / mm.

[0060] The dielectric constant of pure PVDF is in the range of 7 to 9 at a frequency of 1 Hz. 6 At a frequency of 1 Hz, the dielectric constant ranges from 5 to 7. The dielectric constant of pure PMMA at a frequency of 1 Hz ranges from 3.8 to 4.2. 6 Hz, the dielectric constant ranges from 3.8 to 4.2. PMMA, PMMA and PVDF blended medium and PVDF are subjected to multi-layer hot pressing. The PMMA / 10wt% PMMA-90wt% PVDF / PVDF composite medium has a dielectric constant range of 5.5 to 6 at a frequency of 1 Hz and a dielectric constant range of 1.5 to 2.0 at a frequency of 1×106 At a frequency of 1 Hz, the dielectric constant ranges from 5.2 to 5.7; at a frequency of 1 Hz, the dielectric constant of PMMA / 20wt%PMMA-80wt%PVDF / PVDF composite medium ranges from 5.2 to 5.8. 6 At a frequency of 1 Hz, the dielectric constant ranges from 5 to 5.5; at a frequency of 1 Hz, the dielectric constant of PMMA / 30wt%PMMA-70wt%PVDF / PVDF composite medium ranges from 5 to 5.5. 6 At a frequency of Hz, the dielectric constant ranges from 4.8 to 5.2.

[0061] The discharge energy density of pure PVDF at an electric field strength of 420 kV / mm is in the range of 8.0 to 9.5 J / cm 3 The discharge energy density of pure PMMA at an electric field strength of 500 kV / mm is in the range of 6.5 to 8.5 J / cm 3 The PMMA, PMMA and PVDF blend medium and PVDF are subjected to multi-layer hot pressing, and the discharge energy density of the PMMA / 10wt% PMMA-90wt% PVDF / PVDF composite medium is in the range of 12.1 to 13.4 J / cm at an electric field strength of 500 kV / mm. 3 The discharge energy density of PMMA / 20wt%PMMA-80wt%PVDF / PVDF composite medium at 550kV / mm electric field strength is in the range of 12.8~14.5J / cm 3 The discharge energy density of PMMA / 30wt%PMMA-70wt%PVDF / PVDF composite medium at 590kV / mm electric field strength is in the range of 14.9~15.7J / cm 3

[0062] The charge and discharge efficiency of pure PVDF at an electric field strength of 420kV / mm ranges from 35% to 45%, the charge and discharge efficiency of pure PMMA at an electric field strength of 500kV / mm ranges from 80% to 90%, the charge and discharge efficiency of PMMA / 10wt%PMMA-90wt%PVDF / PVDF composite medium at an electric field strength of 500kV / mm ranges from 72% to 78%; the charge and discharge efficiency of PMMA / 20wt%PMMA-80wt%PVDF / PVDF composite medium at an electric field strength of 550kV / mm ranges from 74% to 78%; the charge and discharge efficiency of PMMA / 30wt%PMMA-70wt%PVDF / PVDF composite medium at an electric field strength of 590kV / mm ranges from 75% to 80%.

[0063] Beneficial effects of the present invention:

[0064] In this invention, a novel asymmetric heterostructure is designed. A transition layer is introduced between the insulating layer and the polarization layer to form a unique asymmetric three-layer linear transition-nonlinear structure. Linear dielectric PMMA and pure PVDF are used as the insulating and polarization layers, respectively, and PMMA-PVDF blended composite material is used as the intermediate transition layer. The optimized intermediate layer can achieve uniform distribution of the electric field. Compared with the traditional symmetrical sandwich structure, the new asymmetric heterostructure has higher η and U d The asymmetric three-layer all-polymer design strategy is to obtain high η and high U d This opens up a new path for dielectric energy storage materials.

[0065] The preparation process and the required equipment of the present invention are low-cost, and the experiment is simple and easy to implement. The uniformly distributed and dense multilayer structure composite medium prepared in the experiment can effectively improve the energy storage performance of the polymer and maintain the excellent mechanical properties of the polymer matrix itself. Therefore, the high energy storage density composite medium prepared in this experiment can be used in the field of energy storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 SEM cross-sectional structure of asymmetric heterostructure composite dielectric A / 1A-9F / A;

[0067] Figure 2 SEM cross-sectional structure of asymmetric heterostructure composite dielectric A / 2A-8F / A;

[0068] Figure 3 SEM cross-sectional structure of asymmetric heterostructure composite dielectric A / 3A-7F / A;

[0069] Figure 4 EDS element mapping images of asymmetric heterostructure composite dielectrics;

[0070] Figure 5 XRD patterns of asymmetric heterostructure composite dielectrics;

[0071] Figure 6 FTIR spectrum of asymmetric heterostructure composite dielectrics;

[0072] Figure 7 Dielectric properties of asymmetric heterostructure composite dielectrics;

[0073] Figure 8 Breakdown properties of asymmetric heterostructure composite dielectrics;

[0074] Fig. 9 Breakdown performance of symmetrical sandwich structure composite dielectrics;

[0075] Fig.10Energy storage performance of asymmetric heterostructure composite dielectrics;

[0076] Fig.11 Energy storage performance of symmetric sandwich structure composite dielectrics. DETAILED DESCRIPTION

[0077] The present invention is described in detail below in conjunction with specific embodiments and drawings. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.

[0078] Example 1

[0079] Ferroelectric polymer polyvinylidene fluoride PVDF (molecular weight 64.034, 10Hz dielectric constant 8), linear dielectric polymethyl methacrylate PMMA powder (molecular weight 100.116, 10Hz dielectric constant 4) and their blend were made into single-layer dielectric films by solution dispersion method, and then the polyvinylidene fluoride film, blend film and linear dielectric PMMA film were hot-pressed at high temperature to prepare asymmetric heterostructure composite dielectric A / 1A-9F / A film.

[0080] Step 1:

[0081] Place polyvinylidene fluoride [PVDF] and polymethyl methacrylate [PMMA] in a forced air drying oven at 60°C for 6 hours. After that, use a digital balance to weigh a portion of 1g of polyvinylidene fluoride powder, a portion of 1g of polymethyl methacrylate powder, and a portion of 0.9g of polyvinylidene fluoride powder + 0.1g of polymethyl methacrylate powder blend, and place them on weighing paper respectively. Use a pipette to weigh three portions of 10ml of N, N-dimethylformamide (DMF) solution and add them to a beaker. The weighed polymethyl methacrylate powder, polyvinylidene fluoride powder, and the blend of polymethyl methacrylate powder and polyvinylidene fluoride powder are added to DMF in turn and stirred at room temperature until completely dissolved. Stir at room temperature for 12 hours until the solution is evenly dispersed.

[0082] Step 2:

[0083] The organic medium solution obtained in step 1 is transferred to a vacuum drying oven, evacuated and left to stand for 3 hours, and then taken out for use after the bubbles of the organic solution are precipitated.

[0084] Step 3:

[0085] Wipe the prepared clean glass plate with alcohol, and place it on the automatic coating machine after confirming that the surface is smooth. Set the coating machine push knife forward speed to 5cm / s and the push knife forward distance to 25cm. Take out the scraper and place it on the glass plate. Level the scraper, rotate the scraper spiral scale 20 grids, pour the organic solution prepared in step 2 on the surface of the glass plate, tilt the glass plate appropriately to allow the organic solution to flow to the scraper, and then perform the coating process.

[0086] Step 4:

[0087] The film prepared by the doctor blade coating method was marked according to different categories and transferred to a blast drying oven, with the temperature set to 80°C and the time set to 8 hours. The glass plate was then taken out and transferred to a vacuum drying oven, evacuated, and the temperature set to 100°C. After heat treatment in the vacuum drying oven for 12 hours, it was taken out and peeled off with a blade under the action of deionized water for later use. The thickness of the prepared single-layer film was 10 μm.

[0088] Step 5:

[0089] The prepared polyvinylidene fluoride, ferroelectric polymer and linear dielectric blend film and polymethyl methacrylate are sequentially laminated; the gradient temperature increase hot pressing treatment comprises: placing the laminated three-layer film into a tablet press, the first stage hot pressing temperature is 60-90°C, the pressure is maintained at 1-15MPa for 10-15min, the pressure is released to remove bubbles, the applied pressure is removed, the temperature is maintained at 60-90°C, and the bubbles are removed for 10-15min; the second stage hot pressing temperature is 90-120°C, the pressure is maintained at 1-15MPa for 10-15min, the pressure is released to remove bubbles, the applied pressure is removed force, keep warm at 90-120°C, and remove bubbles for 10-15min; in the third stage, the hot pressing temperature is 120-150°C, the pressure is maintained at 1-15MPa for 10-15min, the pressure is released to remove bubbles, the applied pressure is removed, the temperature is maintained at 120-150°C, and the bubbles are removed for 10-15min; and / or, the quenching includes: the composite film after the gradient temperature increase hot pressing treatment is quickly cooled to room temperature through a water cooling device, and the pressure is maintained at 1-15MPa for 1-5min; the thickness of the all-organic composite dielectric film based on the asymmetric heterostructure after hot pressing is 27μm.

[0090] Example 2

[0091] The ferroelectric polymer polyvinylidene fluoride PVDF (molecular weight 64.034, 10Hz dielectric constant 8), linear dielectric polymethyl methacrylate PMMA powder (molecular weight 100.116, 10Hz dielectric constant 4) and their blend were respectively made into single-layer dielectric films by solution dispersion method. Then, the polyvinylidene fluoride film, the blend film and the linear dielectric PMMA film were hot-pressed at high temperature to prepare an asymmetric heterostructure composite dielectric A / 2A-8F / A film.

[0092] Step 1:

[0093] Place polyvinylidene fluoride [PVDF] and polymethyl methacrylate [PMMA] in a forced air drying oven at 60°C for 6 hours. After that, use a digital balance to weigh one portion of 1g of polyvinylidene fluoride powder, one portion of 1g of polymethyl methacrylate powder, and one portion of 0.8g polyvinylidene fluoride powder + 0.2g polymethyl methacrylate powder blend on weighing paper, use a pipette to weigh three portions of 10ml N, N-dimethylformamide (DMF) solution and add them to a beaker, and add the weighed polymethyl methacrylate powder, polyvinylidene fluoride powder, and polymethyl methacrylate powder and polyvinylidene fluoride powder blend to DMF in turn and stir at room temperature until completely dissolved, and stir at room temperature for 12 hours until the solution is evenly dispersed.

[0094] Steps 2 to 5 are the same as in Example 1

[0095] Example 3

[0096] Ferroelectric polymer polyvinylidene fluoride PVDF (molecular weight 64.034, 10Hz dielectric constant 8), linear dielectric polymethyl methacrylate PMMA powder (molecular weight 100.116, 10Hz dielectric constant 4) and their blend were made into single-layer dielectric films by solution dispersion method, and then the polyvinylidene fluoride film, blend film and linear dielectric PMMA film were hot-pressed at high temperature to prepare asymmetric heterostructure composite dielectric A / 3A-7F / A film.

[0097] Step 1:

[0098] Place polyvinylidene fluoride [PVDF] and polymethyl methacrylate [PMMA] in a forced air drying oven at 60°C for 6 hours. After that, use a digital balance to weigh one portion of 1g of polyvinylidene fluoride powder, one portion of 1g of polymethyl methacrylate powder, and one portion of 0.7g of polyvinylidene fluoride powder + 0.3g of polymethyl methacrylate powder blend on weighing paper, use a pipette to weigh three portions of 10ml of N, N-dimethylformamide (DMF) solution and add them to a beaker, and add the weighed polymethyl methacrylate powder, polyvinylidene fluoride powder, and polymethyl methacrylate powder and polyvinylidene fluoride powder blend to DMF in turn and stir at room temperature until completely dissolved, and stir at room temperature for 12 hours until the solution is evenly dispersed.

[0099] Steps 2 to 5 are the same as in Example 1

[0100] Figures 1 to 3 This is a scanning electron microscope cross-sectional structure diagram of an asymmetric heterostructure composite dielectric. As shown in the figure, the interfaces between the multilayer composite dielectric layers are clear and obvious, all around 27μm, which provides a guarantee for the energy storage performance of the film.

[0101] Figure 4 This is the EDS element mapping image of the selected asymmetric heterostructure. The brighter area receives more light signals during the scanning process. From the distribution of the F element mapping in the figure, it can be seen that the F element content changes from the brightest on the right to the lighter in the middle, and finally becomes weak on the left corresponding to the linear dielectric. This confirms the successful construction of the asymmetric heterostructure.

[0102] Figure 5 The XRD diffraction pattern of the asymmetric heterostructure composite dielectric obtained in the present invention is observed. It is found that the non-polar α phase diffraction peak of PVDF is detected at 17.9° and 20.2° at 2θ, and the corresponding low-polarity γ diffraction peak is detected at 20.1° and 18.5°. The polar β phase diffraction peak appears at 2θ at 20.9°, corresponding to (100), (021), (110), (020) and (110) crystal planes, respectively. At the same time, since the linear dielectric has a diffraction peak between 10° and 15°, it can be observed in the XRD image that as the content of the linear dielectric increases, the corresponding diffraction peak also increases.

[0103] Figure 6 This is the FTIR characterization image of the asymmetric heterostructure composite dielectric. As shown in the figure, the γ phase 512cm of the composite dielectric PVDF was successfully detected. -1 α phase 611cm -1 and 966cm -1 CF2 asymmetric stretching vibration and symmetric stretching vibration at 840cm -1 and 881cm -1 The characteristic infrared diffraction peak at 1073cm -1 The characteristic infrared absorption peak of CH2 vibration of PVDFβ phase was detected near 989cm -1 、1449cm -1 、1270cm -1 、1729cm -1 、2845cm -1 、2955cm -1 and 3000cm -1 The characteristic absorption peak of PMMA was detected nearby, indicating that PMMA was successfully compounded into the asymmetric heterostructure.

[0104] Figure 7The dielectric properties of asymmetric heterostructure composite dielectrics are studied. The dielectric constant is a key factor in energy storage and reflects the polarization ability of the material. Therefore, the relative dielectric constant and dielectric loss of asymmetric heterostructure composite materials at different frequencies were tested. As can be seen from the figure, it can be found that with the increase of the test frequency, the dielectric constant will decrease and the loss will increase to a certain extent. This is because the interfacial polarization at the interface of the sandwich structure film will be enhanced at high frequencies, resulting in a decrease in the dielectric constant and an increase in the loss. In addition, with the increase of frequency, it can be found that the dielectric constant of PMMA is stable, while the dielectric constant of PVDF shows a downward trend. For linear PMMA, the polarization intensity changes linearly with the electric field within the frequency range, which makes the dielectric constant stable within the test frequency range. As expected, the linear dielectric and pure PVDF show the lowest and highest relative dielectric constants, respectively, while the relative dielectric constant of the constructed x / xF / F asymmetric heterostructure composite medium is slightly higher than that of the pure linear dielectric. For pure PVDF, the dielectric loss at high frequencies is relatively higher than that of pure PMMA. For pure PMMA, its dielectric loss continues to decrease with increasing frequency, which is due to the expansion of β relaxation of PMMA at low frequencies. However, dipole polarization dominates the overall polarization of ferroelectric polymers. Compared with electronic polarization, it takes longer to achieve dipole polarization. Therefore, dipole polarization weakens with increasing frequency, resulting in a decrease in the dielectric constant of the dielectric film. Compared with pure PMMA dielectrics, the dielectric constant of the composite dielectric is improved, which may be due to the higher dielectric constant of the introduced organic polymer PVDF itself and the enhancement of interfacial polarization. At a frequency of 1 Hz, the dielectric constant of the high energy storage density composite dielectric ranges from 4 to 8, and the dielectric loss ranges from 0.01 to 0.05. At 1×10 7 At a frequency of Hz, the dielectric constant of the asymmetric heterostructure composite medium ranges from 5 to 7, and the dielectric loss ranges from 0.05 to 0.20.

[0105] Figure 8 The Weibull distribution diagram of the breakdown strength of asymmetric heterostructure composite dielectrics. In addition to the relative dielectric constant, the breakdown strength also plays a vital role in energy storage performance, especially in applications under high electric fields. Therefore, the dual-parameter Weibull distribution is further used to analyze the breakdown behavior of the composite material. As shown in the figure, the breakdown strength of the single-layer PVDF dielectric is only 423.5 kV / mm, and the breakdown strength of the asymmetric heterostructure composite dielectric A / 3A-7F / F is significantly improved, reaching 581.6 kV / mm, which is 38.4% higher than the PVDF breakdown strength. Fig. 9 As shown, the breakdown strength of the symmetrical sandwich structure composite dielectric is lower than that of the asymmetrical heterostructure composite dielectric, where the DC breakdown strengths of F / A / F and A / F / A are 463.4 kV / mm and 485.9 kV / mm, respectively.

[0106] By comparing and analyzing the data in the figure, we can conclude that the constructed asymmetric heterostructure can effectively improve the insulation performance of the composite medium. There are two main reasons for this phenomenon: First, E b The improvement of E is attributed to the high insulation performance (breakdown strength) of the linear dielectric, which can effectively block the growth of the breakdown path; secondly, due to the introduction of the intermediate transition layer, the electric field distribution of the asymmetric heterogeneous three-layer composite material is more uniform, which effectively avoids the excessive concentration of the interlayer voltage. The interface between the insulating layer, the transition layer and the polarization layer strongly blocks the growth of the breakdown path. This has a great impact on improving the E of the three-layer composite material. b In summary, the E b The significant improvement should be attributed to the uniform distribution of the electric field and the barrier effect of the interface between adjacent layers. The uniformity of the electric field effectively avoids the early breakdown of the composite material and significantly improves the electrochemical performance.

[0107] Fig.10 The energy storage performance diagram of the asymmetric heterostructure composite dielectric shows that, as the electric field increases, U d The energy storage density of the A / 3A-7F / F composite dielectric at an electric field strength of 579.7 kV / mm is 15.3 J / cm 3 At the same time, if Fig.11 It can be observed that compared with the symmetric sandwich structure composite medium, the breakdown performance and energy storage performance of the asymmetric heterostructure are greatly improved. The discharge energy density of the symmetric sandwich structure composite medium is 10.1 J / cm at an electric field strength of 479.7 kV / mm. 3 , the charge and discharge efficiency is 69.6%. The breakdown strength and energy storage density increased by 20.8% and 41.6%, respectively. The constructed asymmetric heterostructure composite dielectric effectively improves the energy storage performance of the composite dielectric by using a novel insulating layer-transition layer-polarization layer model. At the same time, compared with pure PVDF dielectrics, the asymmetric heterostructure significantly improves the discharge energy density while also having excellent charge and discharge efficiency. The charge and discharge efficiency of the A / 3A-7F / F composite dielectric is 77.4%, which is 86.5% higher than that of PVDF. This is because on the one hand, when a linear dielectric composite dielectric with high insulation strength is used as an outer insulating layer, the D rThe value suppresses loss, and when in contact with the electrode, it can effectively suppress the injection of carriers at the electrode, so its leakage current density is also reduced, which improves the insulation performance of the composite medium. On the other hand, the use of the blended dielectric as an intermediate transition layer can effectively even out the electric field distribution inside the composite material, which plays a role in improving the breakdown performance. In addition, the interface polarization of the macroscopic interface between adjacent layers and the microscopic interface inside the transition layer also helps to further improve the energy density. Therefore, the designed asymmetric heterostructure can maintain excellent charge and discharge efficiency while having excellent storage capacity.

[0108] Depend on Figure 7 , Figure 8 and Fig.10 It can be seen that the preparation method of the present invention can make the prepared asymmetric heterostructure composite medium based on polyvinylidene fluoride and polymethyl methacrylate have higher energy storage performance and breakdown strength. The constructed asymmetric heterostructure composite medium significantly improves the DC breakdown strength of the asymmetric heterostructure composite medium A / 3A-7F / F, reaching 581.6kV / mm, which is 38.4% higher than the breakdown strength of PVDF. The interface between the insulating layer, transition layer and polarization layer strongly blocks the growth of the breakdown path. This has a great impact on improving the E of the three-layer composite material. b The uniform distribution of the electric field and the barrier effect of the interface between adjacent layers have a significant effect. The uniformity of the electric field effectively avoids the early breakdown of the composite material, significantly improves the electrochemical performance, and effectively improves the energy storage performance of the composite medium by using a novel insulating layer-transition layer-polarization layer model. The energy storage density of the A / 3A-7F / F composite dielectric at 579.7kV / mm is 15.3J / cm 3 The synergistic effect of the insulating layer, transition layer and polarization layer not only inhibits the injection of carriers at the electrode, but also affects the distribution of the electric field by homogenizing the electric field, thereby reducing structural defects, reducing leakage current density and dielectric loss, and ultimately effectively improving the insulation strength and energy storage capacity of the composite dielectric. The unique asymmetric heterostructure composite material in the present invention exhibits a good combination of high energy density and charge and discharge efficiency, providing a new paradigm for the design of high-performance dielectric materials.

Claims

1. An all-organic composite dielectric film based on an asymmetric heterostructure, comprising an insulating layer, a transition layer and a polarization layer, wherein the transition layer is arranged between the insulating layer and the polarization layer; wherein: The material of the insulating layer is a ferroelectric polymer, the material of the polarization layer is a linear dielectric polymer, and the material of the transition layer is a mixture of a ferroelectric polymer and a linear dielectric polymer.

2. The all-organic composite dielectric film according to claim 1, characterized in that: The ferroelectric polymer is polyvinylidene fluoride, commonly known as polyvinylidene fluoride resin, with a density of 1.0-1.2 g / cm 3 , molecular formula C2H2F2, dielectric constant 8-15, molecular weight 60-65, crystallinity 40-54%, melting point 166-170℃. The linear dielectric polymer is polymethyl methacrylate with a density of 1.0 to 1.3 g / cm 3 , molecular formula C5H8O2, dielectric constant 2~6, molecular weight 100~105, melting point 100~110℃. In the mixture of the ferroelectric polymer and the linear dielectric polymer, the mass ratio of the ferroelectric polymer to the linear dielectric polymer is in the range of 1:9 to 3:

7.

3. The all-organic composite dielectric film according to claim 1, characterized in that: The thicknesses of the insulating layer, transition layer and polarization layer are the same or different, and before hot pressing, the thicknesses of the insulating layer, transition layer and polarization layer are independently 8 to 10 μm; and / or, The thickness of the all-organic composite dielectric film is 25-30 μm.

4. A method for preparing the all-organic composite dielectric film according to any one of claims 1 to 3, comprising: The ferroelectric polymer, the linear dielectric polymer and the mixture of the ferroelectric polymer and the linear dielectric polymer are respectively made into single-layer films by a solution dispersion method, and then the ferroelectric polymer film, the mixture film of the ferroelectric polymer and the linear dielectric polymer and the linear dielectric polymer film are sequentially laminated and hot-pressed to obtain the all-organic composite dielectric film.

5. The preparation method according to claim 4, characterized in that The method comprises: 1) dissolving a ferroelectric polymer in a solvent A to obtain a ferroelectric polymer solution, then scraping the ferroelectric polymer solution to form a film and removing the solvent to obtain a ferroelectric polymer film; 2) dissolving a linear dielectric polymer in solvent B to obtain a linear dielectric polymer solution, then scraping the linear dielectric polymer solution to form a film and removing the solvent to obtain a linear dielectric polymer film; 3) dissolving a mixture of a ferroelectric polymer and a linear dielectric polymer in a solvent C to obtain a mixture solution, and then scraping the mixture solution to form a film and removing the solvent to obtain a mixture film of the ferroelectric polymer and the linear dielectric polymer; 4) The ferroelectric polymer film, the mixture film of the ferroelectric polymer and the linear dielectric polymer, and the linear dielectric polymer film are sequentially laminated, and then subjected to gradient temperature rise hot pressing treatment, and finally quenched to obtain the all-organic composite dielectric film.

6. The preparation method according to claim 5, characterized in that: In step 1), The solvent A is at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and / or, The concentration range of the ferroelectric polymer solution is 0.1-0.2 g / ml; and / or, The conditions for removing the solvent include: temperature of 80-120° C., time of 8-10 h; and / or, The thickness of the ferroelectric polymer film is in the range of 8 to 10 μm.

7. The preparation method according to claim 5, characterized in that: In step 2), The solvent B is at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and / or, The concentration range of the linear dielectric polymer solution is 0.05 to 0.1 g / m1; and / or, The conditions for removing the solvent include: temperature of 80 to 120° C. and time of 8 to 10 hours; and / or, The thickness of the linear dielectric polymer film is in the range of 8 to 10 μm.

8. The preparation method according to claim 5, characterized in that: In step 3), The solvent C is at least one of N,N-dimethylformamide, N,N-dimethylacetamide and N-methyl-2-pyrrolidone; and / or, The concentration range of the mixture solution of the ferroelectric polymer and the linear dielectric polymer is 0.075-0.15 g / ml; and / or, In the mixture of the ferroelectric polymer and the linear dielectric polymer, the mass ratio of the ferroelectric polymer to the linear dielectric polymer is in the range of 1:9 to 3:7; and / or, The conditions for removing the solvent include: temperature of 80-120° C., time of 8-10 h; and / or, The thickness of the mixture film of the ferroelectric polymer and the linear dielectric polymer is in the range of 8 to 10 μm.

9. The preparation method according to claim 5, characterized in that: In step 4), The gradient temperature increase hot pressing treatment comprises: placing the laminated three-layer film into a tablet press, in the first stage, the hot pressing temperature is 60-90° C., maintaining the pressure at 1-15 MPa for 10-15 min, releasing the pressure to remove bubbles, removing the applied pressure, keeping the temperature at 60-90° C., and removing bubbles for 10-15 min; in the second stage, the hot pressing temperature is 90-120° C., maintaining the pressure at 1-15 MPa for 10-15 min, releasing the pressure to remove bubbles, removing the applied pressure, keeping the temperature at 90-120° C., and removing bubbles for 10-15 min; in the third stage, the hot pressing temperature is 120-150° C., maintaining the pressure at 1-15 MPa for 10-15 min, releasing the pressure to remove bubbles, removing the applied pressure, keeping the temperature at 120-150° C., and removing bubbles for 10-15 min; and / or, The quenching comprises: rapidly cooling the composite film after the gradient temperature increase hot pressing treatment to room temperature through a water cooling device, and maintaining the pressure at 1-15 MPa for 1-5 minutes.

10. Use of the all-organic composite dielectric thin film according to any one of claims 1 to 3 or the all-organic composite dielectric thin film obtained by the preparation method according to any one of claims 4 to 9 in a capacitor.