Lithium-rich / micro-lithium-rich material as well as preparation method and application thereof
By using the core-shell structure of spinel phase and the molten salt synthesis method in lithium-rich materials, the composite structure of spherical secondary particles is formed, which solves the problem of poor circulation performance of lithium-rich materials, and significantly improves the first time in lithium-ion batteries. Coulomb efficiency and rate performance are suitable for large-scale industrial production.
Patent Information
- Application Number
- CN202411012014.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Due to its layered structure, lithium-rich materials have poor circulation performance, large irreversible capacity in the first circle, serious oxygen release and poor rate performance, which limits their application in lithium-ion batteries.
Lithium-rich/micro-lithium-rich material with a core-shell structure containing spinel phase is formed through the mixing of molten salt and precursor material and high-temperature calcination process to form a composite structure of spherical secondary particles, and the outer layer is a spinel thin shell. The layer has a large single crystal structure inside, which significantly improves the structural stability of the material.
It significantly improves the efficiency, rate performance and cycle performance of the first Coulomb, and has good material structure stability, suitable for large-scale industrial production, low cost and simple process.
Smart Images

Figure HDA0004964656740000011 
Figure HDA0004964656740000012 
Figure HDA0004964656740000021
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium-rich / slightly lithium-rich material and a preparation method and application thereof. Background Art
[0002] Lithium-rich manganese-based oxide cathode materials have the advantages of high capacity, high energy density and low cost, and are expected to meet the development requirements of the new generation of power batteries. As the price of cobalt continues to remain high, the development of lithium-rich cobalt-free cathode materials has become a research hotspot, and is expected to be actually applied as cathode materials in the next generation of high specific capacity lithium-ion batteries.
[0003] However, due to their layered structure, the cycling performance of such materials has gradually become prominent, which has become a problem restricting their practical application. In addition, the large irreversible capacity of this type of material in the first cycle, severe oxygen release, and poor rate performance have greatly limited the application of this material in lithium-ion batteries. Studies have shown that the degree of lithium desorption in layered structures is high under high specific capacity, which leads to drastic changes in lattice volume, resulting in stress concentration in polycrystalline particles, and the resulting intercrystalline cracks exacerbate the process of material deactivation and interface aging.
[0004] In order to overcome the above shortcomings of lithium-rich materials in the cycle process, it is usually necessary to modify the material. Usually, the methods to improve its electrochemical properties mainly include element doping and surface modification. In most cases, element doping and surface modification are achieved by introducing heteroatoms from the outside or subjecting the material to acid and alkali treatment, which will lead to complex processes for preparing materials, increased costs, and environmental damage caused by the addition of acids and alkalis. Therefore, it is necessary to develop a modification method that is simple to operate and more applicable, so that the material can be modified in situ during the synthesis process, and at the same time significantly improve its electrochemical performance, so that it can be suitable for large-scale industrial production, which has strong practical significance. Summary of the invention
[0005] The purpose of the present invention is to provide a lithium-rich / micro-lithium-rich material and its preparation method and application. The material is a core-shell structure containing a spinel phase, and the overall structure is stable. It is used in lithium-ion battery positive electrode materials to comprehensively improve the first coulomb efficiency, rate performance and cycle performance.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] Provide a lithium-rich / micro-lithium-rich material with the structural formula Li 1+x Mn y Ni z N w O r; Wherein, the N element is one or more of Ni, Al, Mg, Ti, Fe, Cu, Cr, Mo, Zr, and Ru; the parameters x, y, z, w, and r satisfy the following conditions: 0<x≤0.2, 0<y≤1, 0≤z<1, 0≤w≤1, 1.8≤r≤3;
[0008] The lithium-rich / slightly lithium-rich material is a spherical secondary particle, with large single crystal structures of the spinel phase of 2-5 μm dispersed inside, and the large single crystal structure is surrounded by primary particles, and the primary particles are radiated; the outermost layer of the lithium-rich / slightly lithium-rich material is a thin shell layer of the spinel phase.
[0009] According to the above scheme, the thickness of the thin shell layer is 450 to 550 nm.
[0010] A method for preparing the above-mentioned lithium-rich / slightly lithium-rich material is provided, comprising the following steps:
[0011] 1) Mixing a molten salt with a precursor material to obtain a mixture; wherein the molten salt is two or more lithium salts in an appropriate ratio, which will melt simultaneously at a certain temperature to form an ion melt;
[0012] 2) The mixture obtained in step 1) is heat treated in air or oxygen at the lowest melting temperature of the molten salt used, and finally calcined to obtain the lithium-rich / slightly lithium-rich material.
[0013] According to the above scheme, in the step 1), the lithium salt is: a mixed system of lithium nitrate and lithium hydroxide, in which the molar amount of lithium hydroxide accounts for 0.393 of the total molar amount; or, a mixed system of lithium carbonate and lithium sulfate, in which the molar amount of lithium carbonate accounts for 0.6 of the total molar amount; or, a mixed system of lithium carbonate and lithium fluoride, in which the molar amount of lithium carbonate accounts for 0.48 of the total molar amount; or, a mixed system of lithium carbonate and lithium nitrate, in which the molar amount of lithium carbonate accounts for 0.993 of the total molar amount; or, a mixed system of lithium carbonate and lithium hydroxide, in which the molar amount of lithium carbonate accounts for 0.843 of the total molar amount; or, a mixed system of lithium nitrate and lithium hydroxide, in which the molar amount of lithium nitrate accounts for 0.393 of the total molar amount.
[0014] According to the above scheme, in step 1), the molar ratio of the precursor material to the lithium element in the lithium salt is 1:1.02 to 1:1.25.
[0015] According to the above scheme: in the step 1), the precursor material is a carbonate or hydroxide precursor material containing two elements of manganese and nickel or three elements of manganese, nickel and N; wherein the N element is one or more of Ni, Al, Mg, Ti, Fe, Cu, Cr, Mo, Zr, and Ru.
[0016] According to the above scheme: in step 1), the lithium salt and the precursor material are mixed evenly by mechanical stirring or manual grinding.
[0017] According to the above scheme: in step 2), the heat treatment time is 2-5h.
[0018] According to the above scheme: in step 2), the calcination process is: the temperature is 800-900°C, the holding time is 12-24h. Preferably, the heating rate is 2-5°C / min, and the product is taken out after being naturally cooled to room temperature.
[0019] Provided is an application of the lithium-rich / slightly lithium-rich material as a positive electrode material in a lithium-ion battery.
[0020] The beneficial effects of the present invention are as follows:
[0021] 1. The present invention provides a lithium-rich / slightly lithium-rich material, which is a core-shell structure containing a spinel phase, with large-grained single crystals of the spinel phase dispersed inside, and the outermost layer is a thin shell layer of the spinel phase. Compared with the traditional layered structure, the structural stability of the material is significantly improved. When used in the positive electrode material of lithium-ion batteries, the first coulombic efficiency, rate performance and cycle performance are comprehensively improved.
[0022] 2. The present invention provides a method for preparing lithium-rich / slightly lithium-rich materials, by mixing two or more lithium salts in a certain ratio as molten salts with a precursor material, utilizing the special property that molten salts will melt at the same time at a certain temperature to form an ion melt, and keeping the reaction at the lowest temperature for forming a eutectic. Due to the different binding energies between different ions and transition metal elements in the precursor, the surface and internal structure of the slightly lithium-rich material are affected, and then high-temperature calcination is performed to form a composite slightly lithium-rich material with a spinel shell on the outside and large-grained spinel single crystals on the inside. The obtained composite slightly lithium-rich material has good structural stability and is used as a positive electrode material in lithium-ion batteries, significantly improving the first-cycle coulomb efficiency, cycle and rate performance.
[0023] 3. The present invention has the characteristic of having the lowest eutectic temperature after mixing two or more lithium salts with a suitable molar ratio, and directly uses lithium salt as both molten salt and lithium source, avoiding the addition of salts such as potassium chloride, sodium chloride, etc. in the traditional molten salt method, thereby avoiding the introduction of other impurity cations.
[0024] 4. The process of the present invention is simple, the cost is low, the product is controllable, the purity is high, and it has the potential for large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is the X-ray diffraction pattern (XRD) of the original sample obtained in comparative example 1 and the molten salt sample obtained in example 1.
[0026] Figure 2 is the original sample obtained in Comparative Example 1 ( Figure 2 a and 2b) and the molten salt sample obtained in Example 1 ( Figure 2c and 2d) scanning electron micrographs (SEM).
[0027] Figure 3 is the original sample obtained in Comparative Example 1 ( Figure 3 a) and the molten salt sample obtained in Example 1 ( Figure 3 b) Thermogravimetric and differential scanning calorimetry (TG-DSC) diagram.
[0028] Figure 4 is the original sample obtained in Comparative Example 1 ( Figure 4 a and 4b) and the molten salt sample obtained in Example 1 ( Figure 4 c and 4d) scanning transmission electron micrographs (STEM).
[0029] Figure 5 The electrochemical performance diagram of the original sample obtained in Example 1 and the molten salt sample obtained in Example 1 is shown; Figure 5 a and 5b are the electrochemical curves of the original sample and the molten salt sample, respectively; Figure 5 c is the rate performance diagram of the two samples; Figure 5 d is the cycling performance diagram of the two samples at a current density of 50 mA / g. DETAILED DESCRIPTION
[0030] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.
[0031] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0032] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0033] Embodiment 1:
[0034] A method for preparing a slightly lithium-rich material from molten salt is provided, comprising the following steps:
[0035] 1) 0.5798gNi 0.25 Mn 0.75 CO3 precursor powder, 0.0860g LiOH·H2O and 0.2120g LiNO3 (calculated by molar amount, LiOH / (LiNO3+LiOH)=0.393, at this molar ratio, the two substances can form a eutectic with a minimum eutectic temperature of 190°C) are put into a ball mill and mixed thoroughly. Ni 0.25 Mn0.75 The molar ratio of CO3 precursor to molten salt was 1:1.15, the rotation speed was 600 r / min, and the mixing was performed for 2 h.
[0036] 2) The mixture obtained in step 1) is placed under air conditions, heated to 190°C, kept warm for 3 hours, then heated to 900°C at a heating rate of 5°C / min, kept warm for 10 hours, and naturally cooled to room temperature to obtain a slightly lithium-rich material, which is recorded as a molten salt sample.
[0037] Comparative Example 1
[0038] A method for preparing a slightly lithium-rich material using a single lithium salt is provided, comprising the following steps:
[0039] 1) 0.5798gNi 0.25 Mn 0.75 CO3 precursor powder was mixed with 0.2643 g LiOH·H2O and put into a ball mill to mix thoroughly. 0.25 Mn 0.75 The molar ratio of CO3 precursor to lithium hydroxide was 1:1.15, the rotation speed was 600 r / min, and the mixing was performed for 2 h.
[0040] 2) The mixture obtained in step 1) is placed under air conditions, heated to 300°C, kept warm for 3 hours, and then heated to 900°C at a heating rate of 5°C / min, kept warm for 10 hours, and naturally cooled to room temperature and taken out to obtain a slightly lithium-rich material synthesized by a single lithium salt, which is recorded as the original sample.
[0041] Taking the product of this example, the slightly lithium-rich material synthesized by molten salt, as an example, its structure was determined by X-ray diffractometer and scanning electron microscope. The X-ray diffraction spectrum (XRD) shows that the original sample synthesized by lithium salt alone is an α-NaFeO2 structure, an O3-type layered compound, and has no obvious impurity peaks; the structure of the molten salt sample is roughly the same, but the peak near 37° is split, which indicates that there is a spinel phase inside the material ( Figure 1 ).
[0042] Scanning electron microscopy (SEM) Figure 2 The results show that both the synthesized original sample and the molten salt sample are spherical secondary particles with an average diameter of 10 μm. There may be a small amount of floccules on the surface of the particles, which may be unreacted lithium salts. The morphology of the two materials did not change significantly, indicating that the method of molten salt synthesis has no significant effect on the morphology of the materials.
[0043] Figure 3These are the thermogravimetric and differential scanning calorimetry (TG-DSC) images of lithium salt and precursor mixed in proportion. It can be seen that the weight of the original sample decreased significantly when the temperature rose to about 320°C, indicating that the material reacted at this temperature; while the weight of the molten salt sample began to decrease significantly at about 190°C, indicating that the sample mixed with molten salt had already started to react at a lower temperature, and the internal transition metal ions and lithium salt were more tightly bound.
[0044] Figure 4 The thermal scanning transmission electron micrographs (STEM) of the two materials. Figures a and b are scanned images after the original sample is cut open. It can be seen that it is a structure with primary particles that continuously diverge from the center to the outside and extend along the radius. When the internal primary particles are magnified, there are many irregular channels inside, and there is a thin layer of about 800nm thickness on the surface. After electron diffraction testing, it was found to be a layered phase; Figures c and d are samples synthesized with molten salt. It can be seen that a large single crystal structure of about 2-5μm appears inside. This particle is dispersed inside the secondary particles and surrounded by primary particles. There is a thin layer of about 500nm thickness on the surface. After electron diffraction testing, it was found to be a spinel phase.
[0045] The electrochemical performance test of the original material and molten salt material prepared in this example was conducted by assembling a button-type half-cell, with a metal lithium sheet as the counter electrode. Cyclic voltammetry test ( Figure 5 a, b) show that the cyclic voltammograms of the two materials are similar, except that the redox peak of the molten salt sample at 3.0 V is enhanced. Figure 5 c is the rate performance diagram of the two samples. It can be seen that the discharge capacity of the half-cell assembled with molten salt material at current densities of 0.1C, 0.2C, 0.5C, 1C, and 2C is approximately 270mA / g, 250mA / g, 240mA / g, 200mA / g, and 160mA / g, while the capacity of the original sample at the same current density is 270mA / g, 220mA / g, 170mA / g, 150mA / g, and 120mA / g, respectively. This shows that the material prepared by the molten salt method has better rate performance. Figure 5 d is the cycle performance diagram of the two materials at a current density of 50 mA / g, indicating that at 0.4C (1C = 250 mAh g -1 ), after 100 cycles of the molten salt sample, the capacity retention rate was 91%, while the capacity retention rate of the original sample was only 88.7%. Therefore, the cycle performance of the molten salt sample is better than that of the original sample.
[0046] Embodiment 2:
[0047] A method for preparing a lithium-rich material from molten salt is provided, comprising the following steps:
[0048] 1) 2.319 g Ni 0.25 Mn 0.75 CO3 precursor powder and 1.2588g LiOH·H2O and 0.4130g Li2CO3 (calculated by molar amount, LiOH / (Li2CO3+LiOH)=0.843, the molar amount of lithium hydroxide accounts for 0.843 of the total molar amount, and at this molar ratio, the two substances can form a eutectic with a minimum eutectic temperature of 425°C), Ni 0.25 Mn 0.75 The molar ratio of CO3 precursor to molten salt was 1:1.25, and the mixture was put into a ball mill and mixed thoroughly at a speed of 600 r / min for 4 hours.
[0049] 2) The mixture obtained in step 1) is placed in air or oxygen conditions, heated to 425°C, kept warm for 3 hours, with a heating rate of 5°C / min, and then continued to heat to 900°C and kept warm for 10 hours, and naturally cooled to room temperature and taken out to obtain a lithium-rich material.
[0050] Embodiment 3:
[0051] A method for preparing a slightly lithium-rich material from molten salt is provided, comprising the following steps:
[0052] 1) 0.5841 g Ni 0.5 Mn 0.5 The CO3 precursor powder, 0.0881g LiOH·H2O and 0.2172g LiNO3 (calculated by molar amount, LiOH / (LiNO3+LiOH)=0.393, the molar amount of lithium hydroxide accounts for 0.393 of the total molar amount. At this molar ratio, the two substances can form a eutectic with a minimum eutectic temperature of 190°C) are placed in a ball mill and mixed thoroughly at a speed of 200r / min for 4h.
[0053] 2) The mixture is placed in air or oxygen, heated to 190°C, kept warm for 3 hours, with a heating rate of 5°C / min, and then continued to be heated to 850°C and kept warm for 10 hours. The mixture is naturally cooled to room temperature and taken out to obtain a slightly lithium-rich material.
[0054] Embodiment 4:
[0055] A method for preparing a slightly lithium-rich material from molten salt is provided, comprising the following steps:
[0056] 1) 0.5841 g Ni 0.5 Mn 0.5The CO3 precursor powder, 0.1857g LiOH·H2O and 0.0552g Li2CO3 (calculated by molar amount, LiOH / (Li2CO3+LiOH)=0.843, the molar amount of lithium hydroxide accounts for 0.843 of the total molar amount. At this molar ratio, the two substances can form a eutectic with a minimum eutectic temperature of 425°C) are placed in a ball mill and mixed thoroughly at a speed of 200r / min for 4h.
[0057] 2) The mixture is placed in air or oxygen, heated to 425°C, kept warm for 3 hours, with a heating rate of 7°C / min, and then continued to be heated to 900°C and kept warm for 12 hours. It is naturally cooled to room temperature and taken out to obtain a slightly lithium-rich material.
[0058] The above descriptions are only some implementation examples of the present invention and do not constitute any form of limitation to the present invention. Any equivalent changes, modifications and evolutions made to the above implementation examples based on the essential technology of the present invention shall fall within the protection scope of the technical solution of the present invention.
Claims
1. A lithium-rich / slightly lithium-rich material, characterized in that: The structural formula of the lithium-rich / slightly lithium-rich material is Li 1+ x Mn y Ni z N w O r ; wherein the N element is one or more of Ni, Al, Mg, Ti, Fe, Cu, Cr, Mo, Zr, and Ru; the parameters x, y, z, w, and r satisfy the following conditions: 0<x≤0.2, 0<y≤1, 0≤z<1, 0≤w≤1, 1.8≤r≤3; wherein: The lithium-rich / slightly lithium-rich material is a spherical secondary particle, with large single crystal structures of the spinel phase of 2-5 μm dispersed inside, and the large single crystal structure is surrounded by primary particles, and the primary particles are radiated; the outermost layer of the lithium-rich / slightly lithium-rich material is a thin shell layer of the spinel phase.
2. The lithium-rich / slightly lithium-rich material according to claim 1, characterized in that: The thickness of the thin shell is 450-550nm.
3. A method for preparing a lithium-rich / slightly lithium-rich material as claimed in claim 1, characterized in that: The following steps are involved: 1) Mixing a molten salt with a precursor material to obtain a mixture; wherein the molten salt is two or more lithium salts in an appropriate ratio, which will melt simultaneously at a certain temperature to form an ion melt; 2) The mixture obtained in step 1) is heat treated in air or oxygen at the lowest melting temperature of the molten salt used, and finally calcined to obtain the lithium-rich / slightly lithium-rich material.
4. The preparation method according to claim 3, characterized in that: In the step 1), the lithium salt is: a mixed system of lithium nitrate and lithium hydroxide, in which the molar amount of lithium hydroxide accounts for 0.393 of the total molar amount; or, a mixed system of lithium carbonate and lithium sulfate, in which the molar amount of lithium carbonate accounts for 0.6 of the total molar amount; or, a mixed system of lithium carbonate and lithium fluoride, in which the molar amount of lithium carbonate accounts for 0.48 of the total molar amount; or, a mixed system of lithium carbonate and lithium nitrate, in which the molar amount of lithium carbonate accounts for 0.993 of the total molar amount; or, a mixed system of lithium carbonate and lithium hydroxide, in which the molar amount of lithium carbonate accounts for 0.843 of the total molar amount; or, a mixed system of lithium nitrate and lithium hydroxide, in which the molar amount of lithium nitrate accounts for 0.393 of the total molar amount.
5. The preparation method according to claim 3, characterized in that: In the step 1), the molar ratio of the precursor material to the lithium element in the lithium salt is 1:1.02 to 1:1.
25.
6. The preparation method according to claim 3, characterized in that: In the step 1), the precursor material is a carbonate or hydroxide precursor material containing two elements of manganese and nickel or three elements of manganese, nickel and N; wherein the N element is one or more of Ni, Al, Mg, Ti, Fe, Cu, Cr, Mo, Zr, and Ru.
7. The preparation method according to claim 3, characterized in that: In the step 1), the lithium salt and the precursor material are mixed uniformly by mechanical stirring or manual grinding.
8. The preparation method according to claim 3, characterized in that: In the step 2), the heat treatment time is 2-5 hours.
9. The preparation method according to claim 3, characterized in that: In the step 2), the calcination process is as follows: the temperature is 800-900° C. and the insulation time is 12 to 24 hours.
10. Use of the lithium-rich / slightly lithium-rich material according to claim 1 as a positive electrode material in a lithium-ion battery.
Citation Information
Patent Citations
Preparation method and application of nickel-rich cobalt-free single crystal positive electrode material of lithium ion battery
CN113636606A
Cathode active material for non-aqueous electrolyte rechargeable battery and manufacturing method for same, and non-aqueous electrolyte rechargeable battery
US20160164093A1
Cited By
High-capacity positive electrode lithium supplement agent and preparation method and application thereof
CN122619805A