Preparation method of doped and coated sodium ion battery negative electrode material

By alumina doping and soft carbon coating on the hard carbon surface, a hard carbon-alumina-soft carbon composite material is formed, which solves the battery performance problems caused by hard carbon material defects, and improves the first Coulomb efficiency of sodium ion batteries and Cycling performance, achieving higher energy density and longer service life.

CN118969993APending Publication Date: 2024-11-15SHUANGDENG GRP CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411028221.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Hard carbon has a large number of defects and active sites as the negative electrode material of sodium ion batteries, resulting in irreversible sodium ion adsorption and electrolyte decomposition, reducing the first-time balun efficiency and energy density of the battery and increasing the battery cost.

Method used

The doping coating method is adopted, first doping alumina on the hard carbon surface, and then soft carbon coating to form a hard carbon-alumina-soft carbon composite material. The layer spacing and mass ratio are controlled by calcining temperature. , inhibit electrolyte decomposition and side reactions, and improve the intercalation ability of sodium ions and the interfacial density of electrolytes.

Benefits of technology

The first Coulomb efficiency and cycling performance of sodium ion batteries have been significantly improved, the first discharge capacity reaches 380mAh/g, and the cycling performance reaches more than 2,500 times, reducing the battery cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118969993A_ABST
    Figure CN118969993A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a doped and coated sodium ion battery negative electrode material, and the preparation method comprises the following steps: uniformly placing hard carbon particles in a solution containing an aluminum oxide doping source, and drying while stirring; after the mixture is completely dried, roasting the mixture for the first time, and mixing and stirring carbon sources doped with hard carbon and soft carbon after ball milling for the first time; and carrying out secondary ball milling on the sintered mixture to obtain a more excellent sodium electric hard carbon negative electrode material. The key of the composite negative electrode material is that the soft carbon coating and the hard carbon particles are doped with aluminum oxide for modification, and the soft carbon coating hinders formation of defect structures and oxygen-containing groups on hard carbon; the doping of aluminum oxide constructs a homotype heterojunction, shields part of active sites, inhibits the reaction degradation of the electrolyte, constructs a stable electrolyte interface, and improves the initial coulombic efficiency and cycle performance of the battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy sodium ion battery materials, and in particular to a method for preparing a doped and coated sodium ion battery negative electrode material. Background Art

[0002] In recent years, problems such as limited and uneven distribution of lithium resources have become increasingly prominent, making it difficult to simultaneously support the development of large-scale energy storage and electric vehicles. As the price of raw materials for lithium-ion batteries continues to rise, sodium-ion batteries have received widespread attention in various fields. Sodium-ion battery raw materials are cheap and widely distributed, highly safe, and have outstanding low-temperature capabilities. They can meet the requirements of high safety and low cost in the new energy field, and to a certain extent alleviate the problem of limited battery development caused by resource shortages.

[0003] Among them, hard carbon is the main negative electrode material for sodium ion batteries, and it has a theoretical reversible specific capacity of 500-700mAh / g. However, hard carbon has a large number of defects and active sites, which will produce irreversible sodium ion adsorption and electrolyte decomposition, resulting in low initial coulombic efficiency and reduced energy density, which will greatly increase the cost of the battery. At this stage, hard carbon is still in a development stage and has great potential for improving its capacity and battery stability. Summary of the invention

[0004] The purpose of the present invention is to solve the defects of existing hard carbon and provide a method for preparing a doped and coated sodium ion battery negative electrode material, which can improve the initial efficiency of the sodium ion battery and increase its cycle performance. The specific technical scheme is as follows: A method for preparing a doped and coated sodium ion battery negative electrode material comprises the following steps: Step 1: evenly place the hard carbon particles in a solution containing a doping source, continuously stir at a temperature of T1, dry while stirring, and continue to keep the temperature for t1 hours after the liquid is dry; Step 2: After being completely dried, calcining at a temperature T2 for t2 hours in an inert gas atmosphere without oxygen; the weight content percentage wt% of the hard carbon-alumina material is within the range of a; Step 3: ball milling the obtained composite material to obtain doped hard carbon; mixing and stirring the doped hard carbon and the carbon source of soft carbon; Step 4: After stirring evenly, calcining at T3 temperature for t3 hours in an inert gas atmosphere without oxygen; the weight content percentage wt% of the hard carbon and soft carbon materials after doping is within the range of b; Step 5: The sintered mixture is ball-milled again to obtain the above-mentioned negative electrode material.

[0005] Preferably, in step 1, the doping source is any one of aluminum nitrate, pseudo-boehmite, and aluminum hydroxide solution; the solvent of the solution is any one of methanol, ethanol, isopropanol, acetone, and toluene; the T1 temperature is 60-90° C., and the t1 time is 2-3 h.

[0006] Preferably, in step 2, the inert gas is any one of helium, argon, and nitrogen, and any mixture thereof; T2 temperature is 400-1000°C; t2 time is 3-7h; a ranges from 1% to 10%.

[0007] Preferably, the carbon source of the soft carbon in step 3 is any one of coal tar pitch, petroleum residue oil pitch, polyacrylonitrile, epoxy resin, and phenolic resin.

[0008] Preferably, in step 4, the inert gas is any one of helium, argon, and nitrogen, and any mixture thereof; T3 temperature is 600-1500°C; t2 time is 3-7h; b range is 1%-15%.

[0009] Preferably, the first coulombic efficiency of the prepared sodium ion battery negative electrode material is above 89%, and the cycle performance is above 2500 times.

[0010] Compared with the closest prior art, the technical solution provided by the present invention has the following beneficial effects: (1) The present invention first performs aluminum oxide doping on the hard carbon surface and then performs soft carbon coating in sequence, so that aluminum oxide and soft carbon layers are uniformly formed on the hard carbon surface, thereby obtaining a hard carbon-aluminum oxide-soft carbon composite material, wherein the interlayer spacing of the hard carbon can be regulated according to the calcination temperature. The lower the temperature, the larger the interlayer spacing, which is conducive to the embedding of sodium ions. The thickness of the aluminum oxide and soft carbon layers on the surface can be regulated according to the added mass ratio; (2) The core of the composite material of the present invention is hard carbon particles that are modified by adding element doping. From the inside to the outside, they are hard carbon, aluminum oxide, and soft carbon coating layers. Aluminum oxide doping shields the active sites on the hard carbon surface, further inhibits the decomposition of the electrolyte and the occurrence of side reactions, and reduces the accumulation of NaF, thereby forming a thinner and denser electrolyte interface film, improving the sodium storage performance, and the first discharge capacity can reach 380mAh / g; the soft carbon coating also fills part of the defects on the hard carbon surface, reduces the formation of dead sodium, and reduces the consumption of sodium ions during charging, thereby improving the first coulomb efficiency, which can reach more than 89%; at the same time, the excellent mechanical properties of soft carbon are used to prevent the rupture of the electrolyte interface film during use, thereby improving the cycle performance of the negative electrode, which can reach more than 2500 times. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 This is a schematic diagram of the structure of the doped and coated sodium ion battery negative electrode material of the present invention; Among them: 1. Hard carbon, 2. Alumina, 3. Soft carbon. DETAILED DESCRIPTION

[0012] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0013] See also Figure 1 : Example 1 A method for manufacturing a hard carbon composite material comprises the following steps: Step 1: evenly placing hard carbon particles in a solution containing aluminum nitrate, stirring continuously at 70° C., and drying while stirring; Step 2: After complete drying, calcination was performed at 400°C for 4 hours under a nitrogen atmosphere. The wt% of the hard carbon-alumina material was controlled at 3%; Step 3: ball milling the obtained composite material to obtain doped hard carbon, and mixing the doped hard carbon and coal tar pitch; Step 4: After stirring evenly, calcining is performed at 900° C. for 7 hours in a nitrogen atmosphere. The wt% of the hard carbon and soft carbon materials after doping is 7%.

[0014] Step 5: The sintered mixture is ball-milled again to obtain the above-mentioned negative electrode material.

[0015] Example 2 A method for manufacturing a hard carbon composite material comprises the following steps: Step 1: placing hard carbon particles uniformly in a solution containing pseudo-boehmite, stirring continuously at 50° C., and drying while stirring; Step 2: After being completely dried, the mixture was calcined at 850°C for 5 hours in a nitrogen atmosphere, and the wt% of the hard carbon-alumina material was controlled at 5%. Step 3: ball milling the obtained composite material to obtain doped hard carbon, and mixing the doped hard carbon and epoxy resin; Step 4: After stirring evenly, calcining at 1300° C. for 6 hours in a nitrogen atmosphere, the wt% of the hard carbon and soft carbon materials after doping is 12%; Step 5: The sintered mixture is ball-milled again to obtain the above-mentioned negative electrode material.

[0016] Example 3 A method for manufacturing a hard carbon composite material comprises the following steps: Step 1: placing hard carbon particles uniformly in a solution containing aluminum hydroxide, stirring continuously at 50° C., and drying while stirring; Step 2: After being completely dried, the hard carbon-alumina material was calcined at 600°C for 7 hours in a helium atmosphere, and the wt% was controlled at 6%. Step 3: ball-milling the obtained composite material to obtain doped hard carbon; mixing and stirring the doped hard carbon and phenolic resin; Step 4: After stirring evenly, calcining at 1400° C. for 5 hours in a helium atmosphere, wherein the wt% of the hard carbon and soft carbon materials after doping is 14%; Step 5: The sintered mixture is ball-milled again to obtain the above-mentioned negative electrode material.

[0017] Comparative Example 1 The hard carbon material was prepared by referring to the method of Example 1, except that the alumina doping in step 1 and step 2 was omitted.

[0018] Comparative Example 2 The hard carbon material was prepared by referring to the method of Example 2, except that the soft carbon coating in step 3 and step 4 was omitted.

[0019] The first discharge capacity, first coulombic efficiency and cycle performance tests were conducted on Examples 1-3 and Comparative Examples 1-2 at 25° C. The results are shown in Table 1.

[0020] Table 1 Test data of Examples 1-3 and Comparative Examples 1-2 It can be seen from the test data in Table 1 that the preparation method of the present invention is used to prepare the negative electrode material for sodium ion batteries, which can obtain a better first coulombic efficiency and good cycle stability while maintaining the high capacity of hard carbon.

[0021] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the same. Although the present invention has been described in detail with reference to the above embodiments, a person skilled in the art can still modify or make equivalent substitutions to the specific implementations of the present invention. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention are within the scope of protection of the claims of the present invention to be approved.

Claims

1. A method for preparing a doped and coated sodium ion battery negative electrode material, characterized in that: The following steps are involved: Step 1: evenly place the hard carbon particles in a solution containing a doping source, continuously stir at a temperature of T1, dry while stirring, and continue to keep the temperature for t1 hours after the liquid is dry; Step 2: After being completely dried, calcining at a temperature T2 for t2 hours in an inert gas atmosphere without oxygen; the weight content percentage wt% of the hard carbon-alumina material is within the range of a; Step 3: ball milling the obtained composite material to obtain doped hard carbon; mixing and stirring the doped hard carbon and the carbon source of soft carbon; Step 4: After stirring evenly, calcining at T3 temperature for t3 hours in an inert gas atmosphere without oxygen; the weight content percentage wt% of the hard carbon and soft carbon materials after doping is within the range of b; Step 5: The sintered mixture is ball-milled again to obtain the above-mentioned negative electrode material.

2. The method for preparing a doped and coated sodium ion battery negative electrode material according to claim 1, characterized in that: In step 1, the doping source is any one of aluminum nitrate, pseudo-boehmite, and aluminum hydroxide solution; the solvent of the solution is any one of methanol, ethanol, isopropanol, acetone, and toluene; the T1 temperature is 60-90° C., and the t1 time is 2-3 hours.

3. The method for preparing a doped and coated sodium ion battery negative electrode material according to claim 1, characterized in that: In step 2, the inert gas is any one of helium, argon, and nitrogen, and any mixture thereof; T2 temperature is 400-1000°C; t2 time is 3-7h; a range is 1%-10%.

4. The method for preparing a doped and coated sodium ion battery negative electrode material according to claim 1, characterized in that: The carbon source of the soft carbon in step 3 is any one of coal tar pitch, petroleum residue oil pitch, polyacrylonitrile, epoxy resin, and phenolic resin.

5. The method for preparing a doped and coated sodium ion battery negative electrode material according to claim 1, characterized in that: In step 4, the inert gas is any one of helium, argon, and nitrogen, and any mixture thereof; T3 temperature is 600-1500° C.; t2 time is 3-7 hours; and b ranges from 1% to 15%.

6. The method for preparing a doped and coated sodium ion battery negative electrode material according to claim 1, characterized in that: The first coulombic efficiency of the prepared sodium-ion battery negative electrode material is over 89%, and the cycle performance is over 2,500 times.

Citation Information

Cited By

  • Lithium-rich manganese-based positive electrode material and preparation method thereof, positive plate, lithium ion battery and power-related equipment

    CN119481032A