Amino-modified wood charcoal / iodine integrated electrode material and preparation method and application thereof
By modifying the integrated electrode material of wood charcoal/iodine, using the three-dimensional porous structure and amino modification of the wood charcoal base, the problems of poor conductivity and low iodine load of zinc-iodine batteries are solved, and efficient iodine load and electrochemistry are achieved The performance has been improved, which has inhibited the shuttle of multiple iodine ions and promoted the application of zinc-iodine batteries.
Patent Information
- Application Number
- CN202411171242.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-26
AI Technical Summary
The poor conductivity of the electrode material, low active iodine loading and the shuttle effect of multiple iodine ions in the positive electrode of the zinc-iodine battery hinder the practical application of zinc-iodine batteries.
Using amino-modified wood charcoal/iodine integrated electrode material, the three-dimensional layered porous structure of the wood charcoal substrate and the chemical bonding of amino-to-iodine carbon atoms are used to improve iodine Loading and conductivity inhibit the shuttle of multi-iodine ions.
It achieves high conductivity and high capacity, improves the energy density and circulation performance of zinc-iodine batteries, inhibits the shuttle effect of multiple iodides, and improves the overall performance of electrode materials.
Smart Images

Figure CN118970025A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrode materials, and more specifically, to an amino-modified wood charcoal / iodine integrated electrode material and a preparation method and application thereof. Background Art
[0002] Zinc-based aqueous batteries have a high theoretical specific capacity (820 mAh g -1 ), abundant zinc reserves, low electrode potential (-0.76 V relative to standard hydrogen electrode), and good air stability have made it one of the most promising candidate batteries in the past few decades. Various aqueous zinc batteries, such as zinc-manganese oxide, zinc-vanadium oxide, zinc-Prussian blue analogs, zinc-air and zinc-halogen batteries have been developed with the expectation of improving energy and power density. Iodine (I2) has a low solubility in water (≈0.29 g L -1 ), making it suitable for aqueous batteries. 2+ Different from the insertion and extraction of ions, aqueous zinc-iodine batteries store energy through the redox reaction of iodine at the positive electrode and the deposition / stripping of zinc at the negative electrode. The electrochemical redox reaction of iodine in zinc-based aqueous batteries can provide considerable potential and 211 mAh·g -1 Due to its high theoretical capacity, it has attracted widespread attention. In addition, the multiple valence states of iodine (−1, 0, +1, +3, +5 and +7) make it theoretically have great potential for multi-electron conversion reactions. In recent years, static zinc-iodine batteries have made great progress in the development of high specific capacity and long-life positive electrode materials, mainly focusing on various carbon materials, single-atom materials, coordination materials, conductive polymers, etc., while also attempting to inhibit the growth of zinc negative electrode dendrites, inhibit the generation of by-products and prevent polyiodide corrosion. In addition, new electrolytes and functionalized separators have made major breakthroughs in zinc-iodine batteries. Although many advances have been made, the development of zinc-iodine batteries is still in its infancy, and there are key problems such as slow reaction kinetics, multi-iodine ion shuttling effect, low energy density, and unstable zinc negative electrode, which greatly hinder the practical application of zinc-iodine batteries. Summary of the invention
[0003] The present application is provided to solve the above-mentioned defects existing in the prior art. An amino-modified wood charcoal / iodine integrated electrode material and its preparation method and application are needed to solve the problems of poor conductivity of electrode materials in the positive electrode of zinc-iodine batteries, low active iodine loading, and multi-iodine ion shuttle effect.
[0004] According to an embodiment of the present application, an amino-modified wood charcoal / iodine integrated electrode material is provided, wherein the electrode material comprises an amino-modified wood charcoal substrate and elemental iodine, wherein the amino-modified wood charcoal substrate is loaded with the elemental iodine I2, and the iodine in the elemental iodine exists in an amorphous form on the wood charcoal substrate, wherein the wood charcoal substrate has a three-dimensional layered porous structure, wherein the elemental iodine is loaded on the surface and in the microchannels of the wood charcoal substrate, and the amino groups modified on the wood charcoal substrate are chemically bonded to carbon atoms.
[0005] In some embodiments, the diameter of the microchannels on the wood charcoal substrate is 5 μm-50 μm.
[0006] According to the embodiments of the present application, there is also provided a method for preparing the amino-modified wood charcoal / iodine integrated electrode material described in any embodiment of the present application, the preparation method comprising: in an ammonia atmosphere, plasma depositing an amino modifier on a carbonized wood charcoal substrate to obtain an amino-modified wood charcoal substrate; electrochemically depositing elemental iodine on the amino-modified wood charcoal substrate to obtain an amino-modified wood charcoal / iodine integrated electrode material.
[0007] In some embodiments, the power of plasma deposition is 300-500 W, and the pressure is 10-30 Pa. Preferably, the plasma deposition power may be 350-450 W, and the pressure may be 15-25 Pa. For example, the deposition power may be 400 W, 430 W, etc., and the pressure may be 20 Pa, 25 Pa, etc.
[0008] In some embodiments, the plasma deposition time is 0.5 min-30 min. Preferably, the deposition time is 1-15 min; more preferably, the deposition time is 1-2 min; for example, 1 min, 1.2 min, 2 min, etc.
[0009] In some embodiments, electrochemically depositing elemental iodine on the wood charcoal substrate comprises: mixing the wood charcoal substrate with an electrolyte solution of elemental iodine, and obtaining an amino-modified wood charcoal / iodine integrated electrode material by electrochemical deposition.
[0010] In some embodiments, during electrochemical deposition, the voltage is 1-4V and the power-on time is 10-50min. Preferably, the voltage is 1-2V and the power-on time is 20-40min. For example, 1V, 1.6V and 2V, etc. The power-on time is 20min, 30min, 35min, etc.
[0011] In some embodiments, the carbonized wood charcoal substrate is obtained by the following method: soaking wood in a hydrochloric acid solution to remove impurities; and carbonizing the wood after the impurities are removed.
[0012] In some embodiments, after the wood is soaked in the hydrochloric acid solution, the soaked wood is washed and dried to remove impurities in the wood, and then the wood is carbonized. The washing can be done with water, ethanol, or a mixture of both.
[0013] In some embodiments, the process of carbonizing wood can be carried out in a tube furnace or other closed suitable equipment. The carbonization process includes: treating at 20-50°C for 20-50 minutes; heating to 250-350°C at a first heating rate, carbonizing at 250-350°C for a first time period, heating to 850-950°C at a second heating rate, and carbonizing at 850-950°C for a second time period to obtain carbonized wood charcoal.
[0014] In some embodiments, the first heating rate is 1-3°C / min, and the corresponding first time period is 30min-2h.
[0015] In some embodiments, the second heating rate is 3-6°C / min, and the corresponding second time period is 50min-3h.
[0016] According to the embodiments of the present application, there is also provided an application of the amino-modified wood charcoal / iodine integrated electrode material described in any embodiment of the present application or a method for preparing the amino-modified wood charcoal / iodine integrated electrode material described in any embodiment of the present application in a battery.
[0017] The embodiments of the present application provide an amino-modified wood charcoal / iodine integrated electrode material and a preparation method and application thereof. The amino-modified wood charcoal substrate in the electrode material is loaded with the iodine element I2, and the wood charcoal substrate has a three-dimensional layered porous structure. The iodine element is loaded in the microchannels of the wood charcoal substrate. The amino groups modified on the wood charcoal substrate are chemically bonded to the carbon atoms. The electrode material has the advantages of high conductivity and high capacity. As a zinc-iodine battery, it can increase the iodine loading capacity and inhibit the shuttling of multiple iodides, thereby improving the performance of the electrode. Therefore, it can solve the problems of poor conductivity of the electrode material in the positive electrode of the current zinc-iodine battery, low active iodine loading capacity, and multiple iodide ion shuttling effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In the drawings, which are not necessarily drawn to scale, the same reference numerals may describe similar parts in different views. The same reference numerals with letter suffixes or different letter suffixes may represent different instances of similar parts. The accompanying drawings generally illustrate various embodiments by way of example and not limitation, and together with the specification and claims, are used to illustrate the embodiments applied for. When appropriate, the same reference numerals are used throughout the drawings to refer to the same or similar parts. Such embodiments are illustrative and are not intended to be exhaustive or exclusive embodiments of the present apparatus or method.
[0019] Figure 1 X-ray diffraction patterns of electrode materials of different embodiments are shown; FIG2( a ) shows a first cross-sectional SEM image of carbonized wood (CW) according to Example 1 of the present application; FIG2( b ) shows a second cross-sectional SEM image of the carbonized wood (CW) according to Example 1 of the present application; FIG2( c ) shows a first longitudinal cross-sectional SEM image of the wood after carbonization and ammoniation according to Example 1 of the present application; FIG2( d ) shows a second longitudinal cross-sectional SEM image of the wood after carbonization and ammoniation according to Example 1 of the present application; FIG2( e ) shows a first cross-sectional SEM image of N-CW-1 / I2 according to Example 1 of the present application; FIG2( f ) shows a second cross-sectional SEM image of N-CW-1 / I2 according to Example 1 of the present application; FIG3 (a) shows a first SEM energy spectrum scanning image of the electrode material according to Example 1 of the present application; FIG3( b ) shows a second SEM energy spectrum scanning image of the electrode material according to Example 1 of the present application; FIG3( c ) shows a third SEM energy spectrum scanning image of the electrode material according to the first embodiment of the present application; FIG3( d ) shows a fourth SEM energy spectrum scanning image of the electrode material according to Example 1 of the present application; FIG3( e ) shows a fifth SEM energy spectrum scanning image of the electrode material according to the first embodiment of the present application; Figure 4 The infrared spectra of materials prepared according to different steps of different embodiments of the present application are shown; Figure 5 A diagram showing constant current charge and discharge measurement results of electrode materials according to different embodiments of the present application; Figure 6 A graph showing test results of rate performance of electrode materials according to different embodiments of the present application; FIG. 7( a ) shows a first cyclic voltammetry graph of electrode materials according to different embodiments of the present application; FIG. 7( b ) shows a second cyclic voltammetry graph of electrode materials according to different embodiments of the present application; Figure 8 Electrochemical impedance spectra of electrode materials according to different embodiments of the present application are shown. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to better understand the technical solution of the present application, the present application is described in detail below in conjunction with the accompanying drawings and specific implementation examples. The embodiments of the present application are further described in detail below in conjunction with the accompanying drawings and specific implementation examples, but are not intended to limit the present application.
[0021] The words "first", "second" and similar words used in this application do not indicate any order, quantity or importance, but are only used to distinguish. The words "include" or "comprise" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.
[0022] According to an embodiment of the present application, an amino-modified wood charcoal / iodine integrated electrode material is provided, wherein the electrode material comprises an amino-modified wood charcoal substrate and elemental iodine, wherein the amino-modified wood charcoal substrate is loaded with the elemental iodine I2, and the iodine in the elemental iodine exists in an amorphous form on the wood charcoal substrate, wherein the wood charcoal substrate has a three-dimensional layered porous structure, wherein the elemental iodine is loaded on the surface and in the microchannels of the wood charcoal substrate, and the amino groups modified on the wood charcoal substrate are chemically bonded to carbon atoms.
[0023] The three-dimensional hierarchical porous structure of the wood charcoal substrate has a high porosity, the arrangement of the pore structure is highly ordered, and the pores are in the form of low curvature, which provides abundant loading sites for the loading of iodine, realizes strong adsorption of iodine, and limits active iodine. And the iodine is loaded in the microchannel, which is conducive to improving the coating of iodine. The abundant microchannels can also adjust the performance of zinc-iodine electrode materials.
[0024] The woody carbon substrate with excellent electrical conductivity can be used as a Zn 2+ and I − The redox reaction between them provides enough electrons, and the assembled zinc-iodine battery has significant energy storage performance, which can solve the problem of poor conductivity of the electrode material in the positive electrode of the current zinc-iodine battery.
[0025] The amino groups on the wood charcoal substrate are chemically bonded to the carbon atoms, so that the surface of the wood charcoal can firmly bind the amino groups, which is beneficial to the restriction of active iodine.
[0026] The amino-modified wood charcoal substrate, the Coulomb interaction between the positively charged amino groups on the wood charcoal substrate and the negatively charged polyiodide anions and the synergistic iodine storage mechanism of the physical confinement of porous carbon, effectively increase the iodine species loading and inhibit the shuttling of polyiodides.
[0027] Heteroatom-doped carbon materials can improve electrical conductivity, reduce electrochemical polarization, improve electrochemical reaction kinetics and surface electron mobility of wood carbon substrates, and provide additional pseudocapacitance. Therefore, the electrode material composed of amino-modified wood carbon substrate and iodine element has high conductivity, which can improve its applicability as a positive electrode material and is beneficial to improving the performance of the electrode material.
[0028] In some embodiments, the diameter of the microchannel on the wood charcoal substrate is 5 μm-50 μm. The wood charcoal substrate has abundant microchannels, and some small holes are distributed between two adjacent large holes, providing abundant loading sites.
[0029] According to the embodiments of the present application, there is also provided a method for preparing the amino-modified wood charcoal / iodine integrated electrode material described in any embodiment of the present application, the preparation method comprising: utilizing the carbonized wood charcoal base, and in an ammonia atmosphere, depositing an amino modifier on the wood charcoal by plasma to obtain an amino-modified wood charcoal base; and electrochemically depositing elemental iodine on the amino-modified wood charcoal base to obtain an amino-modified wood charcoal / iodine integrated electrode material.
[0030] In some embodiments, the power of plasma deposition is 300-500W, and the pressure is 10-30 Pa. Preferably, the plasma deposition power can be 350-450W, and the pressure is 15-25 Pa. For example, the deposition power is 400W, 430W, etc.; the pressure is 20Pa, 25Pa, etc., so that the wood charcoal is combined with ammonia to form amino groups on the surface of the wood charcoal.
[0031] In some embodiments, the plasma deposition time is 0.5 min-30 min. Preferably, the deposition time is 1-15 min. The amino-modified wood charcoal substrate can be obtained in a shorter time. The longer the deposition time, the more amino groups are grafted, the more iodine is electrodeposited, the more polarization of the battery increases, and the capacity decreases. Therefore, further preferably, the deposition time is 1-3 min; for example, 1 min, 1.2 min, 2 min, etc.
[0032] In some embodiments, electrochemically depositing elemental iodine on the wood charcoal substrate comprises: mixing the wood charcoal substrate with an electrolyte solution of elemental iodine, and obtaining an amino-modified wood charcoal / iodine integrated electrode material by electrochemical deposition.
[0033] In some embodiments, during the electrochemical deposition, the voltage is 1-4V and the power-on time is 10-50min. Preferably, the voltage is 1-2V and the power-on time is 20-40min. For example, 1V, 1.6V and 2V, etc. The power-on time is 20min, 30min, 35min, etc., so that the iodine element can be adsorbed and deposited on the wood charcoal substrate.
[0034] In some embodiments, the carbonized wood charcoal substrate is obtained by the following method: soaking wood in a hydrochloric acid solution to remove impurities; and carbonizing the wood after the impurities are removed.
[0035] In some embodiments, after the wood is soaked in the hydrochloric acid solution, the soaked wood is washed and dried to remove impurities in the wood, and then the wood is carbonized. The washing can be done with water, ethanol, or a mixture of both.
[0036] In some embodiments, the process of carbonizing wood can be carried out in a tube furnace or other closed suitable equipment. The carbonization process includes: treating at 20-50°C for 20-50min; heating to 250-350°C at a first heating rate, carbonizing at 250-350°C for a first time period, heating to 850-950°C at a second heating rate, and carbonizing at 850-950°C for a second time period to obtain carbonized wood charcoal. In some embodiments, the first heating rate is 1-3°C / min, and the corresponding first time period is 30min-2h.
[0037] In some embodiments, the second heating rate is 3-6°C / min, and the corresponding second time period is 50min-3h.
[0038] In this way, a carbonized wood charcoal with a three-dimensional layered porous structure can be obtained. The carbonized wood charcoal has a low-bend microchannel, that is, a number of microchannels in the wood charcoal are arranged along one direction to form a relatively regular microchannel structure. The pore size of the microchannel ranges from 5 to 50 microns, including both small-pore microchannels and large-pore microchannels. This makes it easier for iodine to be encapsulated in the porous structure.
[0039] According to the embodiments of the present application, there is also provided an application of the amino-modified wood charcoal / iodine integrated electrode material described in any embodiment of the present application or a preparation method of the amino-modified wood charcoal / iodine integrated electrode material described in any embodiment of the present application in a battery. Further application in zinc-iodine batteries.
[0040] The amino-modified wood charcoal / iodine integrated electrode material can be used as the positive electrode material in the battery and has good battery performance, including good cycle performance and rate performance, which improves the performance of the zinc-iodine battery and is conducive to the widespread application of zinc-iodine batteries.
[0041] Embodiment 1 (1) Preparation of CW electrode: Cut the natural poplar wood into 2×2×0.2 cm pieces along the growth direction. 3, soaked in 1 mol / L HCl solution for 1 h to remove impurities. Washed repeatedly with deionized water and ethanol, dried naturally for 12 h, and then placed in a N2-filled tube furnace at 20 °C for 30 min, then heated at 300 °C, 2 °C·min -1 Carbonization was performed for 1 h under the following conditions, and then heated to 900 °C, 5 °C min -1 Carbonization was carried out under the same conditions for 2 h to obtain carbonized wood charcoal (CW); (2) Preparation of N-CW-1 electrode: The wood charcoal carrier prepared in step (1) of ammonia plasma treatment was placed in a plasma enhanced chemical vapor deposition system and ammonia was introduced. The plasma power was 400 W, the pressure was 20 Pa, and the treatment time was set to 1 min. The obtained products were marked as N-CW-1; (3) Preparation of N-CW-1 / I2 electrode: Electrochemical deposition of iodine loading (N-CW / I2): The N-CW-1 electrode prepared in step (2) was charged at 1.6 V (relative to Zn metal anode) in 1 mol / L ZnI2 electrolyte for 30 min to obtain an I2 electrode. After being placed in a refrigerator for 12 h, it was freeze-dried at -80 °C, 0 Pa for 24 h, and the resulting product was labeled as N-CW-1 / I2.
[0042] The zinc-iodine battery assembled with the iodine cathode of N-CW-1 prepared in Example 1 can provide 6.82 mg cm -2 High iodine mass loading, at 2 mA·cm -2 It still has 0.026 mAh·cm -2 It has a high capacity and can run stably 1,000 times, achieving high capacity and high energy density.
[0043] Embodiment 2 Preparation of N-CW-2 / I2 electrode: (1) Same as step (1) of Example 1; (2) The wood charcoal carrier prepared in step (1) was placed in a plasma enhanced chemical vapor deposition system and ammonia was introduced. The plasma power was 400 W, the pressure was 20 Pa, and the treatment time was set to 2 min. The obtained products were labeled as N-CW-2. (3) The same as step (3) of Example 1, denoted as N-CW-2 / I2.
[0044] Embodiment 3 Preparation of N-CW-15 / I2 electrode: (1) Same as step (1) of Example 1; (2) The wood charcoal carrier prepared in step (1) was placed in a plasma enhanced chemical vapor deposition system and ammonia was introduced. The plasma power was 400 W, the pressure was 20 Pa, and the treatment time was set to 15 min. The obtained products were labeled as N-CW-15. (3) The same as step (3) of Example 1, denoted as N-CW-15 / I2.
[0045] Embodiment 4 Preparation of N-CW-20 / I2 electrode: (1) Same as step (1) of Example 1; (2) The wood charcoal carrier prepared in step (1) was placed in a plasma enhanced chemical vapor deposition system and ammonia was introduced. The plasma power was 400 W, the pressure was 20 Pa, and the treatment time was set to 20 min. The obtained products were labeled as N-CW-20. (3) The same as step (3) of Example 1, denoted as N-CW-20 / I2.
[0046] Comparative Example 1 Preparation of N-CW-0 / I2 electrode: (1) Same as step (1) of Example 1; denoted as N-CW-0; (2) Same as step (3) of Example 1, denoted as N-CW-0 / I2.
[0047] Figure 1 The X-ray diffraction patterns of the carbonized wood (CW) prepared in Example 1, the carbonized and ammoniated wood (N-CW-1), and the iodine-loaded wood with different ammonia treatment times are shown. Two broad diffraction peaks were observed at 25.8° and 43.1°, belonging to the (002) and (100) crystal planes of graphite carbon, respectively. In addition, the XRD spectra of N-CW-1 / I2 (A4 curve) prepared in Example 1, N-CW-2 / I2 (A5 curve) prepared in Example 2, and N-CW-15 / I2 (A3 curve) prepared in Example 3 did not show obvious I2-related diffraction peaks, indicating that iodine is well combined with the carbon host and exists in an amorphous state.
[0048] Figures 2 (a) and 2 (b) are SEM images of the cross section of the carbonized wood (CW) prepared in Example 1 (step 1). It can be clearly seen that CW has a three-dimensional porous structure composed of many arranged open microchannels, which is conducive to the rapid penetration of the electrolyte and the loading of iodine when used as the positive electrode carrier of the zinc-iodine battery. Figures 2 (c) and 2 (d) are SEM images of the longitudinal section of the carbonized ammonium treated wood (N-CW-1) prepared in Example 1 (step 2). After the carbonized wood was treated with ammonia plasma for 1 min, the porous morphology did not change significantly, and a multi-level pore structure was formed on the wall of the pipe. The internal structure is relatively stable, and the small pores are still evenly distributed without obvious collapse and destruction. These pores connect the inherent channels of the carbon to form a three-dimensional network transmission structure. The increase in the specific surface area of the ammonium carbonized wood leads to an increase in the loading and dispersion of the active components. Figure 2 (e) and Figure 2 (f) are SEM images of the cross-section of the carbonized aminated iodine-loaded wood (N-CW-1 / I2) prepared in Example 1 (step 3); after the aminated carbonized wood was electrochemically deposited with iodine, N-CW-1 / I2 retained the three-dimensional anisotropic porous structure of CW, with abundant pores with pore sizes ranging from 5 to 50 μm on the top surface and a large number of neatly arranged open microchannels along the vertical direction, indicating that the coating of iodine species and the introduction of N heteroatoms have no significant effect on the porous structure of the carbon substrate, because most of the iodine is encapsulated in the porous structure rather than accumulated on the sample surface.
[0049] In addition to retaining the porous structure, the in-situ generation of iodine particles on N-CW-1 and their uniform distribution were further confirmed by the corresponding SEM energy dispersive X-ray (EDX) elemental mapping analysis, as shown in Figure 3 (a), Figure 3 (b) corresponds to N element, Figure 3 (c) corresponds to Zn element, Figure 3 (d) corresponds to C element, and Figure 3 (e) corresponds to iodine I element. In addition to the uniform N doping in the NCW matrix, the signal of I element can also be detected throughout the N-CW-1, which confirms the uniform coating of I species on the inner and outer microchannels of N-CW-1 / I2. Most importantly, the self-supporting wood carbon electrode with complete macrostructure is obtained, which can be directly used as the positive electrode of Zn-I battery, avoiding the lengthy slurry-based electrode assembly process using adhesives.
[0050] Figure 4 The infrared spectra of carbonized (CW) prepared in Example 1 (step 1), carbonized aminated for 1 min (N-CW-1) prepared in Example 1 (step 2), and iodine-loaded wood (N-CW-1 / I2) prepared in Example 1 (step 3) are shown. Figure 4The horizontal axis is wavelength, and the vertical axis is transmittance. All three materials have obvious diffraction peaks. Compared with CW, N-CW-1 and N-CW-1 / I2 treated with ammonia plasma have diffraction peaks at 3300-3400 cm -1 The NH stretching vibration absorption peak appeared at 1600-1650 cm -1 The NH bending vibration absorption peak appeared at (slightly lower than the NH stretching vibration absorption peak), indicating that the ammonium cations were successfully modified on the surface of the wood charcoal electrode after the ammonia plasma treatment.
[0051] Performance Testing Figure 5 The current density is 2 mA·cm -2 The cycle performance of N-CW-0 / I2 prepared in Comparative Example 1, N-CW-1 / I2 prepared in Example 1, N-CW-2 / I2 prepared in Example 2, N-CW-15 / I2 prepared in Example 3 and N-CW-20 / I2 prepared in Example 4 was tested by constant current charge and discharge measurement. Figure 5 The horizontal axis is the number of cycles, and the vertical axis is the discharge capacity. After 1000 cycles, N-CW-0 / I2, N-CW-1 / I2, N-CW-2 / I2, N-CW-15 / I2 and N-CW-20 / I2 electrodes have a current density of 2 mA·cm -2 When the capacity is 0.002, 0.026, 0.021, 0.019 and 0.008 mAh·cm -2 Since the shuttle effect of iodide is suppressed, it can be seen that the N-CW-1 / I2 cathode prepared in Example 1 has a good capacity retention rate.
[0052] Figure 6 The rate performance of N-CW-0 / I2 prepared in Comparative Example 1, N-CW-1 / I2 prepared in Example 1, N-CW-2 / I2 prepared in Example 2, N-CW-15 / I2 prepared in Example 3 and N-CW-20 / I2 prepared in Example 4 at different current densities is shown in FIG. Figure 6 The vertical order of image points is indicated by arrows at different positions. Figure 6 The horizontal axis is the number of cycles, and the vertical axis is the discharge capacity. When the current density is stable at 1, 2, 3, 4 and 5 mA·cm -2 When N-CW-0 / I2 cathode is used, the specific capacity of the battery is only 0.433, 0.065, 0.026, 0.024, and 0.020 mAh·cm -2In comparison, the capacity decay of N-CW-1 / I2, N-CW-2 / I2, N-CW-15 / I2 and N-CW-20 / I2 electrodes is better than that of N-CW-0 / I2 electrode, among which N-CW-1 / I2 electrode has the smallest capacity decay and the best performance.
[0053] The current density was stable at 1, 2, 3, 4 and 5 mA·cm -2 When the specific capacities of the N-CW-1 / I2 electrode prepared in Example 1 are 0.49, 0.17, 0.11, 0.08 and 0.07 mAh·cm -2 This excellent rate performance can be attributed to the fast electrochemical reaction kinetics of the N-CW-1 / I2 electrode prepared in Example 1.
[0054] Figure 7 (a) shows the CV curve (D2) of N-CW-2 / I2 prepared in Example 2, the CV curve (D1) of N-CW-15 / I2 prepared in Example 3, and the CV curve (D3) of N-CW-20 / I2 prepared in Example 4. Figure 7 (b) shows the CV curve (E2) of N-CW-0 / I2 prepared in Comparative Example 1 and the CV curve (E1) of N-CW-1 / I2 prepared in Example 1. In Figures 7 (a) and 7 (b), the horizontal axis is voltage and the vertical axis is current. The N-CW-1 / I2 battery prepared in Example 1 is the result of diffusion control during the charge and discharge cycle, showing a typical battery type. CV tests were performed on N-CW-0 / I2 and N-CW-1 / I2, and a pair of representative redox peaks were observed on the N-CW-0 / I2 and N-CW-1 / I2 electrodes, which is consistent with the I2 / I - The voltage difference of the cell using N-CW-1 / I2 cathode is significantly reduced (0.163 mV) compared with N-CW-0 / I2 electrode (0.173 mV), which indicates that the electrochemical polarization is reduced and the reaction kinetics are accelerated. This favorable property can be attributed to the doping of nitrogen, which is conducive to faster reaction kinetics. In addition, the high peak current of the cell using N-CW-1 / I2 cathode is much greater than that of N-CW-0 / I2, which indicates that the capacity of the cell using N-CW-1 / I2 cathode is greater than that of the cell using N-CW-0 / I2 cathode.
[0055] Figure 8The electrochemical impedance spectra of N-CW-0 / I2 prepared in Comparative Example 1, N-CW-1 / I2 prepared in Example 1, N-CW-2 / I2 prepared in Example 2, N-CW-15 / I2 prepared in Example 3 and N-CW-20 / I2 prepared in Example 4 are shown in FIG. 1 , wherein at the position corresponding to the arrow, the curves from bottom to top in the direction of the arrow are N-CW-1 / I2, N-CW-20 / I2, N-CW-15 / I2, N-CW-2 / I2 and N-CW-0 / I2, respectively. Figure 8 The horizontal and vertical axes are the real and imaginary parts of the electrochemical impedance, respectively. The N-CW-1 / I2 electrode prepared in Example 1 has the smallest charge transfer impedance compared to N-CW-0 / I2, N-CW-2 / I2, N-CW-15 / I2 and N-CW-20 / I2, which indicates that the appropriate ammonia plasma strategy improves the surface electron mobility and electrochemical reaction kinetics of the carbonized wood charcoal substrate.
[0056] In addition, although exemplary embodiments have been described herein, the scope includes any and all embodiments based on the present application with equivalent elements, modifications, omissions, combinations (e.g., various embodiments intersecting schemes), adaptations or changes. The elements in the claims are to be interpreted broadly based on the language adopted in the claims, and are not limited to the examples described in this specification or during the practice of this application, and the examples are to be interpreted as non-exclusive. Therefore, this specification and examples are intended to be considered as examples only, and the true scope and spirit are indicated by the following claims and the full scope of their equivalents.
[0057] The above description is intended to be illustrative rather than restrictive. For example, the above examples (or one or more schemes thereof) may be used in combination with each other. For example, a person of ordinary skill in the art may use other embodiments when reading the above description. In addition, in the above-mentioned specific embodiments, various features may be grouped together to simplify the present application. This should not be interpreted as an intention that a feature of an application that does not require protection is necessary for any claim. On the contrary, the subject matter of the present application may be less than all the features of an embodiment of a particular application. Thus, the following claims are incorporated herein in the specific embodiments as examples or embodiments, wherein each claim is independently a separate embodiment, and it is considered that these embodiments may be combined with each other in various combinations or arrangements. The scope of the present invention should be determined with reference to the appended claims and the full scope of equivalent forms granted by these claims.
[0058] The above embodiments are only exemplary embodiments of the present application and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present application, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.
Claims
1. An amino-modified wood charcoal / iodine integrated electrode material, characterized in that: The electrode material includes an amino-modified wood charcoal substrate and elemental iodine, wherein the amino-modified wood charcoal substrate is loaded with the elemental iodine I2, and the iodine in the elemental iodine exists in an amorphous form on the wood charcoal substrate, the wood charcoal substrate has a three-dimensional layered porous structure, the elemental iodine is loaded on the surface and microchannels of the wood charcoal substrate, and the amino groups modified on the wood charcoal substrate are chemically bonded to carbon atoms.
2. The electrode material according to claim 1, characterized in that The diameter of the microchannel on the wood charcoal substrate is 5 μm-50 μm.
3. A method for preparing the electrode material according to claim 1 or 2, characterized in that: The preparation method comprises: In an ammonia atmosphere, amino modifiers are deposited on the carbonized wood charcoal substrate by plasma to obtain an amino-modified wood charcoal substrate; and iodine is electrochemically deposited on the amino-modified wood charcoal substrate to obtain an amino-modified wood charcoal / iodine integrated electrode material.
4. The preparation method according to claim 3, characterized in that The power of plasma deposition is 300-500W and the pressure is 10-30Pa.
5. The preparation method according to claim 3, characterized in that: The plasma deposition time is 0.5min-30min.
6. The preparation method according to claim 3, characterized in that: The electrochemical deposition of elemental iodine on the wood charcoal substrate comprises: mixing the wood charcoal substrate with an electrolyte solution of elemental iodine, and obtaining an amino-modified wood charcoal / iodine integrated electrode material by electrochemical deposition.
7. The preparation method according to claim 6, characterized in that: In electrochemical deposition, the voltage is 1-4V and the power-on time is 10-50min.
8. The preparation method according to claim 3, characterized in that: The carbonized wood charcoal substrate is obtained by the following method: the wood is soaked in a hydrochloric acid solution to remove impurities; and the wood after the impurities are removed is carbonized.
9. The preparation method according to claim 8, characterized in that: The carbonization process includes: treating at 20-50°C for 20-50min; heating to 250-350°C at a first heating rate, carbonizing at 250-350°C for a first time period, heating to 850-950°C at a second heating rate, and carbonizing at 850-950°C for a second time period to obtain carbonized wood charcoal.
10. Use of the amino-modified wood charcoal / iodine integrated electrode material according to any one of claims 1 to 2 or the preparation method of the amino-modified wood charcoal / iodine integrated electrode material according to any one of claims 3 to 9 in batteries.
Citation Information
Patent Citations
High-iodine-loading carbon material composite positive electrode, aqueous zinc ion iodine secondary battery and preparation method
CN116864603A
Carbon-iodine composite material and preparation method thereof, iodine positive electrode and zinc-iodine battery
CN117855407A
Biomass carbon used as host material for static zinc-iodine battery cathode
CN118263544A